Process for extracting lithium from bauxite through high-temperature roasting of sulfate
The lithium extraction method from bauxite is solved by the sulfate high-temperature roasting process, which is complicated, low purity and low recovery in the existing technology of bauxite lithium extraction methods, and achieves efficient, economical and environmentally friendly lithium resource utilization, which is suitable for use in the existing technology. Industrialized production.
Patent Information
- Application Number
- CN202410980366.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-22
AI Technical Summary
Existing bauxite lithium extraction methods such as acid leaching and alkali leaching methods are complex in operations, the lithium purity is not high, there are many impurities, the lithium recovery rate is low, and the resource waste is serious, making it difficult to achieve industrialization and industrial production.
Using the high-temperature sulfate roasting process, lithium is extracted from bauxite, and bauxite powder is mixed with sulfate mixed salt additives and roasted in a rotary kiln, and then leaching with dilute aqueous sulfuric acid solution for washing and solid-liquid separation. Combined with disodium EDTA and sodium carbonate, and finally obtained a refined lithium solution through purification.
It achieves simple operation, good control performance, high lithium extraction purity, high lithium recovery rate, high resource utilization rate, suitable for industrial and industrial production, and has a stable and continuous process, making it easy to achieve the unity of economic and environmental benefits.
Smart Images

Figure CN118910427A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of aluminum oxide and material processing thereof, and in particular to a process for extracting lithium from bauxite by high-temperature roasting of sulfate. Background Art
[0002] In addition to the typical chemical elements of aluminum, silicon, and iron, bauxite is usually enriched with some valuable metal elements that are crucial to modern industry during the mineralization process, such as lithium, vanadium, potassium, gallium, scandium, titanium, niobium, and tantalum, which makes bauxite gradually become one of the important sources of these key metal minerals. At present, the main way to obtain lithium resources from bauxite is to chemically treat bauxite and then extract lithium. The existing methods for extracting lithium from bauxite mainly include acid leaching, alkaline leaching, etc. Among them, acid leaching and alkaline leaching are more common methods. However, acid leaching and alkaline leaching have the defects of complex operation, low purity of extracted lithium, more impurities, low lithium recovery rate, and serious waste of resources, which are not conducive to industrialization and industrial production. Summary of the invention
[0003] The object of the present invention is to provide a process for extracting lithium from bauxite by high temperature roasting of sulfate, so as to solve the problems raised in the above background technology.
[0004] To achieve the above object, the present invention provides the following technical solutions: A process for extracting lithium from bauxite by high-temperature calcination of sulfate, comprising the following steps: S1, mixing bauxite powder and sulfate mixed salt additive to obtain a mixture, subjecting the mixture to aging treatment, feeding the aged mixture into a rotary kiln, and roasting it at a high temperature to obtain a clinker; S2, mixing the clinker obtained in step S1 with water and then ball-milling it, then leaching it with a dilute sulfuric acid aqueous solution to obtain a lithium sulfate solid-liquid mixture, and performing a first solid-liquid separation on the lithium sulfate solid-liquid mixture to obtain a leached residue and a leachate; S3, after washing the leached residue obtained in step S2, the washing liquid is combined with the leached liquid obtained in step S2, and evaporated and concentrated to obtain a lithium production solution, the pH of the lithium production solution is adjusted to a strong alkaline state, and then disodium EDTA and an aqueous sodium carbonate solution are added to react, and the reaction product is subjected to a second solid-liquid separation to obtain a preliminary lithium solution and a filter residue, and the filter residue is treated as a raw material for an aluminum plant; S4. Purify the preliminary lithium solution obtained in step S3 to obtain a refined lithium solution.
[0005] Preferably, the mass ratio of the bauxite powder and the sulfate mixed salt additive in step S1 is (70-80): (20-30).
[0006] Preferably, the water content of the mixture in step S1 is ≤1wt%, and the proportion of 60-80 mesh particles is ≥80%.
[0007] Preferably, the aging temperature in step S1 is room temperature and the time is ≥12h.
