Solid steel slag recovery treatment method based on grading system
Through the solid steel slag recovery and treatment method based on the grading system, the steel slag parameters are detected and matching treatment mode is designed, the problems of low treatment efficiency and waste of resources are solved, efficient dephosphorylation iron selection and resource recycling are achieved, and environmental pollution is reduced .
Patent Information
- Application Number
- CN202410995503.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The prior art is inefficient, complex equipment, high cost when dealing with solid steel slag, and it is difficult to achieve stable dephosphorization and iron selection, resulting in waste of resources and environmental pollution.
Using solid steel slag recycling and treatment methods based on the grading system, a quality data set is established by detecting the steel slag parameters, a grading system is formulated, and a matching treatment model is designed for different levels of steel slag, including selecting appropriate treatment temperature, airflow conditions and additives to achieve steel slag classification processing.
It improves the efficiency and stability of solid steel slag treatment, reduces resource waste and environmental pollution, increases the economic benefits of steel enterprises, and realizes efficient recycling and utilization of steel slag.
Smart Images

Figure BDA0004960050660000051 
Figure BDA0004960050660000052 
Figure BDA0004960050660000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of iron and steel metallurgy, and in particular relates to a method for recycling and treating solid steel slag based on a grading system. Background Art
[0002] Steel slag contains valuable components such as iron, phosphorus, and manganese, and has great recycling value. Currently, commonly used steel slag treatment methods include magnetic separation, hot stewing, and hot pouring. These methods have the characteristics of low one-time processing efficiency, complex equipment, and high cost. Some steel companies sell the tailings after iron separation, resulting in a large waste of resources. The steel slag treatment process mainly relies on human experience control. It is difficult to achieve the effect of stable dephosphorization and iron selection by uniformly treating different steel slags. The complex composition of solid steel slag and large differences in particle size are factors that lead to unstable control of solid steel slag treatment. There is no method in the prior art that can effectively treat solid steel slag. Summary of the invention
[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to propose a method for recycling and treating solid steel slag based on a grading system, in which solid steel slag with large fluctuations in composition is classified, and solid steel slag falling into the same category can be regarded as stable and controlled by the same treatment method, so as to achieve smooth treatment of waste solid steel slag, and ultimately achieve efficient recycling of solid steel slag, reduce industrial solid waste accumulation and environmental pollution, increase the economic benefits of steel enterprises, and have important reference and guiding significance for the recycling of metallurgical waste solid steel slag.
[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0005] A method for recycling solid steel slag based on a classification system comprises the following steps:
[0006] S1. Detect the parameters of solid steel slag and establish a solid steel slag quality data set;
[0007] S2. Select solid steel slag classification indicators and formulate solid steel slag classification system;
[0008] S3. Design a matching treatment mode for different levels of solid slag;
[0009] S4. Obtain parameters of the solid slag to be processed and select a corresponding processing mode for processing.
[0010] As a preferred embodiment of the method for recycling and treating solid steel slag based on a grading system described in the present invention, in step S1, the solid steel slag quality data set includes: density, particle size, main components, and production batch.
[0011] As a preferred embodiment of the method for recycling and treating solid steel slag based on a grading system described in the present invention, in step S2, the solid steel slag grading index includes the main components of the solid steel slag and their contents.
[0012] As a preferred embodiment of the method for recycling and treating solid steel slag based on a grading system described in the present invention, wherein: in the step S2, the grading system of the main components of the solid steel slag and their contents is based on the phosphorus content detected: a phosphorus content of less than 1wt% is defined as low-phosphorus solid steel slag, a phosphorus content of 1-3wt% is defined as medium-phosphorus solid steel slag, and a phosphorus content of more than 3wt% is defined as high-phosphorus solid steel slag.
[0013] As a preferred embodiment of the method for recycling and treating solid steel slag based on a grading system described in the present invention, wherein: in the step S2, the grading system of the main components of the solid steel slag and their contents is based on the total iron content detected: the total iron content of the solid steel slag is divided based on 20wt%, wherein the solid steel slag with a total iron content ≤20wt% is defined as low-iron solid steel slag, and the solid steel slag with a total iron content >20wt% is defined as high-iron solid steel slag.
