Carrier for cell culture and tissue repair

By modifying α-amino acids or oxazoline polymers on the carrier material, the problem of poor adhesion performance of traditional cell culture materials is solved, large-scale cell amplification and tissue repair are achieved, and cost and risk are reduced.

CN118909934APending Publication Date: 2024-11-08EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410997433.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional two-dimensional cell culture materials lack active molecules that promote cell adhesion, resulting in poor cell adhesion performance, unable to meet the needs of large-scale amplification and tissue repair, and the proteins or peptides used are expensive and unstable, and there is a risk of pathogenic bacteria.

Method used

By modifying the surface or internal interface of the carrier material, α-amino acids, β-amino acids, γ-amino acids or oxazoline polymers are used as cell adsorption active molecules to perform physical adsorption or chemical covalent modification to improve cell adhesion performance.

Benefits of technology

It significantly promotes cell adhesion and growth, is suitable for large-scale cell amplification and tissue repair, reduces material costs, and improves stability and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004960637320000021
    Figure BDA0004960637320000021
  • Figure BDA0004960637320000031
    Figure BDA0004960637320000031
  • Figure BDA0004960637320000081
    Figure BDA0004960637320000081
Patent Text Reader

Abstract

The invention relates to a carrier for cell culture and tissue repair. Specifically, the invention provides an application of a modified carrier material in cell expansion and / or in-vivo tissue repair, and the modification means that the surface or internal interface of the material is modified by active molecules capable of promoting cell adhesion. The cell adhesion promoting active molecules are one or more than two homopolymers, bipolymers or multipolymers selected from the following groups: alpha-amino acid, beta-amino acid, gamma-amino acid and oxazoline. The modified carrier provided by the invention can significantly promote the adhesion growth of cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomedical materials and relates to a carrier for cell culture and tissue repair. The carrier can promote cell adhesion and can be used for large-scale cell proliferation and tissue repair. Background Art

[0002] Large-scale and efficient cell expansion and transplantation systems are crucial for fields such as vaccine production and tissue repair, and are the premise and basis for the clinical application of cell therapy. At present, two-dimensional culture dishes are commonly used in vitro cell expansion systems, but traditional two-dimensional cell culture has many shortcomings, such as low space utilization and the inability of the resulting cells to meet clinical needs. Three-dimensional carrier materials provide us with a better choice because they have a larger specific surface area and can carry cells directly injected into the body.

[0003] The cell culture materials currently used, such as polystyrene, agarose, sodium alginate, hyaluronic acid, etc., lack active molecules that promote cell adhesion on their surfaces, which is not conducive to the attachment and proliferation of cells. In order to improve the cell adhesion performance of these materials, cell adhesion proteins (such as fibronectin, vitronectin, laminin, collagen) or cell adhesion polypeptides (such as RGD) are usually used to activate the plane or carrier material. However, proteins and polypeptides are expensive and easily inactivated by protease hydrolysis, and proteins also have risks such as instability between batches and possible carrying of pathogens. Therefore, finding active molecules that are cheap and have stable structures to replace proteins or polypeptides, and at the same time can achieve rapid preparation of plane and inert carrier materials with good cell adhesion performance has great practical significance for large-scale cell culture and in vivo treatment. Summary of the invention

[0004] The purpose of the present invention is to provide a carrier for cell culture and tissue repair.

[0005] In a first aspect, the present invention provides a use of a modified carrier material in preparing a carrier for cell expansion and / or in vivo tissue repair, wherein the modification refers to modification of the surface or internal interface of the material with active molecules that promote cell adhesion.

[0006] The cell adhesion promoting active molecule is one or more homopolymers, binary copolymers or multi-polymers selected from the following group: α-amino acids, β-amino acids, γ-amino acids and oxazoline.

[0007] In another preferred embodiment, the cell adhesion promoting active molecule comprises a polymer segment represented by Formula I, Formula II or Formula III in CN113185740A.

[0008] In another preferred embodiment, one end of the chain segment is a monomer residue, and the other end is optionally a terminal group selected from the following group: H, C1-C18 alkyl, C1-C18 haloalkyl, -R a 、C1-C18 alkylene R a (such as -tBu tert-butyl R a ), C1-C18 haloalkyl R a (preferably C3-C18 fluorinated alkyl R a ), -NHC1-C12 alkylene R a、 -OC1-C12 alkylene R a 、-COC1-C12 alkylene R a ; Each R a Independently selected from the group consisting of: -SH, -NH 2 , -COOH, -Br, -Cl, -OH, epoxy, alkenyl, alkynyl, -COCl, azido, maleimide, o-pyridyldisulfide (OPSS).

[0009] In another preferred embodiment, one end of the chain segment is a monomer residue, and the other end is optionally a terminal group selected from the following group: H, C1-C6 alkyl, C1-C6 haloalkyl, R a 、C1-C6 alkylene R a 、C1-C6 haloalkyl R a 、-NHC1-C6 alkylene R a、 -OC1-C6 alkylene R a 、-COC1-C6 alkylene R a ; Each R a Independently selected from the group consisting of: -SH, -NH 2 , -COOH, -Br, -Cl, -OH, epoxy, alkenyl, alkynyl, -COCl, azido, maleimide, o-pyridyldisulfide (OPSS).

[0010] In another preferred embodiment, the cell adhesion promoting active molecule has one or more polymer segments selected from the following group:

[0011]

[0012]

[0013] In each formula, each x is independently 1-99%, y=1-x;

[0014] Each n is independently 5-200.

[0015] In another preferred embodiment, the cell adhesion promoting active molecule has one or more polymer segments selected from the following group: -(DM x CO y)n、-(DM x CH y )n,-(Lys x Nle y )n and -(NPrOx x CHO y )n;

[0016] wherein each x is independently 1-99%, y=1-x;

[0017] Each n is independently 5-200.

[0018] In another preferred embodiment, one end of the chain segment has an end group independently selected from the following groups: H, C1-C18 alkyl, C1-C18 haloalkyl, -R a 、C1-C18 alkylene R a (such as -tBu tert-butyl R a ), C1-C18 haloalkyl R a (preferably C3-C18 fluorinated alkyl R a ), -NHC1-C12 alkylene R a、 -OC1-C12 alkylene R a 、-COC1-C12 alkylene R a ; Each R a Independently selected from the group consisting of: -SH, -NH 2 , -COOH, -Br, -Cl, -OH, epoxy, alkenyl, alkynyl, -COCl, azido, maleimide, o-pyridyldisulfide (OPSS).

[0019] In another preferred embodiment, one end of the chain segment has an end group independently selected from the following group: H, C1-C6 alkyl, C1-C6 haloalkyl, R a 、C1-C6 alkylene R a 、C1-C6 haloalkyl R a 、-NHC1-C6 alkylene R a、 -OC1-C6 alkylene R a 、-COC1-C6 alkylene R a ; Each R a Independently selected from the group consisting of: -SH, -NH 2 , -COOH, -Br, -Cl, -OH, epoxy, alkenyl, alkynyl, -COCl, azido, maleimide, o-pyridyldisulfide (OPSS).