[0008] Preferably, the rotary kiln in step S1 uses water gas, natural gas or coal powder as fuel, the roasting temperature of the rotary kiln is 900° C. to 950° C., and the roasting time is 40 to 60 min.
[0009] Preferably, in step S2, the mass ratio of clinker to water is (0.85-0.95):1, the pH of the dilute sulfuric acid aqueous solution leaching is 3-4, the temperature is room temperature, and the time is 1h-2h.
[0010] Preferably, the lithium content in the leached slag after washing in step S3 is ≤0.09wt%, and the leached slag after washing is used as raw material for an aluminum plant.
[0011] Preferably, the pH corresponding to the strong alkalinity in step S3 is ≥ 12.5, the reaction time is 30 min, and the temperature is 80-95°C.
[0012] Preferably, the carbonate concentration of the sodium carbonate aqueous solution in step S3 is 96-107 g / L, the dosage of the sodium carbonate aqueous solution is 1.5-2.5 times the theoretical value, and the dosage of disodium EDTA is 1.5 times the theoretical value.
[0013] Preferably, the purification in step S4 uses chelating resin D401 to remove impurities from calcium and magnesium ions. In the refined lithium-making solution, the total content of calcium and magnesium ions is ≤5ppm, and the lithium ion content is ≥10g / L. When the lithium ion content is <10g / L, return to step S3 for evaporation and concentration.
[0014] Compared with the prior art, the present invention has the following beneficial effects: The present application provides a process for extracting lithium from bauxite using a rotary kiln, comprising the steps of subjecting the bauxite to coarse crushing, medium crushing, fine crushing and grinding and powdering pretreatment to obtain bauxite powder, mixing the bauxite powder and a sulfate mixed salt additive to obtain a mixture, aging the mixture, feeding the mixture into a rotary kiln, and roasting the mixture under boiling conditions to obtain a clinker; mixing the clinker with water and ball milling the mixture, leaching the mixture with a dilute sulfuric acid aqueous solution to obtain a lithium sulfate salt solid-liquid mixture, and performing a first solid-liquid separation to obtain a leached residue and a leached liquid; washing the leached residue, combining the washing liquid with the leached liquid, evaporating and concentrating the mixture to obtain a lithium preparation solution, adjusting the pH of the lithium preparation solution to a strong alkaline state, then adding disodium EDTA and an aqueous sodium carbonate solution to react, and performing a second solid-liquid separation on the reaction product to obtain a preliminary lithium solution and a filter residue; purifying the preliminary lithium solution to obtain a refined lithium solution, and the filter residue is used as a raw material for an aluminum plant. This lithium extraction process has the advantages of simple operation, good control performance, high lithium extraction purity, and high lithium recovery rate. It achieves the unity of economic and environmental benefits, enables comprehensive utilization of effective resources, and the entire process can achieve stable and continuous operation, which is easy to industrialize and industrialize. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a process flow chart of the present invention; Figure 2 It is the test record of lithium extraction by the process of the present invention; Figure 3 This is a comparison table of lithium carbonate test results between the embodiment and the comparative example; DETAILED DESCRIPTION
[0016] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0017] A process for extracting lithium from bauxite by high temperature roasting of sulfate, the process flow is as follows Figure 1 As shown, the process experiment record is as follows Figure 2 As shown, the following steps are included: S1, subjecting bauxite to coarse crushing, medium crushing, fine crushing and grinding and powdering pretreatment steps to obtain bauxite powder, mixing the bauxite powder and a sulfate mixed salt additive to obtain a mixture, aging the mixture, feeding the aged mixture into a rotary kiln, and roasting it at a high temperature to obtain a clinker; S2, mixing the clinker obtained in step S1 with water and then ball-milling it, then leaching it with a dilute sulfuric acid aqueous solution to obtain a lithium sulfate solid-liquid mixture, and performing a first solid-liquid separation on the lithium sulfate solid-liquid mixture to obtain a leached residue and a leachate; S3, after washing the leached residue obtained in step S2, the washing liquid is combined with the leached liquid obtained in step S2, and evaporated and concentrated to obtain a lithium preparation solution, the pH of the lithium preparation solution is adjusted to a strong alkaline state, and then disodium EDTA and an aqueous sodium carbonate solution are added to react, and the reaction product is subjected to a second solid-liquid separation to obtain a preliminary lithium solution and a filter residue, and the filter residue is treated as a raw material for an aluminum plant; S4. Purify the preliminary lithium solution obtained in step S3 to obtain a refined lithium solution.
