Method for recovering germanium from high-grade germanium-containing material
Through the fire treatment method, a single crystal furnace is used to perform vacuuming, argon replacement, melting and decomposition purification steps of germanium materials, solving the problems of low recovery rate and difficult waste liquid treatment in germanium materials processing, and achieving high efficiency and economical germanium recycling reaches a recovery rate of more than 98%.
Patent Information
- Application Number
- CN202410977334.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art has problems such as low recovery rate, long process, and difficulty in treating waste liquids during the processing of germanium materials, and the fire treatment method has not been used.
By using the fire treatment method, the germanium recovery is achieved through the vacuuming, argon replacement, melting, decomposition purification and cooling and cooling steps of a single crystal furnace, which can effectively recover germanium, avoid the generation of waste liquid and improve the recovery rate of germanium.
The recovery rate of germanium is achieved by reaching more than 98%, simplifying the processing process, reducing costs, and effectively removing impurities, significantly improving the recycling efficiency of germanium.
Abstract
Description
Technical Field
[0001] The present application relates to the field of metallurgical technology, and in particular to a method for recovering germanium from high-grade germanium-containing materials. Background Art
[0002] In the process of germanium material processing, such as the cutting process of germanium blank, the cutting process of germanium single crystal and the cutting process of zone melting germanium, a large amount of high-grade germanium-containing materials will be produced. The traditional method for processing this part of high-grade germanium-containing materials is to collect them centrally, filter them with a filter press for dehydration, ball mill them, and dry them to prepare germanium mud, and then use FeCl3 and HCl mixed leaching and distillation to recover germanium metal, or use hydrogen peroxide and sodium hydroxide for oxidation reaction, and then perform chlorination distillation to generate germanium tetrachloride to recover germanium.
[0003] Specifically, when FeCl3 and HCl are used as mixed solvents for leaching, there are problems such as the generation of a large amount of waste acid and waste residue, which are difficult to handle later. In addition, this treatment method often involves ball milling and the process of transporting the germanium powder material over long distances and inverting it, resulting in an overall low germanium recovery rate of about 93%.
[0004] The method of oxidizing the germanium mud with hydrogen peroxide and sodium hydroxide and then recovering it by chlorination distillation has the problem that it is difficult to fully oxidize the germanium mud. On the other hand, the treated germanium oxide needs to be distilled, re-distilled, rectified, hydrolyzed and reduced to generate metallic germanium. The overall processing process is too long. Similarly, the recovery rate of germanium is only about 94%.
[0005] There is no report on the use of pyrometallurgy to treat germanium mud in the prior art.
[0006] How to process these high-grade germanium-containing materials obtained in the germanium material processing process economically and efficiently so as to shorten the processing flow, reduce the processing cost, avoid the treatment of waste liquid, and improve the germanium recovery rate has always been a technical problem that needs to be solved urgently by technical personnel in this field. Summary of the invention
[0007] In order to solve or partially solve the problems existing in the related art, the present application provides a method for recovering germanium from high-grade germanium-containing materials. Compared with the existing wet treatment process, this method adopts a pyrolysis method for treatment, has a short process and does not produce any waste liquid during the treatment process. At the same time, the recovery rate of germanium is as high as more than 98%, and this method has a good effect in removing impurities.
[0008] The method for recovering germanium from a high-grade germanium-containing material in the present application comprises the following steps:
[0009] (1) Vacuuming and replacing with argon gas
[0010] The dried germanium-containing material is placed in a crucible of a single crystal furnace, and the single crystal furnace is evacuated and then filled with argon gas for replacement treatment;
[0011] (2) Maintain a certain vacuum degree in the single crystal furnace, and fill a certain amount of argon gas into the single crystal furnace to maintain the argon atmosphere in the furnace;
[0012] (3) Melting materials
[0013] First, heat up to fully melt the germanium-containing material, then lower the temperature to control the liquid surface temperature at 937-950°C; the melting point of germanium is 937.4°C, and controlling the liquid surface temperature at 937-950°C can fully melt the germanium metal;
[0014] (4) Impurity removal and purification
[0015] The crucible is turned on and a heavy hammer with a seed crystal is lowered from the top of the single crystal furnace. A crystal block is grown by seeding and shouldering. After the crystal block grows to a certain size, the seed crystal is lifted to a certain height above the liquid surface for cooling. After cooling for a period of time, the crucible rotation speed is reduced, and the seed crystal position is lowered so that the bottom surface of the crystal block contacts the scum gathered on the liquid surface. The scum adheres to the crystal block, and the crystal block is lifted to a certain height above the liquid surface. The above operation process is repeated several times to complete the impurity removal and purification.