[0020] In another preferred embodiment, each x is independently 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, or 95%.

[0021] In another preferred embodiment, each n is independently 10, 15, 20, 25, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 180 or 200.

[0022] In another preferred embodiment, the cell adhesion promoting active molecule is a random copolymer or a block copolymer.

[0023] In another preferred embodiment, the carrier material is a non-degradable material or a degradable material.

[0024] In another preferred embodiment, the non-degradable material is selected from the group consisting of polystyrene, active glass, poly-ε-caprolactone, acrylamide, polymethyl methacrylate, graphene, polypropylene, polycarbonate, PBS resin, polytetrafluoroethylene, polyurethane, titanium, or a combination thereof;

[0025] In another preferred embodiment, the degradable material is selected from the following group: hyaluronic acid, sodium alginate, gelatin, chitosan, agarose, dextran, cellulose, chitin, polyethylene glycol, polylactic acid, polyglycolic acid, or a combination thereof.

[0026] In another preferred embodiment, the active molecules that promote cell adhesion are modified on the surface of the carrier material by physical adsorption.

[0027] In another preferred embodiment, the physical adsorption comprises the steps of:

[0028] (1) A solution of active molecules that promote cell adhesion is prepared using pure water or phosphate buffered saline (PBS) or physiological saline, with a concentration of 0.00025 mg / mL or above, preferably 0.0025-0.5 mg / mL.

[0029] (2) Immerse the hydrophobic material to be modified in the above-prepared active molecule solution that promotes cell adhesion for more than 10 seconds.

[0030] (3) After finishing, clean the surface with pure water and blow dry.

[0031] In another preferred embodiment, the active molecules that promote cell adhesion can be covalently grafted onto the surfaces of various materials by chemical methods.

[0032] In another preferred embodiment, the cells in the cell culture are adherent cultured cells.

[0033] In another preferred embodiment, the cells in the cell culture are selected from the following group: stem cells, osteoblasts, chondrocytes, bone marrow mesenchymal stem cells, tendon cells, cardiomyocytes, corneal cells, fibroblasts, endothelial cells, smooth muscle cells, Chinese hamster ovary cells (CHO), African green monkey kidney cells (VERO), human colorectal adenocarcinoma epithelial cells (DLD-1), and human embryonic kidney cells (HEK-293T).

[0034] In another preferred embodiment, the microcarrier modified with the cell adhesion promoting active molecule can be used for in vitro cell culture, large-scale expansion, vaccine or virus production.

[0035] In another preferred embodiment, the carrier modified with cell adhesion promoting active molecules can adhere to and expand cells in vitro, and at the same time load the cells and implant them into the body for the repair of tissues such as bone, cartilage, tendon, myocardium, cornea, blood vessel, and skin.

[0036] The second aspect of the present invention is an in vitro cell culture method, comprising the steps of:

[0037] Contacting the cells with a carrier material modified with an active molecule that promotes cell adhesion, wherein the active molecule that promotes cell adhesion is modified at least on the surface or internal interface of the carrier material in contact with the cells; and

[0038] expanding cells under culture conditions;

[0039] The cell adhesion promoting active molecule is one or more homopolymers, binary copolymers or multi-polymers selected from the following group: α-amino acids, β-amino acids, γ-amino acids, and oxazoline.

[0040] In another preferred embodiment, the carrier material is a plane, a container or a microcarrier.

[0041] In another preferred embodiment, the cells in the cell culture are selected from the following group: stem cells, osteoblasts, chondrocytes, tenocytes, cardiomyocytes, keratocytes, fibroblasts, endothelial cells, smooth muscle cells, Chinese hamster ovary cells (CHO), African green monkey kidney cells (VERO), human colorectal adenocarcinoma epithelial cells (DLD-1), and human embryonic kidney cells (HEK-293T).

[0042] In a third aspect, the present invention provides an implant, comprising:

[0043] A carrier material at least a portion of which is modified with an active molecule that promotes cell adhesion, wherein the active molecule that promotes cell adhesion is one or more homopolymers, binary copolymers or multi-polymers selected from the group consisting of α-amino acids, β-amino acids, γ-amino acids, and oxazoline; and

[0044] Therapeutic cells adhere to the modified surface.

[0045] In another preferred embodiment, the therapeutic cells are selected from the following group: bone cells, chondrocytes, cardiomyocytes, corneal cells, vascular cells, stem cells, and tendon cells.

[0046] In another preferred embodiment, the product is selected from the following group: orthopedic implants, medical devices, medical catheters, dressings, or other medical materials that can be implanted into the body.

[0047] In another preferred embodiment, the product is selected from the following group: venous indwelling catheters, cardiovascular stents, pacemakers, electrophysiological catheters, and hip implants.

[0048] It should be understood that within the scope of the present invention, the above-mentioned technical features of the present invention and the technical features specifically described below (such as embodiments) can be combined with each other to form a new or preferred technical solution. Due to space limitations, they will not be described one by one here. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 Bone marrow mesenchymal stem cells in PS and modified polymer DM 50 CO 50 Fluorescence photograph of live&dead staining after 24 hours of adhesion on the PS surface.

[0050] Figure 2 Bone marrow mesenchymal stem cells in PS and modified polymer DM 50 CH 50 Fluorescence photograph of live&dead staining after 24 hours of adhesion on the PS surface.

[0051] Figure 3 Bone marrow mesenchymal stem cells in PS and modified polymer DM 40 CO 60 Fluorescence photograph of live&dead staining after 24 hours of adhesion on the PS surface.

[0052] Figure 4 For bone marrow mesenchymal stem cells in PS and modified polymer MM 50 CO 50 Fluorescence photograph of live&dead staining after 24 hours of adhesion on the PS surface.

[0053] Figure 5 For bone marrow mesenchymal stem cells in PDMS and modified polymer DM 50 CO 50 Fluorescence photograph of live&dead staining after 24 hours of adhesion on the PDMS surface.

[0054] Figure 6 Bone marrow mesenchymal stem cells in PET and modified polymer DM50 CO 50 Fluorescence photograph of live&dead staining after 24 hours of adhesion on the PET surface.

[0055] Figure 7 Bone marrow mesenchymal stem cells in PP and modified polymer DM 50 CO 50 Fluorescent photograph of live&dead staining after 24h of adhesion on the PP surface.

[0056] Figure 8 Bone marrow mesenchymal stem cells in PTFE and modified polymer DM 50 CO 50 Fluorescence photograph of live&dead staining after 24 hours of adhesion on the PTFE surface.

