Preparation method of high-toughness ultralight magnesium-lithium alloy wire suitable for electric arc additive manufacturing

The preparation of high-strength, tough, ultralight magnesium-lithium alloy wire material through multi-step process solves the problem that traditional methods are difficult to make high-quality magnesium-lithium alloy wire material, and realizes high-strength and good mechanical properties of magnesium-lithium alloy wire material, suitable for complex structures Manufacturing of parts.

CN118932163APending Publication Date: 2024-11-12NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411006462.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional methods are difficult to efficiently and quickly manufacture high-quality magnesium lithium alloy wire materials, resulting in insufficient mechanical properties in complex structural parts and cannot meet the requirements of complex structural parts.

Method used

Using multi-step processes of smelting, homogenization treatment, extrusion deformation, rotary forging deformation, drawing deformation and peeling treatment, the composition and processing parameters of magnesium-lithium alloy wire are controlled, and the composition and processing parameters of magnesium-lithium alloy wire are prepared to be slender in diameter, smooth in surface, and crystalline. High-strength, tough, ultra-light magnesium lithium alloy wire material with fine particles and uniform microstructure.

Benefits of technology

It has achieved high strength and good mechanical properties of magnesium lithium alloy wire, with a density below 1.6g/cm3, a tensile strength above 175MPa, and an elongation above 10%. It is suitable for arc additive manufacturing with lightweight, high performance and complexity of different wall thicknesses. Structural parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932163A_ABST
    Figure CN118932163A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-toughness ultralight magnesium-lithium alloy wire suitable for electric arc additive manufacturing, which comprises the following steps: step 1, smelting Mg, Li, Zn and Mg-Y intermediate alloys to obtain a cast ingot; 2, homogenizing the cast ingot to obtain a homogenized cast ingot; thirdly, the homogenized cast ingot is subjected to extrusion deformation and rotary swaging deformation, and a rotary swaging wire is obtained; fourthly, the rotary swaging wire is subjected to drawing deformation, and a drawn wire is obtained; and fifthly, the drawn wire is scalped, and the high-toughness ultra-light magnesium-lithium alloy wire is obtained. Through smelting, homogenization, extrusion, rotary swaging, drawing and scalping, the prepared high-toughness ultralight magnesium-lithium alloy wire is equal in diameter, long and thin, smooth in surface, good in formability which can reach hundreds of meters, fine in grain, uniform in microstructure and good in mechanical property, the density is lower than 1.6 g / cm < 2 >, the tensile strength is larger than 175 MPa, the ductility is larger than 10%, and the tensile strength is larger than 175 MPa. The method can be used for electric arc additive manufacturing of light high-performance complex structural parts with different wall thicknesses.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of metal material processing, and in particular relates to a method for preparing a high-strength and tough ultra-light magnesium-lithium alloy wire suitable for arc additive manufacturing. Background Art

[0002] Magnesium-lithium alloy is the lightest metal structural material currently used. It has outstanding advantages in reducing the weight of low-strength load-bearing structural parts and is an important material of choice for aerospace, weapons and equipment. With the iteration and update of products, complex structural parts of magnesium-lithium alloy have been more widely used, while traditional casting, plastic deformation and other methods are difficult to efficiently and quickly manufacture complex components such as magnesium alloy thin-walled shells and brackets. Therefore, how to shorten the processing cycle, save costs, and obtain high-quality magnesium-lithium alloy components is the main problem at present. Arc additive manufacturing technology can effectively overcome the problem of poor formability of magnesium-lithium alloy, and can realize the forming of complex structures. At the same time, the processing cycle is short and the material loss is small. These advantages are not available in traditional methods. However, high-quality magnesium-lithium alloy wire lacks mature processing and preparation technology, and the length, diameter, and strength and toughness of the wire cannot be effectively guaranteed.