[0018] The reaction mechanism is as follows: 1.Li2O·6Al2O3·SiO2+Na2SO4→ Na2O·6Al2O3·SiO2 +Li2SO4 (900-950℃); 2.Li2O·6Al2O3·SiO2 + K2SO4→K2O·6Al2O3·SiO2 + Li2SO4 (900-950℃); The high-temperature roasting in a rotary kiln causes the valuable metal lithium ions in bauxite and the sodium and potassium ions in the sulfate mixed salt additive to undergo "solid-solid mass transfer and phase reorganization" in the molten state to form soluble lithium sulfate, which can be extracted efficiently.
[0019] In an optional embodiment, the mass ratio of bauxite powder to sulfate mixed salt additive in step S1 is (70-80): (20-30).
[0020] Optionally, the mass ratio of bauxite to sulfate mixed salt additive may be 70:30, 65:35, 80:20, or any value between (70-80): (20-30).
[0021] In an optional embodiment, the water content of the mixture in step S1 is ≤1wt%, and the proportion of 60-80 mesh particles is ≥80%.
[0022] Optionally, the water content of the mixture can be 0.1wt% or 0.5wt% or 1wt% or any value ≤1wt%, and the proportion of 60-80 mesh particles can be 80% or 90% or any value not less than 80%.
[0023] In an optional embodiment, the aging temperature in step S1 is room temperature and the time is ≥12h.
[0024] In an optional embodiment, in step S1, the rotary kiln uses water gas, natural gas, or pulverized coal as fuel, the roasting temperature of the rotary kiln is 900° C. to 950° C., and the roasting time is 40 to 60 minutes.
[0025] Optionally, the rotary kiln roasting temperature can be 900°C, 910°C, 920°C, 950°C, or any value between 900°C and 950°C, and the roasting time can be 40 min, 50 min, 60 min, or any value between 40 and 60 min.
[0026] In an optional embodiment, the mass ratio of clinker to water in step S2 is (0.85-0.95):1, the pH of the dilute sulfuric acid aqueous solution leaching is 3-4, the temperature is room temperature, and the time is 1h-2h.
[0027] Optionally, the mass ratio of clinker to water can be 0.85:1 or 0.87:1 or 0.9:1 or 0.95:1 or any value between (0.85 and 0.95):1, the pH of the leaching of dilute sulfuric acid aqueous solution can be 3 or 3.5 or 4 or any value between 3 and 4, and the time can be 1h or 1.5h or 2h or any value between 1h and 2h.
[0028] In an optional embodiment, the lithium content in the leached slag after washing in step S3 is ≤0.09wt%, and the leached slag after washing is used as a raw material for an aluminum plant.
[0029] In an optional embodiment, in step S3, the pH corresponding to the strong alkalinity is ≥ 12.5, the reaction time is 30 min, and the temperature is 80-95°C.
[0030] In an optional embodiment, the carbonate concentration of the sodium carbonate aqueous solution in step S3 is 96-107 g / L, the amount of the sodium carbonate aqueous solution used is 1.5-2.5 times the theoretical value, and the amount of disodium EDTA used is 1.5 times the theoretical value.
[0031] Optionally, the carbonate concentration of the sodium carbonate aqueous solution can be 96 g / L or 100 g / L or 107 g / L or any value between 96 and 107 g / L, and the dosage of the sodium carbonate aqueous solution can be 1.5 times or 2 times or 2.5 times or any value between 1.5 and 2.5 times the theoretical value.