[0014] As a preferred embodiment of the method for recycling and treating solid steel slag based on a grading system described in the present invention, in step S2, the solid steel slag is divided into six levels according to the phosphorus content and total iron content of the solid steel slag, namely, low phosphorus and low iron, low phosphorus and high iron, medium phosphorus and low iron, medium phosphorus and high iron, high phosphorus and low iron, and high phosphorus and high iron.
[0015] As a preferred embodiment of the method for recycling and treating solid steel slag based on a grading system described in the present invention, in step S3, a processing mode matching different grades of solid steel slag is designed, specifically:
[0016] Low-phosphorus and low-iron solid steel slag treatment mode: Low-phosphorus and low-iron solid steel slag has a strong dephosphorization ability when it is reused in converter slag making due to its low phosphorus content, and the iron content in the slag is low, so no iron separation treatment is required; therefore, low-phosphorus and low-iron solid steel slag does not need to be treated;
[0017] Low-phosphorus high-iron solid slag treatment mode: Low-phosphorus high-iron solid slag needs to be treated with iron selection. The temperature is maintained at 1300-1500℃ during melting in the induction heating furnace. After melting, it is kept warm for 10-20 minutes. At the same time, argon is blown at the bottom to stir the molten pool evenly. The argon flow rate is 100-300Nm 3 / (h·t 渣 ), the temperature of the argon gas is 1200-1400°C; after the insulation is completed, it is allowed to stand for 0.5-1h to allow the slag and the molten metal to separate, and the molten metal flows out from the tapping port for recovery;
[0018] Medium-phosphorus and low-iron solid slag treatment mode: Medium-phosphorus and low-iron solid slag needs to be dephosphorized. The treatment process is as follows: add Fe2O3 to the induction heating furnace, the added mass is 5-15% of the total mass of the solid slag; then add medium-phosphorus and low-iron solid slag, add carbonaceous reducing agent with the slag flow, the amount of carbonaceous reducing agent added is 1-1.5 times the amount of carbonaceous reducing agent required to completely reduce FeO and P2O5 in the slag; then heat to 1300-1500℃ to melt the slag, keep it warm for 10-20 minutes after melting, and blow argon gas at the bottom to stir the molten pool evenly while keeping it warm, the argon gas flow rate is 100-300Nm 3 / (h·t 渣 ), the temperature of the argon gas is 1200-1400°C; after the insulation is completed, it is left to stand for 0.5-1h to separate the slag and the molten metal; the phosphorus vapor is collected by the phosphorus recovery device on the upper part of the furnace body, and the molten metal flows out through the steel outlet for recovery;
[0019] Medium-phosphorus high-iron solid slag treatment mode: Medium-phosphorus high-iron solid slag needs to be dephosphorized and iron selected. The treatment process is as follows: add medium-phosphorus high-iron solid slag, add carbonaceous reducing agent with the slag flow, and the amount of carbonaceous reducing agent added is 1 to 2 times the amount of carbonaceous reducing agent required to completely reduce FeO and P2O5 in the slag; then heat to 1300-1500℃ to melt the slag, keep it warm for 10-20 minutes after melting, and blow argon gas at the bottom to stir the molten pool evenly while keeping it warm. The argon gas flow rate is 100-300Nm 3 / (h·t 渣 ), the temperature of the argon gas is 1200-1400°C; after the insulation is completed, it is left to stand for 0.5-1h to separate the slag and the molten metal; the phosphorus vapor is collected by the phosphorus recovery device on the upper part of the furnace body, and the molten metal flows out through the steel outlet for recovery;
[0020] High-phosphorus, low-iron solid steel slag treatment mode: High-phosphorus, low-iron solid steel slag needs to be dephosphorized. The treatment process is as follows: add Fe2O3 to the induction heating furnace to increase the iron content in the slag. Fe2O3 has a low melting point and can reduce the overall melting point of the slag. The added mass is 5-15% of the total mass of the solid steel slag; then add high-phosphorus, low-iron solid steel slag, and add carbonaceous reducing agent and catalyst with the slag flow. The catalyst is heavy metal industrial waste slag including red mud, copper slag, and nickel slag. The catalyst can accelerate the slag dephosphorization reaction, shorten the reaction time, and improve the dephosphorization efficiency; the