[0057] Fig. 9 Bone marrow mesenchymal stem cells in TPU and modified polymer DM 50 CO 50 Fluorescence photograph of live&dead staining on the TPU surface after 24 hours of adhesion.

[0058] Fig.10 Bone marrow mesenchymal stem cells in PVC and modified polymer DM 50 CO 50 Fluorescent photograph of live&dead staining after 24 hours of adhesion on the PVC surface.

[0059] Fig.11 For fibroblasts in PS and modified polymer DM 50 CO 50 Fluorescence photograph of live&dead staining after 24 hours of adhesion on the PS surface.

[0060] Fig.12 For osteoblasts in PS and modified polymer DM 50 CO 50 Fluorescence photograph of live&dead staining after 24 hours of adhesion on the PS surface.

[0061] Fig.13 VERO cells in PS and modified polymer DM 50 CO 50 Fluorescence photograph of live&dead staining after 24 hours of adhesion on the PS surface.

[0062] Fig.14 For CHO cells in PS and modified polymer DM 50 CO 50 Fluorescence photograph of live&dead staining after 24 hours of adhesion on the PS surface.

[0063] Fig.15 For HEK-293T cells in PS and modified polymer DM 50 CO 50 Fluorescence photograph of live&dead staining after 24 hours of adhesion on the PS surface.

[0064] Fig.16 For DLD-1 cells in PS and modified polymer DM 50 CO 50 Fluorescence photograph of live&dead staining after 24 hours of adhesion on the PS surface.

[0065] Fig.17 Bone marrow mesenchymal stem cells in PS and modified polymer DM 50 CO 50 Fluorescence photograph of live&dead staining after 24 hours of adhesion to PS microspheres.

[0066] Fig.18 Bone marrow mesenchymal stem cells in PS and modified polymer DM 50 CO 50 Fluorescent photographs of live&dead staining after 1, 2, and 3 days of proliferation on PS microspheres.

[0067] Fig.19 Bone marrow mesenchymal stem cells in GelMA and modified polymer DM 50 CO 50 Fluorescence photograph of live&dead staining after 24 hours of adhesion to GelMA microspheres.

[0068] Fig. 20 For chondrocytes in alginate and modified polymer DM 50 CO 50 White field microscope photograph of alginate microspheres after 8 days of proliferation.

[0069] Fig.21 For chondrocytes in alginate and modified polymer DM 50 CO 50 Fluorescence photograph of DAPI staining after 8 days of proliferation in alginate microspheres.

[0070] Fig. 22 For bone marrow mesenchymal stem cells in modified polymer Lys 50 Nle 50 White field photo after being adhered to the glass surface for 24 hours.

[0071] Fig.23 For rat primary cardiomyocytes in modified polymer DM 50 NB 50 White field photo after being adhered to the glass surface for 24 hours.

[0072] Fig.24 Modified polymer NPrOx for osteoblasts 30 CHOx 70 Fluorescence photograph of the glass surface after 24 hours of adhesion. DETAILED DESCRIPTION

[0073] The inventors have conducted extensive and in-depth research, and through a large number of screenings and tests, provided a modified carrier material. The inventors unexpectedly found that the modified carrier can significantly promote the adhesion and growth of cells, can rapidly expand cells, can be used as a container or carrier for large-scale expansion of cells, and is very suitable for the production of various substances in cell engineering. In addition, after the cells used for treatment adhere and grow, the carrier can be used as an implant carrier to promote tissue repair. The present invention was completed on this basis.

[0074] the term

[0075] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.

[0076] As used herein, when used in reference to a specific recited numerical value, the term "about" means that the value may vary by no more than 1% from the recited value. For example, as used herein, the expression "about 100" includes all values ​​between 99 and 101 (e.g., 99.1, 99.2, 99.3, 99.4, etc.).

[0077] As used herein, the term "comprising" or "including (comprising)" may be open, semi-closed and closed. In other words, the term also includes "consisting essentially of" or "consisting of".

[0078] As used herein, the term "room temperature" or "normal temperature" refers to a temperature of 4-40°C, preferably, 25±5°C.

[0079] Cell adhesion promoting molecules

[0080] As used in the present invention, the cell adhesion promoting active molecule is one or more homopolymers, binary copolymers or multi-polymers selected from the group consisting of α-amino acids, β-amino acids, γ-amino acids, and oxazolines, such as α-amino acid polymers, β-amino acid polymers, γ-amino acid polymers or oxazoline polymers.

[0081] Typically, the cell adhesion promoting active molecule comprises a polymer segment represented by Formula I, Formula II or Formula III in CN113185740A, the contents of which are incorporated herein by reference for all purposes.

[0082] Preferably, the cell adhesion promoting active molecule has one or more polymer segments selected from the following group:

[0083]

[0084] In each formula, each x is independently 1-99%, y=1-x;

[0085] Each n is independently 5-100 (wherein n refers to the total number of monomers / monomer fragments).

[0086] More preferably, the cell adhesion promoting active molecule has one or more polymer segments selected from the group consisting of: -(DM x CO y )n、-(DM x CH y )n,-(Lys x Nle y )n and -(NPrOx x CHO y )n;

[0087] wherein each x is independently 1-99%, y=1-x;

[0088] Each n is independently 5-200.

[0089] In another preferred embodiment, the cell adhesion promoting active molecule may be a random copolymer or a block copolymer.

[0090] Typically, one end of the cell adhesion promoting active molecule is any monomer residue, and the other end is optionally a terminal group selected from the following group: H, C1-C18 alkyl, C1-C18 haloalkyl, -R a 、C1-C18 alkylene R a (such as -tBu tert-butyl R a ), C1-C18 haloalkyl R a (preferably C3-C18 fluorinated alkyl R a ), -NHC1-C12 alkylene R a、 -OC1-C12 alkylene R a 、-COC1-C12 alkylene R a ; Each R a Independently selected from the group consisting of: -SH, -NH 2 , -COOH, -Br, -Cl, -OH, epoxy, alkenyl, alkynyl, -COCl, azido, maleimide, o-pyridyldisulfide (OPSS).

[0091] Preferred terminal groups are H, C1-C6 alkyl, C1-C6 haloalkyl, R a 、C1-C6 alkylene Ra 、C1-C6 haloalkyl R a 、-NHC1-C6 alkylene R a、 -OC1-C6 alkylene R a 、-COC1-C6 alkylene R a ; Each R a Independently selected from the group consisting of: -SH, -NH 2 , -COOH, -Br, -Cl, -OH, epoxy, alkenyl, alkynyl, -COCl, azido, maleimide, ortho-disulfide pyridyl (OPSS). Among them, active groups such as -SH, -NH 2 , -COOH, -Br, -Cl, -OH, epoxy, alkene, alkynyl, -COCl, azido, maleimide, and o-pyridyldisulfide (OPSS) can advantageously be used to stably covalently modify the material.