[0032] In an optional embodiment, in step S4, chelating resin D401 is used to remove impurities from calcium and magnesium ions. In the refined lithium solution, the total content of calcium and magnesium ions is ≤5ppm, and the lithium ion content is ≥10g / L. When the lithium ion content is <10g / L, return to step S3 for evaporation and concentration. Example
[0033] A process for extracting lithium from bauxite by high-temperature calcination of sulfate, comprising the following steps: The bauxite is firstly crushed into particles with a size of 6-7cm by a rough crushing process, and then the coarsely crushed bauxite is medium-crushed into particles with a size of 4-5cm. The medium-crushed bauxite is then finely crushed into particles with a size of 1-2cm. The finely crushed bauxite is then ground and powdered for lithium treatment. After the powdered bauxite is sieved, the particle size distribution is 80 mesh ≥90%. The bauxite and sulfate mixed salt additive are mixed at a mass ratio of 70:30. The sulfate mixed salt is industrial grade, and its external The mixture is in the form of fine powder. After being stirred by a spiral mixer for 40 minutes, it becomes a mixture. The moisture content of the mixture is 0.95%, and the proportion of 80 mesh particles is 81.7%. The mixture is transported to the high-level silo by a spiral conveyor and aged for 14 hours. The mixture is pre-treated by mechanical activation. With water gas as fuel, the aged mixture enters the kiln from the kiln tail of the rotary kiln and is discharged from the kiln head of the rotary kiln. The residence time of the mixture in the rotary kiln is 60 minutes. The roasting temperature is 900℃±10℃, and the operation is stable. The roasted clinker is fully ball-milled with water, and the pH is adjusted to 4 with dilute sulfuric acid. The leaching water is washed and treated. After ball milling, a soluble lithium sulfate solid-liquid mixture is formed. The mass ratio of roasted clinker and water is controlled to be 0.85:1, the temperature of the leaching water is room temperature, and the leaching time is 1h. The solid-liquid mixture of lithium sulfate salt is subjected to the first solid-liquid separation through a filtering device to obtain leached residue and leached liquid. The leached residue is reversely washed three times. The filtering device is a belt filter. The lithium ion concentration in the leached residue is controlled to be 0.09wt%. The leached residue after washing is used as a raw material for the aluminum plant. The leached liquid and washing liquid prepared above are combined to form a lithium solution A. The lithium solution A is evaporated and concentrated to obtain a lithium solution B. In order to obtain a qualified refined lithium solution, an appropriate amount of sodium hydroxide and lime milk are added to the lithium solution B to adjust the alkalinity to 12.5, and 1.5 times the theoretical value of disodium EDTA and 2 times the theoretical value of sodium carbonate aqueous solution (carbonate concentration is 95g / L) are added to react. The reaction time is 30min and the reaction temperature is 90°C. The second solid-liquid separation is carried out by filtration with a plate and frame filter press to remove impurities Ca 2+ Mg 2+ , Fe 3+ , Mn 2+ 、Al 3+ The filtrate is the preliminary lithium solution, and the residue is acidified, washed, recycled and reused as raw material for aluminum plant processing. The preliminary lithium solution in the previous step is deeply purified and impurities removed by chelating resin D401, and Ca 2+ Mg 2+ After removal, a refined lithium solution is obtained after purification. The Ca 2+ Mg 2+The mass concentration of ions is ≤5ppm, and the chelating resin D401 can be recycled after alkaline washing, acid washing, water washing and analysis. The mass concentration of lithium ions in the refined lithium solution is 11.20g / L, and the refined lithium solution becomes the raw material for the subsequent lithium precipitation module to prepare battery-grade lithium carbonate and battery-grade lithium hydroxide. From a practical point of view, the lithium extraction process has a high production operation rate and sustainable production, achieving a safe, stable and good operating state. Example