amount of carbonaceous reducing agent added is 1-1.5 times the amount of carbonaceous reducing agent required to completely reduce FeO and P2O5 in the slag, and the amount of catalyst added is 0.2-0.5 times the amount of high-phosphorus, low-iron solid steel slag; then heat to 1300-1500℃ to melt the steel slag, keep it warm for 10-20 minutes after melting, and blow argon gas at the bottom to stir the molten pool evenly while keeping it warm. The argon gas flow rate is 100-300Nm 3 / (h·t 渣), the temperature of the argon gas is 1200-1400°C; after the insulation is completed, it is left to stand for 0.5-1h to separate the slag and the molten metal; the phosphorus vapor is collected by the phosphorus recovery device on the upper part of the furnace body, and the molten metal flows out through the steel outlet for recovery;
[0021] High-phosphorus high-iron solid steel slag treatment mode: High-phosphorus high-iron solid steel slag needs to be dephosphorized and iron selected. The treatment process is: add high-phosphorus high-iron solid steel slag, add carbonaceous reducing agent and catalyst with the slag flow, the catalyst is heavy metal industrial waste slag including red mud, copper slag, nickel slag, the amount of carbonaceous reducing agent added is 1 to 1.5 times the amount of carbonaceous reducing agent required to completely reduce FeO and P2O5 in the slag, and the amount of catalyst added is 0.2 to 0.5 times the amount of high-phosphorus high-iron solid steel slag; then heat to 1300 to 1500 ° C to melt the steel slag, keep it warm for 10 to 20 minutes after melting, and blow argon gas at the bottom to stir the molten pool evenly while keeping it warm, and the argon gas flow rate is 100 to 300Nm 3 / (h·t 渣 ), the temperature of argon gas is 1200~1400℃; after the insulation is completed, it is left to stand for 0.5~1h to allow the slag and the molten metal to separate; the phosphorus vapor is collected by the phosphorus recovery device on the upper part of the furnace body, and the molten metal flows out through the steel outlet for recovery.
[0022] As a preferred embodiment of the solid slag recovery method based on the classification system described in the present invention, the treated slag is directly added to the converter steelmaking process as a converter slag-making agent, and the addition amount is 5-8 kg / t 钢 .
[0023] The beneficial effects of the present invention are as follows:
[0024] The present invention proposes a method for recycling and treating solid steel slag based on a grading system. The parameters of solid steel slag are detected to establish a solid steel slag quality data set; solid steel slag grading indicators are selected to formulate a solid steel slag grading system; for solid steel slag of different levels, matching treatment modes are designed; the parameters of the solid steel slag to be treated are obtained, and the corresponding treatment mode is selected for treatment. The method of the present invention is simple and reliable, with high treatment efficiency. The solid steel slag is graded before being treated, and the slag of the same level is controlled by the same treatment method, which can achieve smooth operation of the solid steel slag treatment process and avoid waste of resources caused by large fluctuations in the composition of the solid steel slag. It not only reduces the consumption of slag treatment raw materials and shortens the treatment time, but also reduces industrial solid waste emissions and environmental pollution, increases the economic benefits of steel enterprises, and has important reference and guiding significance for the efficient recycling of metallurgical industrial waste slag. DETAILED DESCRIPTION
[0025] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0027] Example 1
[0028] This method is applied to treat the solid steel slag piled up in the converter steelmaking of a certain factory. The specific implementation process is as follows: 100g of slag sample is taken, and the composition of the solid steel slag is tested. The phosphorus content in the slag is 2.15wt%, and the total iron content is 24.31wt%, which belongs to medium-phosphorus and high-iron solid steel slag. Coal powder is used as a reducing agent, and the addition amount is 30g, which is added to the induction furnace with the slag flow. The reaction temperature is controlled to 1450℃, and the insulation time is 15min. While the insulation is carried out, argon is blown at the bottom for stirring, and the argon flow rate is 200Nm 3 / (h·t 渣 ), the temperature of argon gas is 1300°C. After the insulation is completed, it is allowed to stand for 0.5h.
