Preparation method of enhanced Mo2NiB2 alloy

By optimizing the preparation process of Mo2NiB2 alloy, including ball milling and sintering treatment, combined with the use of grinding aids and sintering aids, the problems of insufficient hardness and toughness of traditional alloys are solved, and its mechanical properties are significantly improved.

CN118910450AInactive Publication Date: 2024-11-08DONGGUAN JINGHENG MASCH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410976547.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-20
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In certain working conditions, the hardness and toughness of traditional Mo2NiB2 alloy cannot meet higher requirements.

Method used

Mo powder, Ni powder, B powder and SiCw powder are used as raw materials, and the ball mill mixing, cold isostatic molding and vacuum sintering processes are used to optimize the ball milling time, sintering temperature and insulation time, and add grinding aids and sintering aids to form and enhance the formation. Mo2NiB2 alloy.

Benefits of technology

It significantly improves the hardness and toughness of Mo2NiB2 alloy, making its mechanical properties more excellent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910450A_ABST
    Figure CN118910450A_ABST
Patent Text Reader

Abstract

The invention relates to the field of metal material preparation, in particular to a preparation method of an enhanced Mo2NiB2 alloy, which comprises the following steps: proportioning Mo powder, Ni powder, B powder and SiCw powder as raw materials according to the mass ratio of Mo powder to Ni powder to B powder to SiCw powder of (45-60): (25-40): (5-10): 4; the preparation method has the beneficial effects that the Mo powder, the Ni powder and the B powder serve as raw materials, the SiCw powder is added into the raw materials at the same time to serve as a reinforcing phase material, the ball milling time, the sintering temperature and the heat preservation time are optimized at the same time, the microstructure of the alloy is more uniform, the mechanical property is more excellent, and therefore the hardness and toughness of the Mo2NiB2 alloy can be remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal material preparation, and in particular to a method for preparing an enhanced Mo2NiB2 alloy. Background Art

[0002] Cermet is a non-homogeneous composite material composed of one or several ceramics of metal or alloy, the latter accounting for about 15% to 85% of the total volume. It takes into account the high toughness and plasticity of metal and the high temperature resistance, wear resistance and corrosion resistance of ceramics. It is a new type of material that combines the performance advantages of both metal and ceramics. Among them, Mo2NiB2-based cermet has high hardness, good mechanical properties and chemical stability, and has broad application prospects in the fields of tooling materials and high-temperature materials.

[0003] Mo2NiB2 metal ceramic material has excellent properties such as high melting point, high hardness, high wear resistance and high corrosion resistance, and is widely used in machinery, chemical industry, aerospace and other fields.

[0004] However, the hardness and toughness of traditional Mo2NiB2 alloy still cannot meet higher requirements under certain specific working conditions. Summary of the invention

[0005] In order to overcome the above-mentioned shortcomings, the present invention provides a technical solution that can solve the above-mentioned problems.

[0006] A method for preparing an enhanced Mo2NiB2 alloy comprises the following steps:

[0007] (1) Mo powder, Ni powder, B powder and SiCw powder are used as raw materials, and the ingredients are prepared according to the mass ratio of Mo powder: Ni powder: B powder: SiCw powder = (45-60): (25-40): (5-10): 4;

[0008] (2) placing the prepared raw materials into a ball mill for ball milling and mixing, the ball milling time is 20-30 hours, and the ball milling speed is 200-300 rpm;

[0009] (3) placing the ball-milled mixed powder into a mold and pressing it using a cold isostatic pressing process at a pressing pressure of 100-200 MPa for a holding time of 1-5 minutes;

[0010] (4) placing the pressed green body into a vacuum sintering furnace for sintering; the sintering temperature is 1200°C-1300°C, and the holding time is 30-60 minutes;

[0011] (5) After sintering, the sample is taken out for post-processing steps such as cooling, grinding, and polishing to obtain the final enhanced Mo2NiB2 alloy.

[0012] As a further solution of the present invention: in step 2, a grinding aid is added, the mass ratio of the grinding aid is 5% of the total mass of the raw materials, and the grinding aid is anhydrous ethanol.

[0013] As a further solution of the present invention: a sintering aid is added in step 4, the mass ratio of the sintering aid is 2% of the total mass of the raw materials, and the sintering aid is Ti powder.

[0014] As a further solution of the present invention: the purity of Mo powder, Ni powder, B powder and SiCw powder is greater than 99.9%.

[0015] Compared with the prior art, the beneficial effects of the present invention are: by using Mo powder, Ni powder and B powder as raw materials, and adding SiCw powder as a reinforcing phase material to the raw materials, the ball milling time, sintering temperature and holding time are optimized, so that the microstructure of the alloy is more uniform and the mechanical properties are more excellent, thereby significantly improving the hardness and toughness of the Mo2NiB2 alloy.