[0034] A process for extracting lithium from bauxite by high-temperature calcination of sulfate, comprising the following steps: The bauxite is firstly crushed into particles with a size of 6 to 7 cm by a rough crushing process. The coarsely crushed bauxite is then medium crushed into particles with a size of 4 to 5 cm. The medium crushed bauxite is then finely crushed into particles with a size of 1 to 2 cm. The finely crushed bauxite is then ground and powdered for lithium pretreatment. The powdered bauxite is sieved to a particle size of 70 mesh ≥ 80%. The bauxite and sulfate mixed salt additive are mixed according to a mass ratio of 80:20, and a mixture is formed by stirring with a spiral mixer for 50 minutes. The moisture content of the mixture is 0.80%, and the particle size of 80 mesh is 90%. The mixture is transported to a high-level silo by a spiral conveyor, aged for 16 hours, and mechanically activated for pretreatment of the mixture. Water gas is used as fuel. The aged mixture enters the kiln from the kiln tail of the rotary kiln and is discharged from the kiln head of the rotary kiln. The mixture stays in the rotary kiln for 60 minutes, and the roasting temperature is 940℃±10℃, with stable operation. After the roasting, the clinker is fully ball-milled with water, and the pH value of the dilute sulfuric acid aqueous solution is adjusted to 3 with dilute sulfuric acid, and the leaching water is washed to form a soluble solid-liquid mixture of lithium sulfate salt. The mass ratio of the roasting clinker and water is controlled to be 0.95:1, the temperature of the leaching water is room temperature, and the leaching time is 1 hour. The solid-liquid mixture of lithium sulfate salt is subjected to the first solid-liquid separation through a filtering device to obtain leaching residue and leaching liquid. The leaching residue is reversely washed three times. The filtering device is a belt filter. The lithium ion concentration in the leaching residue is controlled to be 0.08wt%. The washed leaching residue is used as a raw material for the aluminum plant. The prepared leaching solution and washing solution are combined to obtain lithium solution A, and lithium solution A is evaporated and concentrated to obtain lithium solution B. In order to obtain qualified refined lithium solution, lithium solution B is added with appropriate amount of sodium hydroxide and lime milk to adjust the alkalinity to 12.9, and 1.5 times the theoretical value of disodium EDTA and 2 times the theoretical value of sodium carbonate aqueous solution (carbonate concentration is 100g / L) are added to react, the reaction time is 30min, and the reaction temperature is 95℃. The second solid-liquid separation is carried out by plate and frame filter press to remove impurities Ca 2+ Mg 2+ , Fe 3+ , Mn 2+ 、Al 3+The filtrate is the preliminary lithium solution, and the residue is acidified, washed, recycled and reused as raw material for aluminum plant processing. The preliminary lithium solution in the previous step is deeply purified and impurities removed by chelating resin D401, and Ca 2+ Mg 2+ After removal, a refined lithium solution is obtained after purification. The Ca 2+ Mg 2+ The ion mass concentration is ≤5ppm, and the chelating resin D401 can be recycled after alkali washing, acid washing, water washing and analysis. The lithium ion mass concentration in the refined lithium solution is 12.20g / L, and the refined lithium solution becomes the raw material for the subsequent lithium precipitation module to prepare battery-grade lithium carbonate and battery-grade lithium hydroxide. From a practical point of view, the lithium extraction process has a good production operation and sustainable production.
[0035] Comparative Example 1: The difference from Example 1 is that the lithium extraction method is different. Instead of using the form of high-temperature calcination of sulfate, an acid leaching method is used. After the industrial-grade sulfuric acid and bauxite are fully mixed, the sulfuric acid content is ≥98%. The other process technical parameters are controlled exactly the same. For specific test data, see Figure 3 .
[0036] Comparative Example 2: The difference from Example 1 is that the lithium extraction method is different. Instead of using the form of high-temperature roasting of sulfate, an alkali leaching method is used. After the industrial-grade liquid alkali and bauxite are fully mixed, the main content of the liquid alkali is ≥31%. The other process technical parameters are controlled exactly the same. The specific test data is shown in Figure 3 .
[0037] Figure 3 This is a comparison table of the test results of preparing lithium carbonate from lithium extraction using Example 1 and Example 2 of the process method of the present invention and Comparative Example 1 and Comparative Example 2.