[0029] The composition comparison of the slag before and after the treatment of the solid slag from converter steelmaking in this embodiment is shown in Table 1. As can be seen from Table 1, after being treated by the method of the present invention, the P2O5 content in the slag is reduced from 2.15wt% to 0.17wt%, and the total iron content is reduced from 24.31wt% to 10.01wt%. The dephosphorization and iron selection effects are significant. The treated slag can be directly added to the converter steelmaking process as a slag-making agent to achieve efficient utilization of the solid slag from converter steelmaking.
[0030] Table 1 Solid slag composition before and after treatment (wt%)
[0031]
[0032] Example 2
[0033] This method is applied to treat the solid steel slag piled up in the converter steelmaking of a certain factory. The specific implementation process is as follows: Take 100g of slag sample, test the composition of the solid steel slag, and obtain the phosphorus content of 5.43wt% and the total iron content of 16.26wt% in the slag, which belongs to high-phosphorus and low-iron solid steel slag. Add 10g Fe2O3. Use coal powder as the reducing agent, the addition amount is 40g, and use nickel slag as the catalyst, the addition amount is 35g, and add them into the induction furnace with the slag flow. Control the reaction temperature to 1500℃, and the insulation time is 20min. While keeping warm, blow argon gas at the bottom for stirring, and the argon gas flow rate is 200Nm 3 / (h·t 渣), the temperature of argon gas is 1300°C. After the insulation is completed, it is allowed to stand for 0.5h.
[0034] The composition of the slag before and after the treatment of the solid slag from converter steelmaking in this embodiment is shown in Table 2. As can be seen from Table 2, after being treated by the method of the present invention, the P2O5 content in the slag is reduced from 5.43wt% to 0.33wt%, and the total iron content is reduced from 16.26wt% to 11.31wt%. The dephosphorization and iron selection effects are significant. The treated slag can be directly added to the converter steelmaking process as a slag-making agent to achieve efficient utilization of the solid slag from converter steelmaking.
[0035] Table 2 Solid slag composition before and after treatment (wt%)
[0036]
[0037] Comparative Example 1
[0038] The difference from Example 2 is that no catalyst is added during the treatment process.
[0039] The composition comparison of the solid slag from converter steelmaking in this comparative example before and after the treatment is shown in Table 3. It can be seen from Table 3 that after being treated by the method of the present invention, the P2O5 content in the slag is reduced from 5.43wt% to 1.67wt%, and the total iron content is reduced from 16.26wt% to 12.41wt%. The dephosphorization effect of this comparative example is worse than that of Example 2, and the iron selection effect is worse than that of Example 2. The treated slag cannot be directly added to the converter steelmaking process for utilization.
[0040] Table 3 Solid slag composition before and after treatment (wt%)
[0041]
[0042]
[0043] Comparative Example 2
[0044] The difference from Example 2 is that no Fe2O3 is added during the treatment process.
[0045] The composition comparison of the solid slag from converter steelmaking in this comparative example before and after the treatment is shown in Table 4. As can be seen from Table 4, after being treated by the method of the present invention, the P2O5 content in the slag is reduced from 5.43wt% to 1.48wt%, and the total iron content is reduced from 16.26wt% to 12.37wt%. The dephosphorization effect of this comparative example is not ideal, and the iron selection effect is poor. The treated slag cannot be directly added to the converter steelmaking process for utilization.
[0046] Table 4 Solid slag composition before and after treatment (wt%)
[0047]
[0048] The present invention performs dephosphorization and iron selection treatment on solid steel slag based on the steel slag classification system, and can obtain a higher dephosphorization and iron selection efficiency. The phosphorus content in the slag after dephosphorization is low, and it can be directly reused in the converter steelmaking process, and finally achieve the purpose of efficient utilization of converter solid steel slag. The method is simple and reliable, with high dephosphorization efficiency. It can not only solve the problem of large solid steel slag inventory and large environmental pollution, but also reduce the consumption of slag-making materials in converter steelmaking, shorten the pretreatment time, reduce slag-making heat loss, and increase the economic benefits of steel enterprises. It has important reference and guiding significance for the efficient recycling of metallurgical industrial waste slag.