[0016] (5) Cooling the ingot
[0017] After the impurity removal and purification are completed, the heating power of the single crystal furnace is gradually reduced to 0kw through power control, the crucible rotation is turned off, and after the metal liquid is fully cooled and solidified, the furnace cover is opened and the germanium metal block that has been cast is taken out.
[0018] Optionally, in some embodiments, in the step (4), after the crystal block grows to a diameter of 50-100 mm, the seed crystal is raised to a position 50-200 mm above the liquid surface for cooling, the cooling time is 2-10 min, the crucible rotation speed is reduced to less than or equal to 2 r / min, and the seed crystal is lowered so that the bottom surface of the crystal block contacts the scum gathered on the liquid surface, the crystal block is lifted to 50-200 mm above the liquid surface, and the scum is attached to the crystal block, and the above operation process is repeated 3-5 times to complete the impurity removal and purification.
[0019] Optionally, in some embodiments, when melting the material in step (3), the power is increased to a temperature of 1000-1100°C in 3-5 times evenly within 1 hour to fully melt the germanium-containing material, and then the temperature is lowered to control the liquid surface temperature at 937-950°C.
[0020] Optionally, in some embodiments, in step (2), the vacuum degree in the single crystal furnace is below 200 mTorr, and the gas pressure in the furnace is 10-20 Torr.
[0021] Optionally, in some embodiments, the germanium-containing material in step (1) has a water content of <0.01%.
[0022] Optionally, in some embodiments, in step (5), the power is gradually reduced to 0 kW in 2-3 times within 1 hour, the crucible rotation is turned off, and the temperature in the furnace is waited for 6-12 hours to drop below 50° C. before opening the furnace cover and taking out the completed germanium metal block.
[0023] The technical solution provided by this application may have the following beneficial effects:
[0024] 1. This application realizes the efficient treatment of germanium mud for the first time. Based on the existing single crystal furnace equipment, the single crystal furnace is vacuumed, argon gas is passed to replace the gas, and then the germanium mud is heated to melt, thereby preventing the raw material from being oxidized; and the melted material is removed from impurities and cooled to finally prepare a germanium metal block. In particular, in the process of removing impurities from the melted material, based on the CZ method, the process of crystal growth is introduced, and the removal of impurities and the growth of crystals are combined. After the crystal block grows to a certain size, the seed crystal position is lifted to a certain height above the metal liquid surface for cooling and cooling. After cooling and cooling for a period of time, the crucible rotation speed is reduced, and the seed crystal position is lowered so that the bottom surface of the crystal block contacts the scum gathered on the metal liquid surface, and the crystal block is lifted again to a certain height above the liquid surface, and the scum is attached to the crystal block; repeat the above operation process several times, that is, the impurity removal and purification of the melted material are completed, and a germanium metal block with higher purity is prepared. The pyrometallurgical treatment of germanium mud in this application has a germanium recovery rate of more than 98%, which is significantly higher than the germanium recovery rate of germanium mud treatment in the prior art.
[0025] 2. The method in the present application is based on the use of pyrometallurgical treatment throughout the entire process, which completely avoids the problem of difficult treatment of waste liquid generated by the prior art when treating germanium mud using wet methods, i.e., mixed leaching and distillation of FeCl3 and HCl, or oxidation reaction followed by chlorination and distillation using hydrogen peroxide and sodium hydroxide. DETAILED DESCRIPTION
[0026] The embodiments of the present application will be described in more detail below with reference to examples. Although the embodiments of the present application are shown in the examples, it should be understood that the present application can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present application more thorough and complete, and the scope of the present application can be fully communicated to those skilled in the art.
[0027] Example 1
[0028] The method for recovering germanium from germanium mud in this embodiment uses a single crystal furnace in the prior art, wherein the single crystal furnace is connected to a vacuum system, which consists of a vacuum pump, a vacuum pipeline, a vacuum gauge, an argon tank, a pipeline valve, and a pressure gauge.