[0092] As used herein, the term "alkyl" by itself or as part of another substituent refers to a straight or branched hydrocarbon group having the specified number of carbon atoms (i.e., C1-C18 means having 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17 or 18 carbons), preferably C1-C12, C1-C6 or C1-C3. Examples of alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, isobutyl, sec-butyl, n-pentyl, n-hexyl, and the like. The term "alkylene" by itself or as part of another substituent refers to a divalent radical derived from an alkyl group, the alkyl group having the above definition. Exemplary alkylene groups are -CH 2 -、-CH 2 CH 2 -、-CH 2 CH 2 CH 2 -or-CH 2 CH 2 CH 2 CH 2 -.

[0093] "Halogen" or "halo" refers to fluorine, chlorine, bromine or iodine.

[0094] Carrier material

[0095] The present invention has no special requirements on the material and shape of the carrier, and it can be a cell culture support carrier, medical implant material, etc. commonly used in the art.

[0096] The carrier material is a non-degradable material or a degradable material. Typical non-degradable materials include (but are not limited to): polystyrene, glass, poly-ε-caprolactone, acrylamide, polymethyl methacrylate, graphene, polypropylene, polycarbonate, PBS resin, polytetrafluoroethylene, polyurethane, or a combination thereof; degradable materials include (but are not limited to): hyaluronic acid, sodium alginate, gelatin, chitosan, agarose, dextran, cellulose, chitin, polyethylene glycol, polylactic acid, polyglycolic acid, or a combination thereof.

[0097] Commonly used cell culture support carriers can be two-dimensional or three-dimensional in space, including (but not limited to) plates, containers (open or closed containers) or microcarriers for cell culture. Commonly used medical implant materials include (but not limited to) orthopedic implants (such as plates, nails, etc.), dental implants, medical devices, medical catheters, dressings, or other medical materials that can be implanted in the body.

[0098] Material modification

[0099] In the present invention, it is unexpectedly found that after the cell adhesion promoting active molecules are modified onto the surface or internal interface (surface in contact with cells) of the carrier material, cell adhesion and growth can be significantly promoted, which is very suitable for large-scale cell expansion.

[0100] The present invention has no particular requirements for the modification method, which can be physical adsorption or chemical modification. Typical physical adsorption includes contacting the active molecule solution with the carrier surface (especially the hydrophobic surface) and drying. Chemical modification can adopt the chemical modification method commonly used in the art, such as the modification method described in CN113185740A.

[0101] A specific chemical modification method comprises the steps of: (a) providing at least a portion of the surface of the carrier,

[0102] (b) pre-activating at least a portion of the surface so that the surface has a reactive group selected from the group consisting of: -NH2, -Br, -Cl, -OH, -COOH, -CHO, epoxy, oxygen free radical, olefin, alkynyl, polydopamine composite layer, or a combination thereof, thereby obtaining a pre-activated surface; and

[0103] (c) contacting and reacting the active molecule with the pre-activated surface, thereby obtaining a substrate having at least a portion of the surface having improved antimicrobial activity and biocompatibility.

[0104] use

[0105] The modified carrier of the present invention can significantly promote the adhesion and growth of cells, can rapidly expand cells, can be used as a container or carrier for large-scale expansion of cells, and is very suitable for the production of various substances (such as polypeptides, sugars, small molecule compounds, vaccines or viruses, and even biological tissues and other materials) in cell engineering.

[0106] In addition, after the cells used for treatment adhere and grow, the modified carrier of the present invention can be used as an implantation carrier to promote tissue repair, and thus can be used to prepare medical materials for tissue repair.

[0107] Generally, cells suitable for culturing using the modified carrier material of the present invention are cells that are cultured in an adherent manner. Typical cells include (but are not limited to): stem cells, osteoblasts, chondrocytes, bone marrow mesenchymal stem cells, tendon cells, cardiomyocytes, corneal cells, fibroblasts, endothelial cells, smooth muscle cells, Chinese hamster ovary cells (CHO), African green monkey kidney cells (VERO), human colorectal adenocarcinoma epithelial cells (DLD-1), human embryonic kidney cells (HEK-293T).

[0108] Furthermore, the present invention provides an in vitro cell culture method, characterized in that it comprises the steps of:

[0109] The cells are contacted with a carrier material modified with an active molecule promoting cell adhesion, wherein the active molecule promoting cell adhesion is modified at least on the surface or internal interface of the carrier material in contact with the cells; and the cells are expanded under culture conditions.

[0110] In addition, the present invention also provides an implant, comprising: a carrier material at least a portion of whose surface is modified with active molecules that promote cell adhesion, and therapeutic cells adhered to the modified surface.

[0111] The main advantages of the present invention include:

[0112] The modified carrier of the present invention can significantly promote the adhesion and growth of cells, can rapidly expand cells, can be used as a container or carrier for large-scale expansion of cells, and is very suitable for the production of various substances in cell engineering.

[0113] In addition, the modified carrier of the present invention can be used as an implant carrier to promote tissue repair after the cells used for treatment adhere and grow, and can therefore be used to prepare medical materials for tissue repair, which is particularly important for the application of materials whose surfaces themselves cannot effectively adhere to cells.

[0114] The present invention will be further described below in conjunction with specific implementation. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually based on conventional conditions or the conditions recommended by the manufacturer. Unless otherwise stated, percentages and parts are calculated by weight.

[0115] DM 50 CO 50 :

[0116]

[0117] DM 50 CH 50 :

[0118]

[0119] DM 40 CO 60 :

[0120] MM 40 CO 60 :

[0121] Lys 50 Nle 50

[0122]

[0123] NPrOx 30 CHOx 70

[0124]

[0125] Surface and abbreviation: polystyrene (PS), polypropylene (PP), polyethylene terephthalate (PET), polyvinyl chloride (PVC), polyurethane (TPU), polytetrafluoroethylene (PTFE), polydimethylsiloxane (PDMS)

[0126] Example 1: Modified polymer DM 50 CO 50 Adhesion experiment of bone marrow mesenchymal stem cells on PS surface

[0127] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of a non-treated PS24-well plate and spread evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0128] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 600μL of cell solution was added to each well, and stained with live&dead dye after 24 hours, and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PS surface, and the bone marrow mesenchymal stem cells on the PS surface modified with polymers were well spread, which could effectively support the adhesion and growth of cells ( Figure 1 ). Promoting good cell adhesion is the primary prerequisite for promoting its proliferation and growth. This result shows that polymers can transform the surface of inert materials that are difficult for cells to adhere to into an active surface that promotes cell adhesion.

[0129] Example 2: Modified polymer DM 50 CH 50 Adhesion experiment of bone marrow mesenchymal stem cells on PS surface

[0130] Weigh 1 mg of polymer DM 50 CH 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of a non-treated PS24-well plate and spread evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0131] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 600μL of cell solution was added to each well, and stained with live&dead dye after 24 hours, and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PS surface, and the bone marrow mesenchymal stem cells on the PS surface modified with polymers were well spread, which could effectively support the adhesion and growth of cells ( Figure 2 ).