[0049] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or direct / indirect application in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for recycling solid steel slag based on a grading system, It is characterized in that The following steps are involved: S1. Detect the parameters of solid steel slag and establish a solid steel slag quality data set; S2. Select solid steel slag classification indicators and formulate solid steel slag classification system; S3. Design a matching treatment mode for different levels of solid slag; S4. Obtain parameters of the solid slag to be processed and select a corresponding processing mode for processing.
2. The method for recycling solid slag based on a grading system according to claim 1, It is characterized in that In the step S1, the solid slag quality data set includes: density, particle size, main components, and production batch.
3. The method for recycling solid slag based on a grading system according to claim 1, It is characterized in that In the step S2, the solid steel slag classification index includes the main components of the solid steel slag and their contents.
4. The method for recycling solid slag based on a grading system according to claim 1, It is characterized in that In step S2, the grading system of the main components of solid steel slag and their contents is based on the phosphorus content detected: a phosphorus content of less than 1wt% is defined as low-phosphorus solid steel slag, a phosphorus content of 1-3wt% is defined as medium-phosphorus solid steel slag, and a phosphorus content of more than 3wt% is defined as high-phosphorus solid steel slag.
5. The method for recycling solid slag based on a classification system according to claim 4, It is characterized in that In step S2, the grading system of the main components of solid steel slag and their contents is based on the total iron content detected: the total iron content of solid steel slag is divided based on 20wt%, wherein solid steel slag with a total iron content ≤20wt% is defined as low-iron solid steel slag, and solid steel slag with a total iron content >20wt% is defined as high-iron solid steel slag.
6. The method for recycling solid slag based on a classification system according to claim 5, It is characterized in that In step S2, the solid steel slag is divided into six levels according to the phosphorus content and the total iron content of the solid steel slag, namely, low phosphorus and low iron, low phosphorus and high iron, medium phosphorus and low iron, medium phosphorus and high iron, high phosphorus and low iron, and high phosphorus and high iron.
7. The method for recycling solid slag based on a classification system according to claim 6, It is characterized in that In step S3, a processing mode matching different levels of solid steel slag is designed, specifically: Low-phosphorus and low-iron solid steel slag treatment mode: low-phosphorus and low-iron solid steel slag does not need to be treated; Low-phosphorus high-iron solid slag treatment mode: Low-phosphorus high-iron solid slag needs to be treated with iron selection. The temperature is maintained at 1300-1500℃ during melting in the induction heating furnace. After melting, it is kept warm for 10-20 minutes. At the same time, argon is blown at the bottom to stir the molten pool evenly. The argon flow rate is 100-300Nm 3 / (h·t 渣 ), the temperature of the argon gas is 1200-1400°C; after the insulation is completed, it is allowed to stand for 0.5-1h to allow the slag and the molten metal to separate, and the molten metal flows out from the tapping port for recovery; Medium phosphorus low iron solid steel slag treatment mode: Medium phosphorus low iron solid steel slag needs to be dephosphorized. The treatment process is: add Fe 2 O 3 , the added mass is 5-15% of the total mass of solid steel slag; then add medium-phosphorus and low-iron solid steel slag, and add carbonaceous reducing agent along with the slag flow. The amount of carbonaceous reducing agent added is to reduce the FeO and P in the slag. 2 O 5 1 to 1.5 times the amount of carbonaceous reducing agent required for complete reduction; then heat to 1300 to 1500°C to melt the steel slag, keep it warm for 10 to 20 minutes after melting, and blow argon gas from the bottom to stir the molten pool evenly while keeping it warm. The argon gas flow rate is 100 to 300 Nm 3 / (h·t 渣 ), the temperature of the argon gas is 1200-1400°C; after the insulation is completed, it is left to stand for 0.5-1h to separate the slag and the molten metal; the phosphorus vapor is collected by the phosphorus recovery device on the upper part of the furnace body, and the molten metal