[0029] Specifically, the recycling method comprises the following steps:
[0030] (1) Vacuuming and replacing with argon gas
[0031] Put the dried germanium mud into a graphite crucible, and put the graphite crucible into the single crystal furnace body, and cover the furnace cover; evacuate the single crystal furnace and fill it with argon gas for replacement treatment, specifically: open the vacuum pump valve, adjust the valve opening to 95%, evacuate the furnace to 0.6 Torr, open the charging valve to charge argon, adjust the charging valve flow rate to 100 slpm, and close the charging valve after charging for 5 minutes;
[0032] The germanium mud is obtained from germanium scraps during the cutting process of germanium blanks, the cutting process of germanium single crystals and the cutting process of zone melting germanium. Since it is accompanied by cutting fluid and coolant, the above-mentioned materials containing water and germanium are filtered and dried in sequence. In this embodiment, the moisture content of the dried germanium mud is less than 0.1%; the germanium mud contains 92%-96% germanium;
[0033] (2) Maintaining the vacuum degree in the single crystal furnace at 150 mTorr, and filling a certain amount of argon gas into the single crystal furnace to maintain the argon atmosphere in the furnace. Specifically, the pressure in the furnace is controlled to be 10 Torr;
[0034] (3) Melting materials
[0035] Turn on the heating button and increase the power to the highest power of the equipment 5 times within 1 hour. When the temperature in the furnace rises to 1000℃, switch the power control to SP temperature control and wait for the material in the crucible to melt. After observing the material melting, lower the SP temperature value and control the liquid surface temperature at 937-950℃;
[0036] (4) Impurity removal and purification
[0037] Start the crucible rotation, lower the heavy hammer with seed crystal from the top of the single crystal furnace, grow a crystal block through seeding and shouldering; after the crystal block grows to a diameter of 50-100mm, lift the seed crystal position to 200mm above the liquid surface for cooling and cooling for 5min, reduce the pan speed to 1r / min, observe that the scum on the liquid surface gathers in the center of the liquid surface, and lower the seed crystal position so that the bottom surface of the crystal block contacts the scum gathered on the liquid surface, lift the crystal block to 50-200mm above the liquid surface, and some scum will adhere to the crystal block; repeat the above operation process 3 times to complete the impurity removal and purification;
[0038] (5) Cooling the ingot
[0039] After the impurity removal and purification are completed, the heating power of the single crystal furnace is gradually reduced to 0kw through power control, the crucible rotation is turned off, and after the metal liquid is fully cooled and solidified, the furnace cover is opened and the germanium metal block with a purity of 99% is taken out.
[0040] The scum on the crystal block can be separated from the crystal block by shearing or cutting.
[0041] Example 2
[0042] The method for recovering germanium from germanium mud in this embodiment uses the same equipment as in Example 1. The difference lies in some process control conditions. The specific method is as follows:
[0043] (1) Vacuuming and replacing with argon gas
[0044] Put the dried germanium mud into a graphite crucible, and put the graphite crucible into the single crystal furnace body, and cover the furnace cover; evacuate the single crystal furnace and fill it with argon gas for replacement treatment, specifically: open the vacuum pump valve, adjust the valve opening to 95%, evacuate the vacuum degree in the furnace to 0.8 Torr, open the charging valve to flush in argon, adjust the charging valve flow rate to 100 slpm, and close the charging valve after charging for 3 minutes;
[0045] The germanium mud is obtained from germanium scraps during the cutting process of germanium blanks, the cutting process of germanium single crystals and the cutting process of zone melting germanium. Since it is accompanied by cutting fluid and coolant, the above-mentioned materials containing water and germanium are filtered and dried in sequence. In this embodiment, the moisture content of the dried germanium mud is less than 0.1%; the germanium mud contains 92%-97% germanium;
[0046] (2) Maintaining the vacuum degree in the single crystal furnace at 180 mTorr, and filling a certain amount of argon gas into the single crystal furnace to maintain the argon atmosphere in the furnace. Specifically, the pressure in the furnace is controlled to be 20 Torr;
[0047] (3) Melting materials
[0048] Turn on the heating button and increase the power to the highest power of the equipment 4 times within 1 hour. When the temperature in the furnace rises to 1100℃, switch the power control to SP temperature control and wait for the material in the crucible to melt. After observing the material melting, lower the SP temperature value and control the liquid surface temperature at 937-950℃;
[0049] (4) Impurity removal and purification
[0050] Start the crucible rotation, lower the heavy hammer with seed crystal from the top of the single crystal furnace, grow a crystal block through seeding and shouldering; after the crystal block grows to a diameter of 50-100mm, lift the seed crystal position to 100mm above the liquid surface for cooling and cooling for 2min, reduce the pan rotation speed to 2r / min, observe that the scum on the liquid surface gathers in the center of the liquid surface, and lower the seed crystal position so that the bottom surface of the crystal block contacts the scum gathered on the liquid surface, lift the crystal block to 200mm above the liquid surface, and some scum will adhere to the crystal block; repeat the above operation process 4 times to complete the impurity removal and purification;
[0051] (5) Cooling the ingot
[0052] After the impurity removal and purification are completed, the heating power of the single crystal furnace is gradually reduced to 0kw through power control, the crucible rotation is turned off, and after the metal liquid is fully cooled and solidified, the furnace cover is opened and the ingot is taken out. The purity of the germanium metal block is 98%.