[0132] Example 3: Modified polymer DM 40 CO 60 Adhesion experiment of bone marrow mesenchymal stem cells on PS surface

[0133] Weigh 1 mg of polymer DM 40 CO 60 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of a non-treated PS24-well plate and spread evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0134] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 600μL of cell solution was added to each well, and stained with live&dead dye after 24 hours, and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PS surface, and the bone marrow mesenchymal stem cells on the PS surface modified with polymers were well spread, which could effectively support the adhesion and growth of cells ( Figure 3 ).

[0135] Example 4: Modification of polymer MM 50 CO 50 Adhesion experiment of bone marrow mesenchymal stem cells on PS surface

[0136] Weigh 1 mg of polymer MM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of a non-treated PS24-well plate and spread evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0137] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 600μL of cell solution was added to each well, and stained with live&dead dye after 24 hours, and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PS surface, and the bone marrow mesenchymal stem cells on the PS surface modified with polymers were well spread, which could effectively support the adhesion and growth of cells ( Figure 4 ).

[0138] Example 5: Modified polymer DM 50 CO 50 Bone marrow mesenchymal stem cell adhesion experiment on PDMS surface

[0139] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the PDMS surface and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0140] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged. The cell solution was diluted to 6w / mL, and 40μL of cell solution was dripped onto the surface of each material. After 2 hours, 600μL of culture medium was added to the well plate to immerse the surface of the material. After 24 hours, it was stained with live&dead dye and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PDMS surface, and the bone marrow mesenchymal stem cells on the PDMS surface modified with polymers were well spread, which could effectively support the adhesion and growth of cells ( Figure 5 ).

[0141] Example 6: Modified polymer DM 50 CO 50 Adhesion experiment of bone marrow mesenchymal stem cells on PET surface

[0142] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the PET surface and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0143] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged. The cell solution was diluted to 6w / mL, and 40μL of cell solution was dripped onto the surface of each material. After 2 hours, 600μL of culture medium was added to the well plate to immerse the surface of the material. After 24 hours, it was stained with live&dead dye and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PET surface, and the bone marrow mesenchymal stem cells on the PET surface modified with polymers were well spread, which could effectively support the adhesion and growth of cells ( Figure 6 ).

[0144] Example 7: Modified polymer DM 50 CO 50 Adhesion experiment of bone marrow mesenchymal stem cells on PP surface

[0145] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the PDMS surface and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0146] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged. The cell solution was diluted to 6w / mL, and 40μL of cell solution was dripped onto the surface of each material. After 2 hours, 600μL of culture medium was added to the well plate to immerse the surface of the material. After 24 hours, it was stained with live&dead dye and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PP surface, and the bone marrow mesenchymal stem cells on the surface of the polymer-modified PP were well spread, which could effectively support the adhesion and growth of cells ( Figure 7 ).

[0147] Example 8: Modified polymer DM 50 CO 50 Adhesion experiment of bone marrow mesenchymal stem cells on PTFE surface

[0148] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the PDMS surface and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0149] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged. The cell solution was diluted to 6w / mL, and 40μL of cell solution was dripped onto the surface of each material. After 2 hours, 600μL of culture medium was added to the well plate to immerse the surface of the material. After 24 hours, it was stained with live&dead dye and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PTFE surface, and the bone marrow mesenchymal stem cells on the PTFE surface modified with polymers were well spread, which could effectively support the adhesion and growth of cells ( Figure 8 ).

[0150] Example 9: Modified polymer DM 50 CO 50 Adhesion experiment of bone marrow mesenchymal stem cells on TPU surface

[0151] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the PDMS surface and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0152] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 40μL of cell solution was dripped onto the surface of each material, 600μL of culture medium was added to the well plate 2h later to immerse the surface of the material, and 24h later, it was stained with live&dead dye and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the TPU surface, and the bone marrow mesenchymal stem cells on the surface of the polymer-modified TPU were well spread, which could effectively support the adhesion and growth of cells ( Fig. 9 ).

[0153] Example 10: Modified polymer DM 50 CO 50 Adhesion experiment of bone marrow mesenchymal stem cells on PVC surface

[0154] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the PDMS surface and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0155] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged. The cell solution was diluted to 6w / mL, and 40μL of cell solution was dripped onto the surface of each material. After 2 hours, 600μL of culture medium was added to the well plate to immerse the surface of the material. After 24 hours, it was stained with live&dead dye and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PVC surface, and the bone marrow mesenchymal stem cells on the PVC surface modified with polymers were well spread, which could effectively support the adhesion and growth of cells ( Fig.10 ).

[0156] Example 11: Modified polymer DM 50 CO 50 Fibroblast adhesion assay on PS surface

[0157] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of the PS24-well plate and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0158] NIH-3T3 cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 600μL of cell solution was added to each well, and stained with live&dead dye after 24h, and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PS surface, and the fibroblasts on the PS surface modified with the polymer were well spread, which could effectively support the adhesion and growth of cells ( Fig.11 ).

[0159] Example 12: Modified polymer DM 50 CO 50 Adhesion experiment of osteoblasts on PS surface

[0160] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of the PS24-well plate and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0161] MC-3T3 cells were enzymatically hydrolyzed from the culture dish surface and centrifuged, the cell solution was diluted to 6w / mL, 600μL of cell solution was added to each well, and stained with live&dead dye after 24h, and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PS surface, and the osteoblasts on the PS surface modified with polymers were well spread, which could effectively support the adhesion and growth of cells ( Fig.12 ).

[0162] Example 13: Modified polymer DM 50 CO 50 Adhesion experiment of VERO cells on PS surface

[0163] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of the PS24-well plate and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0164] VERO cells were enzymatically hydrolyzed from the culture dish surface and centrifuged, the cell solution was diluted to 12w / mL, 600μL of cell solution was added to each well, and stained with live&dead dye after 24h, and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PS surface, and the VERO cells on the PS surface modified with the polymer spread well, which could effectively support the adhesion and growth of cells ( Fig.13 ).

[0165] Example 14: Modified polymer DM50 CO 50 Adhesion assay of CHO cells on PS surface

[0166] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of the PS24-well plate and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0167] The CHO cells were enzymatically hydrolyzed from the culture dish surface and centrifuged, the cell solution was diluted to 12w / mL, 600μL of cell solution was added to each well, and it was stained with live&dead dye after 24h and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PS surface, and the CHO cells on the PS surface modified with the polymer spread well, which could effectively support the adhesion and growth of cells ( Fig.14 ).