[0016] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions in this embodiment or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0018] Figure 1 It is a structural schematic diagram of the present invention. DETAILED DESCRIPTION

[0019] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] In the description of the present invention, it should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0021] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0022] In the embodiments of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0023] See also Figure 1 ,

[0024] 1) Mo powder, Ni powder, B powder and SiCw powder are used as raw materials, and the materials are prepared according to the mass ratio of Mo powder: Ni powder: B powder: SiCw powder = (45-60): (25-40): (5-10): 4, and the particle size of Mo powder, Ni powder and B powder is required to be ≤15μm;

[0025] 2) putting the prepared raw materials into a ball mill for ball milling and mixing, adding anhydrous ethanol in an amount of 5% by weight of the total raw materials, the ball milling time is 20-30 hours, the ball milling speed is 200-300 rpm, and a mixed powder is obtained;

[0026] 3) placing the ball-milled mixed powder into a mold, and pressing and molding it by cold isostatic pressing, with a pressing pressure of 100-200 MPa and a holding time of 1-5 minutes to obtain a green body;

[0027] 4) placing the pressed green body into a vacuum sintering furnace for sintering, adding 2% Ti powder by weight of the total raw material; the sintering temperature is 1200°C-1300°C, and the holding time is 30-60min;

[0028] 5) After sintering, the sample is taken out for post-processing steps such as cooling, grinding, and polishing to obtain the final enhanced Mo2NiB2 alloy.

[0029] The base phase is Mo2NiB2 and the reinforcement phase is SiCw.

[0030] The present invention is further described in detail below in conjunction with specific embodiments.

[0031] Embodiment 1:

[0032] 1) Mo powder, Ni powder, B powder, SiCw powder and TiC powder with a purity of not less than 99.9% are selected as raw materials, and the materials are prepared according to the mass ratio of Mo powder: Ni powder: B powder: SiCw powder = 50: 40: 6: 4, and the particle size of Mo powder, Ni powder and B powder is required to be ≤ 15 μm;

[0033] 2) putting the prepared raw materials into a ball mill for ball milling and mixing, adding anhydrous ethanol in an amount of 5% by weight of the total raw materials, the ball milling time is 24 hours, the ball milling speed is 220 rpm, and a mixed powder is obtained;

[0034] 3) placing the ball-milled mixed powder into a mold and pressing it by cold isostatic pressing at a pressure of 130 MPa for 3 minutes to obtain a green body;

[0035] 4) placing the pressed green body into a vacuum sintering furnace for sintering, adding Ti powder with a total weight ratio of 2% of the raw materials; the sintering temperature is 1240°C, and the holding time is 40 minutes;

[0036] 5) After sintering, the sample is taken out for post-processing steps such as cooling, grinding, and polishing to obtain the final enhanced Mo2NiB2 alloy.

[0037] The performance test of the reinforced Mo2NiB2 alloy prepared in Example 1 showed that the density was 97.4%, the three-point bending strength was 1670 MPa, the fracture toughness was 26.8 MPa·m1 / 2, and the hardness was 85.5 HRA.

[0038] Embodiment 2:

[0039] 1) Mo powder, Ni powder, B powder, SiCw powder and TiC powder with a purity of not less than 99.9% are selected as raw materials, and the materials are prepared according to the mass ratio of Mo powder: Ni powder: B powder: SiCw powder = 55: 34: 7: 4, and the particle size of Mo powder, Ni powder and B powder is required to be ≤ 15 μm;

[0040] 2) putting the prepared raw materials into a ball mill for ball milling and mixing, adding 5% anhydrous ethanol in a total mass ratio of the raw materials, the ball milling time is 26 hours, the ball milling speed is 250 rpm, and a mixed powder is obtained;

[0041] 3) placing the ball-milled mixed powder into a mold and pressing it by cold isostatic pressing at a pressure of 160 MPa for 4 minutes to obtain a green body;

[0042] 4) placing the pressed green body into a vacuum sintering furnace for sintering, adding 2% Ti powder in the total mass ratio of the raw materials; the sintering temperature is 1260°C, and the holding time is 50min;

[0043] 5) After sintering, the sample is taken out for post-processing steps such as cooling, grinding, and polishing to obtain the final enhanced Mo2NiB2 alloy.

[0044] The performance test of the reinforced Mo2NiB2 alloy prepared in Example 2 showed that the density was 97.9%, the three-point bending strength was 1710 MPa, the fracture toughness was 26.5 MPa·m1 / 2, and the hardness was 86.1 HRA.