[0053] The embodiments of the present application have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or improvements to the technology in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.
Claims
1. A method for recovering germanium from a high-grade germanium-containing material, characterized in that: The process includes the following steps: (1) vacuuming and replacing with argon gas The dried germanium-containing material is placed in a crucible of a single crystal furnace, and the single crystal furnace is evacuated and then filled with argon for replacement treatment; (2) Maintain a certain vacuum degree in the single crystal furnace, and fill a certain amount of argon gas into the single crystal furnace to maintain the argon atmosphere in the furnace; (3) Melting materials First, heat up to fully melt the germanium-containing material, then lower the temperature to control the liquid surface temperature at 937-950℃; (4) Impurity removal and purification The crucible is turned on and a heavy hammer with a seed crystal is lowered from the top of the single crystal furnace. A crystal block is grown by seeding and shouldering. After the crystal block grows to a certain size, the seed crystal is lifted to a certain height above the liquid surface for cooling. After cooling for a period of time, the crucible rotation speed is reduced, and the seed crystal position is lowered so that the bottom surface of the crystal block contacts the scum gathered on the liquid surface. The scum is attached to the crystal block, and then the crystal block is lifted to a certain height above the liquid surface. The above operation process is repeated several times to complete the impurity removal and purification. (5) Cooling the ingot After the impurity removal and purification are completed, the heating power of the single crystal furnace is gradually reduced to 0kw through power control, the crucible rotation is turned off, and after the metal liquid is fully cooled and solidified, the furnace cover is opened and the germanium metal block that has been cast is taken out.
2. A method for recovering germanium from a high-grade germanium-containing material according to claim 1, characterized in that: In the step (4), after the crystal block grows to a diameter of 50-100 mm, the seed crystal is lifted to a position 50-200 mm above the liquid surface for cooling, the cooling time is 2-10 min, the crucible rotation speed is reduced to less than or equal to 2 r / min, and the seed crystal is lowered so that the bottom surface of the crystal block contacts the scum accumulated on the liquid surface, and the crystal block is lifted to a position 50-200 mm above the liquid surface, and the scum is attached to the crystal block; Repeat the above operation process 3-5 times to complete the purification.
3. A method for recovering germanium from a high-grade germanium-containing material according to claim 1, characterized in that: When melting the material in step (3), the power is increased 3-5 times evenly within 1 hour until the temperature rises to 1000-1100° C. to fully melt the germanium-containing material, and then the temperature is lowered to control the liquid surface temperature at 937-950° C.
4. A method for recovering germanium from a high-grade germanium-containing material according to claim 1, characterized in that: In the step (2), the vacuum degree in the single crystal furnace is below 200 mTorr, and the gas pressure in the furnace is 10-20 Torr.
5. A method for recovering germanium from a high-grade germanium-containing material according to claim 1, characterized in that: The water content of the germanium-containing material in step (1) is less than 0.01%.
6. A method for recovering germanium from a high-grade germanium-containing material according to claim 1, characterized in that: In the step (5), the power is gradually reduced to 0 kW in 2-3 times within 1 hour, the crucible rotation is turned off, and the temperature in the furnace is waited for 6-12 hours to drop below 50° C. before opening the furnace cover and taking out the germanium metal block after the casting is completed.
Citation Information
Patent Citations
Process for producing Czochralski silicon single crystal
CN102242397A
Germanium melt scum removal method
CN105401214A
Method for adhering dirty materials in growth process of germanium crystals
CN111809237A
Impurity removal method for slag inclusion and impurity-containing single crystal germanium waste
CN114622272A
Method for preparing compound crystal via melt migration under supergravity
WO2024027072A1
Cited By
Purification method of germanium and high-purity germanium
CN119614905A
Method for purifying germanium and high-purity germanium
CN119614905B