[0168] Example 15: Modified polymer DM 50 CO 50 Adhesion assay of HEK-293T cells on PS surfaces

[0169] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of the PS24-well plate and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0170] HEK-293T cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 18w / mL, 600μL of cell solution was added to each well, and it was stained with live&dead dye after 24h and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PS surface, and the HEK-293T cells on the PS surface modified with the polymer spread well, which could effectively support the adhesion and growth of cells ( Fig.15 ).

[0171] Example 16: Modified polymer DM 50 CO 50 Adhesion assay of DLD-1 cells on PS surfaces

[0172] Weigh 1 mg of polymer DM 50 CO 50Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of the PS24-well plate and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0173] The DLD-1 cells were enzymatically hydrolyzed from the culture dish surface and centrifuged, the cell solution was diluted to 10w / mL, 600μL of cell solution was added to each well, and it was stained with live&dead dye after 24h and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PS surface, and the DLD-1 cells on the PS surface modified with the polymer spread well, which could effectively support the adhesion and growth of cells ( Fig.16 ).

[0174] Example 17: Modified polymer DM 50 CO 50 Adhesion experiment of bone marrow mesenchymal stem cells on PS microcarriers

[0175] PS microspheres were purchased from Dongguan Kemai, with a diameter of 200 μm. Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2mL PBS to prepare a polymer solution with a concentration of 0.5mg / mL. Take out 400 microspheres with a pipette, add them to a 1.5mL centrifuge tube, and wash them 3 times with PBS solution. Drain as much liquid as possible the last time. Add 1mL polymer solution and shake gently for 3 minutes. After the microspheres settle, drain the polymer solution and wash them 3 times with PBS solution. Drain as much liquid as possible the last time and set aside.

[0176] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged. The cell solution was diluted to 10w / mL. 80μL of cell solution was added to each centrifuge tube containing microspheres. After being placed in an incubator for 2 hours, the microspheres were transferred to a 24-well plate and stained with live&dead dye after 24 hours. The microspheres were photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the surface of the PS microspheres. The surface of the PS microspheres modified with polymers had good spreading of bone marrow mesenchymal stem cells, which could effectively support the adhesion and growth of cells on the surface of the microspheres ( Fig.17 ).

[0177] Example 18: Modified polymer DM 50 CO 50 Proliferation experiment of bone marrow mesenchymal stem cells on PS microcarriers

[0178] PS microspheres were purchased from Dongguan Kemai, with a diameter of 200 μm. Weigh 1 mg of polymer DM 50 CO 50Dissolve in 2mL PBS to prepare a polymer solution with a concentration of 0.5mg / mL. Take out 400 microspheres with a pipette, add them to a 1.5mL centrifuge tube, and wash them 3 times with PBS solution. Drain as much liquid as possible the last time. Add 1mL polymer solution and shake gently for 3 minutes. After the microspheres settle, drain the polymer solution and wash them 3 times with PBS solution. Drain as much liquid as possible the last time and set aside.

[0179] The 2-5th generation BMSCs cells were enzymatically hydrolyzed and centrifuged from the culture dish surface, the cell solution was diluted to 10w / mL, 80μL of cell solution was added to each centrifuge tube containing microspheres, and the microspheres were placed in an incubator for 2 hours before being transferred to a 24-well plate. After 1, 2, and 3 days, the microspheres were stained with live&dead dyes and fluorescent photos were collected. The results showed that there was almost no cell adhesion on the surface of the PS microspheres. At the same time, compared with the commercial polytyrosine-coated microspheres, the surface of the PS microspheres modified with polymers had a good spreading state of bone marrow mesenchymal stem cells, which could effectively support the adhesion and proliferation of cells on the surface of the microspheres. On the 3rd day, the number of cells was 4.5 times that of the polytyrosine-coated microspheres ( Fig.18 ).

[0180] Example 19: Microfluidic preparation of covalently grafted polymer DM 50 CO 50 Adhesion experiment of bone marrow mesenchymal stem cells on the surface of gelatin (GelMA) microspheres

[0181] Two syringe needles of different thicknesses are placed coaxially to form a tube-in-tube structure. The inner and outer diameters of the inner and outer needles are 150μm, 300μm and 330μm, 600μm, respectively. The connecting part of the needle is sealed with a threaded cap. The inner needle is connected to the microfluidic device by a rubber tube with an inner diameter of 1mm. The flow rate of the liquid in the syringe is controlled by a syringe pump. The outer needle is connected to a plastic catheter with an inner diameter of 500μm. After extending the plastic catheter by 20cm, it is suspended on the platform to form a disc-shaped path with a diameter of 20cm. A UV lamp is placed vertically above the platform, and finally, it is connected to the centrifuge tube to receive the hydrogel microspheres.

[0182] Connect the syringe to the microfluidic device and flush the internal hose channel with PBS. Use the propulsion device of the microinjection pump to inject the fluid into the two inlets. A porous hydrogel system was constructed with paraffin oil as the continuous phase and 5% (w / w) Span 80 as the surfactant. First, a PBS solution containing 0.1% of the photoinitiator I2959 was used to dissolve GelMA and the polymer DM with a terminal thiol group. 50 CO 50, a 7% (v / v) GelMA solution with a polymer concentration of 0.5 mg / ml was prepared as the aqueous phase. The syringe pump was started to inject the internal phase and continuous phase liquids into the device at different flow rates. GelMA formed microdroplets under the shear stress of the continuous phase liquid and was transported from the outlet to the crosslinking disk. Under UV (405 nm, 6.9 mW cm -2 ) irradiation, the polymer can be covalently grafted to the GelMA double bond, and the GelMA double bond is photocrosslinked to form solid gel microspheres. The hydrogel microspheres were repeatedly washed with 75% alcohol and PBS to remove the surfactant and mineral oil, and then immersed in fresh PBS, and the PBS solution was replaced every 8 hours to wash the uncrosslinked hydrogel monomers and photocrosslinkers.

[0183] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged. The cell solution was diluted to 15w / mL. 80μL of cell solution was added to each centrifuge tube containing microspheres. After being placed in an incubator for 2 hours, the microspheres were transferred to a 24-well plate and stained with live&dead dye after 24 hours. The microspheres were photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the surface of the GelMA microspheres. The surface of the GelMA microspheres modified with polymers had good spreading of bone marrow mesenchymal stem cells, which could effectively support the adhesion and growth of cells on the surface of the microspheres ( Fig.19 ).

[0184] Example 20: Covalently grafted polymer DM prepared by centrifugation 50 CO 50 Experimental study on encapsulation of primary rat chondrocytes in sodium alginate hydrogel microspheres

[0185] Sodium alginate modified with 5% maleimide groups was used to graft polymer DM with thiol end groups. 50 CO 50 Then, it was prepared into a 1.5% aqueous solution with normal saline, and primary rat chondrocytes (cell density was 1 million cells / mL) were added at the same time. The sodium alginate aqueous solution mixed with cells was transferred into a 5mL syringe, equipped with a 30G needle, and then placed in a 15mL centrifuge tube, and 1mL of calcium chloride aqueous solution (15mg / mL) was added to the centrifuge tube. Finally, the sodium alginate hydrogel microspheres loaded with chondrocytes were collected after centrifugation at a speed of 1000rpm / min for 10 minutes. At the same time, sodium alginate microspheres without modified polymer were used as controls.