flows out through the steel outlet for recovery; Medium phosphorus high-speed iron solid slag treatment mode: Medium phosphorus high-speed iron solid slag needs to be dephosphorized and iron selected. The treatment process is: add medium phosphorus high-speed iron solid slag, add carbonaceous reducing agent with slag flow, and the amount of carbonaceous reducing agent added is to reduce the FeO and P in the slag. 2 O 5 1 to 2 times the amount of carbonaceous reducing agent required for complete reduction; then heat to 1300-1500℃ to melt the steel slag, keep it warm for 10-20min after melting, and blow argon gas at the bottom to stir the molten pool evenly while keeping it warm. The argon gas flow rate is 100-300Nm 3 / (h·t 渣 ), the temperature of the argon gas is 1200-1400°C; after the insulation is completed, it is left to stand for 0.5-1h to separate the slag and the molten metal; the phosphorus vapor is collected by the phosphorus recovery device on the upper part of the furnace body, and the molten metal flows out through the steel outlet for recovery; High-phosphorus and low-iron solid steel slag treatment mode: High-phosphorus and low-iron solid steel slag needs to be dephosphorized. The treatment process is: add Fe 2 O 3 , the added mass is 5-15% of the total mass of solid steel slag; then high-phosphorus and low-iron solid steel slag is added, and carbonaceous reducing agent and catalyst are added with the slag flow. The catalyst is heavy metal industrial waste slag including red mud, copper slag, and nickel slag. The amount of carbonaceous reducing agent added is to reduce the FeO and P in the slag. 2 O 5 The amount of carbonaceous reducing agent required for complete reduction is 1 to 1.5 times, and the amount of catalyst added is 0.2 to 0.5 times the amount of high-phosphorus, low-iron solid steel slag; then heat to 1300 to 1500 ° C to melt the steel slag, keep it warm for 10 to 20 minutes after melting, and blow argon gas from the bottom to stir the molten pool evenly while keeping it warm. The argon gas flow rate is 100 to 300 Nm 3 / (h·t 渣 ), the temperature of the argon gas is 1200-1400°C; after the insulation is completed, it is left to stand for 0.5-1h to separate the slag and the molten metal; the phosphorus vapor is collected by the phosphorus recovery device on the upper part of the furnace body, and the molten metal flows out through the steel outlet for recovery; High-phosphorus high-iron solid steel slag treatment mode: High-phosphorus high-iron solid steel slag needs to be dephosphorized and iron selected. The treatment process is: add high-phosphorus high-iron solid steel slag, add carbonaceous reducing agent and catalyst with the slag flow, the catalyst is heavy metal industrial waste slag including red mud, copper slag, nickel slag, the amount of carbonaceous reducing agent added is to reduce the FeO and P in the slag. 2 O 5 The amount of carbonaceous reducing agent required for complete reduction is 1 to 1.5 times, and the amount of catalyst added is 0.2 to 0.5 times the amount of high-phosphorus and high-iron solid steel slag; then heat to 1300 to 1500 ° C to melt the steel slag, and keep it warm for 10 to 20 minutes after melting. While keeping warm, blow argon gas from the bottom to stir the molten pool evenly, and the argon gas flow rate is 100 to 300 Nm 3 / (h·t 渣 ), the temperature of argon gas is 1200~1400℃; after the insulation is completed, it is left to stand for 0.5~1h to allow the slag and the molten metal to separate; the phosphorus vapor is collected by the phosphorus recovery device on the upper part of the furnace body, and the molten metal flows out through the steel outlet for recovery.
8. The method for recycling solid slag based on a classification system according to claim 1, It is characterized in that The treated steel slag is directly added to the converter steelmaking process as a converter slag-making agent, with an addition amount of 5-8 kg / t 钢 .
Citation Information
Patent Citations
Blast furnace ironmaking production process by cyclically utilizing steel slag and iron slag in metallurgy and chemical industry
CN101532068A
Method for enabling high-phosphorus steel slag fine powder to take part in ingredient mixing
CN110042179A
Method for preparing phosphorus-rich slag by separating iron and phosphorus from steel slag and then oxidizing
CN112746141A
Classification treatment and resource utilization method for steel slag
CN115354091A
Converter steel slag thermal-state cycle full-amount utilization method
CN118166172A
Cited By
Copper slag recovery method and copper slag recovery system
CN120738478A
Copper residue recovery method and copper residue recovery system
CN120738478B