[0045] Embodiment three:

[0046] 1) Mo powder, Ni powder, B powder, SiCw powder and TiC powder with a purity of not less than 99.9% are selected as raw materials, and the materials are prepared according to the mass ratio of Mo powder: Ni powder: B powder: SiCw powder = 58: 30: 8: 4, and the particle size of Mo powder, Ni powder and B powder is required to be ≤ 15 μm;

[0047] 2) putting the prepared raw materials into a ball mill for ball milling and mixing, adding anhydrous ethanol in an amount of 5% by weight of the total raw materials, the ball milling time is 28 hours, the ball milling speed is 280 rpm, and a mixed powder is obtained;

[0048] 3) placing the ball-milled mixed powder into a mold and pressing it by cold isostatic pressing at a pressure of 190 MPa for 5 minutes to obtain a green body;

[0049] 4) placing the pressed green body into a vacuum sintering furnace for sintering, adding 2% Ti powder in the total mass ratio of the raw materials; the sintering temperature is 1280°C, and the holding time is 55min;

[0050] 5) After sintering, the sample is taken out for post-processing steps such as cooling, grinding, and polishing to obtain the final enhanced Mo2NiB2 alloy.

[0051] The performance test of the reinforced Mo2NiB2 alloy prepared in Example 3 showed that the density was 98.4%, the three-point bending strength was 1750 MPa, the fracture toughness was 26.2 MPa·m1 / 2, and the hardness was 86.7 HRA.

[0052] Embodiment 4:

[0053] 1) Mo powder, Ni powder, B powder, SiCw powder and TiC powder with a purity of not less than 99.9% are selected as raw materials, and the materials are prepared according to the mass ratio of Mo powder: Ni powder: B powder: SiCw powder = 59: 48: 9: 4, and the particle size of Mo powder, Ni powder and B powder is required to be ≤ 15 μm;

[0054] 2) putting the prepared raw materials into a ball mill for ball milling and mixing, adding anhydrous ethanol in an amount of 5% by weight of the total raw materials, the ball milling time is 29 hours, the ball milling speed is 290 rpm, and a mixed powder is obtained;

[0055] 3) placing the ball-milled mixed powder into a mold and pressing it by cold isostatic pressing at a pressure of 190 MPa for 5 minutes to obtain a green body;

[0056] 4) placing the pressed green body into a vacuum sintering furnace for sintering, adding 2% Ti powder in the total mass ratio of the raw materials; the sintering temperature is 1280°C, and the holding time is 55min;

[0057] 5) After sintering, the sample is taken out for post-processing steps such as cooling, grinding, and polishing to obtain the final enhanced Mo2NiB2 alloy.

[0058] The performance test of the reinforced Mo2NiB2 alloy prepared in Example 4 showed that the density was 98.8%, the three-point bending strength was 1780 MPa, the fracture toughness was 26.0 MPa·m1 / 2, and the hardness was 87.1 HRA.

[0059] It should also be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the statement "including a ..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.

[0060] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing an enhanced Mo2NiB2 alloy, characterized in that: The following steps are involved: (1) Mo powder, Ni powder, B powder and SiCw powder are used as raw materials, and the ingredients are prepared according to the mass ratio of Mo powder: Ni powder: B powder: SiCw powder = (45-60): (25-40): (5-10): 4; (2) placing the prepared raw materials into a ball mill for ball milling and mixing, the ball milling time is 20-30 hours, and the ball milling speed is 200-300 rpm; (3) placing the ball-milled mixed powder into a mold and pressing it using a cold isostatic pressing process at a pressing pressure of 100-200 MPa for a holding time of 1-5 minutes; (4) placing the pressed green body into a vacuum sintering furnace for sintering; the sintering temperature is 1200°C-1300°C, and the holding time is 30-60 minutes; (5) After sintering, the sample is taken out for post-processing steps such as cooling, grinding, and polishing to obtain the final enhanced Mo2NiB2 alloy.

2. The method for preparing an enhanced Mo2NiB2 alloy according to claim 1, characterized in that: In step 2, anhydrous ethanol is added as a grinding aid, the mass ratio of the grinding aid is 5% of the total mass of the raw materials.

3. The method for preparing an enhanced Mo2NiB2 alloy according to claim 1, characterized in that: In step 4, a sintering aid is added, and the mass ratio of the sintering aid is 2% of the total mass of the raw materials. The sintering aid is Ti powder.

4. The method for preparing an enhanced Mo2NiB2 alloy according to claim 1, characterized in that: The purity of Mo powder, Ni powder, B powder and SiCw powder is greater than 99.9%.

Citation Information

Patent Citations

  • SiC crystal whisker reinforced and toughened Mo2FeB2 matrix metal ceramic and preparation method thereof

    CN101736211A

  • Carbide-reinforced Mo2NiB2 metal ceramic and preparation method thereof

    CN104911434A

  • Yttrium-modified Mo2NiB2-based metal ceramic and preparation method thereof

    CN111116208A

  • Chromium-doped modified Mo2NiB2-based metal ceramic and preparation method thereof

    CN111139390A

  • Preparation method of TiB2-reinforced Mo2NiB2-based composite material

    CN115780812A