[0186] After the cells in the two groups of hydrogel microspheres were cultured in DMEM medium for 8 days, the white field ( Fig. 20 ) and fluorescent photos of cell nuclei stained with DAPI ( Fig.21) It can be clearly seen that in the sodium alginate microspheres modified with polymers, chondrocyte proliferation is more obvious and more chondrocytes are formed. This has outstanding advantages for the in vitro expansion of chondrocytes and their use in cartilage repair in vivo.

[0187] Example 21: Modification of polymer Lys 50 Nle 50 Adhesion experiment of bone marrow mesenchymal stem cells on glass surface

[0188] Weigh 1 mg of polymer Lys 50 Nle 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Covalently modify the polymer on the glass surface and dry it for later use.

[0189] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 40μL of cell solution was dripped onto the surface of each material, and 600μL of culture medium was added to the well plate 2 hours later to immerse the surface of the material, and the microscope was used to take pictures. The results showed that the bone marrow mesenchymal stem cells on the glass surface modified with the polymer were well spread and could effectively support the adhesion and growth of the cells ( Fig. 22 ).

[0190] Example 22: Modified polymer DM 50 NB 50 Adhesion experiment of primary rat cardiomyocytes on glass surface

[0191] Weigh 1 mg of polymer DM 50 NB 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the glass surface and spread evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0192] The 2-5th generation rat primary cardiomyocytes were enzymatically hydrolyzed from the surface of the culture dish and centrifuged. The cell solution was diluted to 6w / mL, and 40μL of cell solution was dripped onto the surface of each material. After 2 hours, 600μL of culture medium was added to the well plate to immerse the surface of the material. After 24 hours, it was stained with phalloidin dye and photographed with a fluorescence microscope. The results showed that the bone marrow mesenchymal stem cells spread well on the glass surface modified with the polymer, which could effectively support the adhesion and growth of cells ( Fig.23 ).

[0193] Example 23: Modified polymer NPrOx 30 CHOx 70 Adhesion experiment of bone marrow mesenchymal stem cells on glass surface

[0194] Weigh 1 mg of polymer NPrOx 30CHOx 70 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Covalently modify the polymer on the glass surface and let it dry for later use.

[0195] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 40μL of cell solution was dripped onto the surface of each material, and 600μL of culture medium was added to the well plate 2 hours later to immerse the surface of the material, and the microscope was used to take pictures. The results showed that the bone marrow mesenchymal stem cells on the glass surface modified with the polymer were well spread and could effectively support the adhesion and growth of the cells ( Fig.24 ).

[0196] Example 24: Modified polymer NPrOx 30 CHOx 70 Adhesion experiment of bone marrow mesenchymal stem cells on PS surface

[0197] Weigh 1 mg of polymer NPrOx 30 CHOx 70 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of a non-treated PS24-well plate and spread evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0198] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 600μL of cell solution was added to each well, and stained with live&dead dye after 24h, and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PS surface, and the bone marrow mesenchymal stem cells on the PS surface modified with the polymer were well spread, and the results were consistent with Example 4, which can effectively support the adhesion and growth of cells.

[0199] Example 25: Modified polymer NPrOx 30 CHOx 70 Bone marrow mesenchymal stem cell adhesion experiment on PDMS surface

[0200] Weigh 1 mg of polymer NPrOx 30 CHOx 70 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the PDMS surface and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0201] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 40 μL of cell solution was dripped onto the surface of each material, 600 μL of culture medium was added to the well plate 2 hours later to immerse the surface of the material, and stained with live&dead dye 24 hours later, and photographed with a fluorescence microscope. The results were consistent with those in Example 5, which can effectively support the adhesion and growth of cells.

[0202] Example 26: Modified polymer NPrOx 30 CHOx 70 Adhesion experiment of bone marrow mesenchymal stem cells on PET surface

[0203] Weigh 1 mg of polymer NPrOx 30 CHOx 70 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the PET surface and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0204] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 40 μL of cell solution was dripped onto the surface of each material, 600 μL of culture medium was added to the well plate 2 hours later to immerse the surface of the material, and stained with live&dead dye 24 hours later, and photographed with a fluorescence microscope. The results were consistent with those in Example 6, which can effectively support the adhesion and growth of cells.

[0205] Example 27: Modified polymer NPrOx 30 CHOx 70 Adhesion experiment of bone marrow mesenchymal stem cells on PP surface

[0206] Weigh 1 mg of polymer NPrOx 30 CHOx 70 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the PDMS surface and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0207] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 40 μL of cell solution was dripped onto the surface of each material, 600 μL of culture medium was added to the well plate 2 hours later to immerse the surface of the material, and stained with live&dead dye 24 hours later, and photographed with a fluorescence microscope. The results were consistent with those in Example 7, which can effectively support the adhesion and growth of cells.

[0208] Example 28: Modified polymer NPrOx 30 CHOx 70Adhesion experiment of bone marrow mesenchymal stem cells on PTFE surface

[0209] Weigh 1 mg of polymer NPrOx 30 CHOx 70 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the PDMS surface and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0210] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 40 μL of cell solution was dripped onto the surface of each material, 600 μL of culture medium was added to the well plate 2 hours later to immerse the surface of the material, and stained with live&dead dye 24 hours later, and photographed with a fluorescence microscope. The results were consistent with those in Example 8, which can effectively support the adhesion and growth of cells.

[0211] Example 29: Modified polymer NPrOx 30 CHOx 70 Adhesion experiment of bone marrow mesenchymal stem cells on TPU surface

[0212] Weigh 1 mg of polymer NPrOx 30 CHOx 70 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the PDMS surface and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0213] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 40 μL of cell solution was dripped onto the surface of each material, 600 μL of culture medium was added to the well plate 2 hours later to immerse the surface of the material, and stained with live&dead dye 24 hours later, and photographed with a fluorescence microscope. The results were consistent with those in Example 9, which can effectively support the adhesion and growth of cells.

[0214] Example 30: Modified polymer Lys 50 Nle 50 Adhesion experiment of bone marrow mesenchymal stem cells on PVC surface

[0215] Weigh 1 mg of polymer Lys 50 Nle 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the PDMS surface and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0216] The 2-5th generation BMSCs cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 40 μL of cell solution was dripped onto the surface of each material, 600 μL of culture medium was added to the well plate 2 hours later to immerse the surface of the material, and stained with live&dead dye 24 hours later, and photographed with a fluorescence microscope. The results were consistent with those in Example 10, which can effectively support the adhesion and growth of cells.