[0038] pass Figure 3 It can be explained that the lithium extraction process provided by this application has a better guarantee for the quality of battery-grade lithium carbonate prepared by extracting lithium compared with conventional acid leaching and alkaline leaching. Through experimental comparison, the lithium carbonate products prepared by acid leaching or alkaline leaching of lithium from bauxite using other process methods, especially the same existing preparation process method and the same technical parameter control, the main content of lithium carbonate does not meet the national standard, and some impurity indicators are far from the national standard requirements. The lithium carbonate products prepared by the lithium extraction process provided by this application can be seen from Table 2 that they fully meet the national standard requirements for battery-grade lithium carbonate, achieve the unity of economic benefits and environmental benefits, and make comprehensive utilization of effective resources.
[0039] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A process for extracting lithium from bauxite by high temperature calcination of sulfate, characterized in that: The following steps are involved: S1, mixing bauxite powder and sulfate mixed salt additive to obtain a mixture, subjecting the mixture to aging treatment, feeding the aged mixture into a rotary kiln, and roasting it at a high temperature to obtain a clinker; S2, mixing the clinker obtained in step S1 with water and then ball-milling it, then leaching it with a dilute sulfuric acid aqueous solution to obtain a lithium sulfate solid-liquid mixture, and performing a first solid-liquid separation on the lithium sulfate solid-liquid mixture to obtain a leached residue and a leachate; S3, after washing the leached residue obtained in step S2, the washing liquid is combined with the leached liquid obtained in step S2, and evaporated and concentrated to obtain a lithium production solution, the pH of the lithium production solution is adjusted to a strong alkaline state, and then disodium EDTA and an aqueous sodium carbonate solution are added to react, and the reaction product is subjected to a second solid-liquid separation to obtain a preliminary lithium solution and a filter residue, and the filter residue is treated as a raw material for an aluminum plant; S4. Purify the preliminary lithium solution obtained in step S3 to obtain a refined lithium solution.
2. The lithium extraction process according to claim 1, characterized in that: The mass ratio of the bauxite powder and the sulfate mixed salt additive in step S1 is (70-80): (20-30).
3. The lithium extraction process according to claim 1, characterized in that: The water content of the mixture in step S1 is ≤1wt%, and the proportion of 60-80 mesh particles is ≥80%.
4. The lithium extraction process according to claim 1, characterized in that: In step S1, the aging temperature is room temperature and the time is ≥12h.
5. The lithium extraction process according to claim 1, characterized in that: The rotary kiln in step S1 uses water gas, natural gas, and coal powder as fuel, and the roasting temperature of the rotary kiln is 900° C. to 950° C., and the roasting time is 40 to 60 minutes.
6. The lithium extraction process according to claim 1, characterized in that: The mass ratio of clinker to water in step S2 is (0.85-0.95):1, the pH of the dilute sulfuric acid aqueous solution leaching is 3-4, the temperature is room temperature, and the time is 1h-2h.
7. The lithium extraction process according to claim 1, characterized in that: The lithium content in the leached slag after washing in step S3 is ≤0.09wt%, and the leached slag after washing is used as raw material for an aluminum plant.
8. The lithium extraction process according to claim 1, characterized in that: The strong alkalinity in step S3 corresponds to a pH of ≥12.5, the reaction time is 30 min, and the temperature is 80-95° C.
9. The lithium extraction process according to claim 1, characterized in that: The carbonate concentration of the sodium carbonate aqueous solution in step S3 is 96-107 g / L, the dosage of the sodium carbonate aqueous solution is 1.5-2.5 times the theoretical value, and the dosage of disodium EDTA is 1.5 times the theoretical value.
10. The lithium extraction process according to any one of claims 1 to 9, characterized in that: The purification in step S4 uses chelating resin D401 to remove impurities from calcium and magnesium ions. In the refined lithium solution, the total content of calcium and magnesium ions is ≤5ppm, and the lithium ion content is ≥10g / L. When the lithium ion content is <10g / L, return to step S3 for evaporation and concentration.
Citation Information
Patent Citations
Method for extracting lithium from lithium chinastone mineral by roasting with mixed sulfate method
CN113999970A
Method for extracting lithium from lepidolite by using fluidized bed
CN115947352A
Comprehensive utilization method of bauxite
CN117535512A
Aluminum and lithium synergistic extraction method for lithium-containing low-grade bauxite