[0217] Example 31: Modification of polymer Lys 50 Nle 50 Fibroblast adhesion assay on PS surface

[0218] Weigh 1 mg of polymer Lys 50 Nle 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of the PS24-well plate and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0219] NIH-3T3 cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 600 μL of the cell solution was added to each well, and after 24 hours, the cells were stained with live&dead dye and photographed with a fluorescence microscope. The results were consistent with those in Example 11, and the adhesion growth of cells was effectively supported.

[0220] Example 32: Modified polymer Lys 50 Nle 50 Adhesion experiment of osteoblasts on PS surface

[0221] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of the PS24-well plate and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0222] MC-3T3 cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 6w / mL, 600μL of cell solution was added to each well, and stained with live&dead dye after 24h, and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PS surface, and the osteoblasts on the PS surface modified with the polymer spread well, which was consistent with Example 12 and could effectively support the adhesion and growth of cells.

[0223] Example 33: Modified polymer Lys 50 Nle 50 Adhesion experiment of VERO cells on PS surface

[0224] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of the PS24-well plate and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0225] VERO cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 12w / mL, 600μL of cell solution was added to each well, and stained with live&dead dye after 24h, and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PS surface, and the VERO cells on the PS surface modified with the polymer spread well, which was consistent with Example 13 and could effectively support the adhesion and growth of cells.

[0226] Example 34: Modification of polymer Lys 50 Nle 50 Adhesion assay of CHO cells on PS surface

[0227] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of the PS24-well plate and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0228] The CHO cells were enzymatically hydrolyzed from the culture dish surface and centrifuged, the cell solution was diluted to 12w / mL, 600μL of cell solution was added to each well, and stained with live&dead dye after 24h, and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PS surface, and the CHO cells on the PS surface modified with the polymer spread well, which was consistent with Example 14 and could effectively support the adhesion and growth of cells.

[0229] Example 35: Modification of polymer Lys 50 Nle 50 Adhesion assay of HEK-293T cells on PS surfaces

[0230] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of the PS24-well plate and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0231] HEK-293T cells were enzymatically hydrolyzed from the culture dish surface and centrifuged, the cell solution was diluted to 18w / mL, 600μL of cell solution was added to each well, and stained with live&dead dye after 24h, and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PS surface, and the HEK-293T cells on the PS surface modified with the polymer spread well, which was consistent with Example 15 and could effectively support the adhesion and growth of cells.

[0232] Example 36: Modification of polymer Lys 50 Nle 50 Adhesion assay of DLD-1 cells on PS surfaces

[0233] Weigh 1 mg of polymer DM 50 CO 50 Dissolve in 2 mL PBS to prepare a polymer solution with a concentration of 0.5 mg / mL. Add the polymer solution dropwise to the surface of the PS24-well plate and spread it evenly on the surface. After standing at room temperature for 30 seconds, wash the surface three times with PBS solution and dry it for later use.

[0234] The DLD-1 cells were enzymatically hydrolyzed from the surface of the culture dish and centrifuged, the cell solution was diluted to 10w / mL, 600μL of cell solution was added to each well, and stained with live&dead dye after 24h, and photographed with a fluorescence microscope. The results showed that there was almost no cell adhesion on the PS surface, and the DLD-1 cells on the PS surface modified with the polymer spread well, and the results were consistent with Example 16, which can effectively support the adhesion and growth of cells.

[0235] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as reference individually. In addition, it should be understood that after reading the above teachings of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. Use of a modified carrier material in preparing a carrier for cell expansion and / or in vivo tissue repair, wherein: The modification refers to modification of the surface or internal interface of the material with active molecules that promote cell adhesion. The cell adhesion promoting active molecule is one or more homopolymers, binary copolymers or multi-polymers selected from the following group: α-amino acids, β-amino acids, γ-amino acids and oxazoline.

2. The use according to claim 1, characterized in that The cell adhesion promoting active molecule has one or more polymer segments selected from the following group: In each formula, each x is independently 1-99%, y=1-x; Each n is independently 5-200.

3. The use according to claim 1, characterized in that The cell adhesion promoting active molecule has one or more polymer segments selected from the following group: x CO y )n、-(DM x CH y )n,-(Lys x Nle y )n and -(NPrOx x CHO y )n; wherein each x is independently 1-99%, y=1-x; Each n is independently 5-200.

4. The use according to any one of claims 1 to 3, characterized in that: One end of the chain segment is a monomer residue, and the other end is optionally a terminal group selected from the following groups: H, C1-C18 alkyl, C1-C18 haloalkyl, -R a 、C1-C18 alkylene R a (such as -tBu tert-butyl R a ), C1-C18 haloalkyl R a (preferably C3-C18 fluorinated alkyl R a ), -NHC1-C12 alkylene R a 、-OC1-C12 alkylene R a 、-COC1-C12 alkylene R a ; Each R a Independently selected from the following group: -SH, -NH2, -COOH, -Br, -Cl, -OH, epoxy, alkenyl, alkynyl, -COCl, azido, maleimido, o-pyridyl disulfide (OPSS).

5. The use according to claim 1, characterized in that The carrier material is a non-degradable material or a degradable material.

6. The use according to claim 1, characterized in that The non-degradable material is selected from the group consisting of polystyrene, active glass, poly-ε-caprolactone, acrylamide, polymethyl methacrylate, graphene, polypropylene, polycarbonate, PBS resin, polytetrafluoroethylene, polyurethane, titanium, or a combination thereof; The degradable material is selected from the group consisting of hyaluronic acid, sodium alginate, gelatin, chitosan, agarose, dextran, cellulose, chitin, polyethylene glycol, polylactic acid, polyglycolic acid, or a combination thereof.

7. The use according to claim 1, characterized in that The active molecules promoting cell adhesion are modified on the surface of the carrier material by physical adsorption or covalently grafted on the surface of the material by chemical methods.

8. The use according to claim 1, characterized in that The cells in the cell culture are adherent culture cells.

9. An in vitro cell culture method, characterized in that: Includes steps: Contacting the cells with a carrier material modified with an active molecule that promotes cell adhesion, wherein the active molecule that promotes cell adhesion is modified at least on the surface or internal interface of the carrier material in contact with the cells; and expanding cells under culture conditions; The cell adhesion promoting active molecule is one or more homopolymers, binary copolymers or multi-polymers selected from the following group: α-amino acids, β-amino acids, γ-amino acids, and oxazoline.

10. An implant comprising: A carrier material at least a portion of which is modified with an active molecule that promotes cell adhesion, wherein the active molecule that promotes cell adhesion is one or more homopolymers, binary copolymers or multi-polymers selected from the group consisting of α-amino acids, β-amino acids, γ-amino acids, and oxazoline; and Therapeutic cells adhere to the modified surface.