[0003] In the past, magnesium-lithium alloy wires were mainly prepared by extrusion combined with drawing. The magnesium-lithium alloy wires obtained by this preparation process have poor uniformity of structure, limited grain refinement, poor strength and plasticity, and deformation cracks are prone to occur inside the wires, which seriously affects their mechanical properties, making it difficult for complex structural parts prepared by arc additive manufacturing at the back end to meet the use requirements. Therefore, in response to the above problems, it is urgently necessary to develop a high-strength and tough magnesium-lithium alloy wire for arc additive manufacturing and a preparation method thereof. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for preparing high-strength and tough ultra-light magnesium-lithium alloy wire suitable for arc additive manufacturing in view of the shortcomings of the above-mentioned prior art. The method is carried out through smelting, homogenization, extrusion deformation, rotary forging deformation, drawing deformation and peeling treatment to obtain high-strength and tough ultra-light magnesium-lithium alloy wire with equal diameter and slenderness, smooth surface and good formability, which can reach hundreds of meters, and at the same time, the grains are fine, the microstructure is uniform, the mechanical properties are good, and the density is less than 1.6g / cm 2 , tensile strength greater than 175MPa, elongation greater than 10%, can be used for arc additive manufacturing of lightweight, high-performance complex structural parts with different wall thicknesses.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a high-strength and tough ultra-light magnesium-lithium alloy wire suitable for arc additive manufacturing, characterized in that the method comprises the following steps:

[0006] Step 1, smelting of magnesium-lithium alloy: smelting Mg, Li, Zn and Mg-Y master alloy in a vacuum induction melting furnace, and grinding after cooling in the furnace to obtain an ingot;

[0007] Step 2: homogenization: homogenizing the ingot obtained in step 1 to obtain a homogenized ingot;

[0008] Step 3: extrusion and rotary forging deformation: the homogenized ingot obtained in step 2 is subjected to extrusion deformation, and then subjected to multiple passes of rotary forging deformation to obtain a rotary forging wire;

[0009] Step 4: Drawing and deformation: drawing and deforming the rotary forging wire obtained in step 3 to obtain a drawn wire;

[0010] Step 5: peeling: peel the drawn wire obtained in step 4 to obtain a high-strength and ultra-light magnesium-lithium alloy wire; the magnesium-lithium alloy wire is composed of the following components by mass fraction: Li 3% to 12%, Zn 5% to 7%, Y1% to 3%, and the remainder is Mg and unavoidable impurities, and the total mass of the unavoidable impurities is less than 0.2%; the density of the magnesium-lithium alloy wire is less than 1.6 g / cm 2 , tensile strength is greater than 175MPa and elongation is greater than 10%.

[0011] The present invention melts the raw materials, grinds off the oxide scale and impurities on the surface and then performs homogenization treatment, performs a large plastic extrusion deformation on the homogenized magnesium-lithium alloy ingot, and then performs multiple rotary forging deformations to obtain rotary forging wires that can be used for drawing processing, further draws and deforms the rotary forging wires to refine their diameters, and draws to obtain drawn wires, and finally winds the drawn wires on a pay-off assembly, selects a stripping die with a proper aperture for stripping treatment, and retracts the stripped wires through a drawing drum to obtain ultra-light magnesium-lithium alloy wires with a smooth surface, which can be used for arc additive manufacturing of complex structural parts with different wall thicknesses.

[0012] The present invention effectively realizes the coexistence of α-Mg and β-Li dual-phase structures in the magnesium-lithium alloy by controlling the Li element content in the magnesium-lithium alloy wire to be 3% to 12%. The dual-phase structure can effectively realize the coordinated improvement of the strength and plasticity of the alloy. The main purpose of the Zn element content of 5% to 7% and the Y element content of 1% to 3% is to realize the precipitation of the second phase in the alloy in nanometer size, which can maintain the coordination of the alloy strength and plasticity to a certain extent. If the addition amount is too high, a coarse eutectic structure is easily formed, which is not conducive to the matching of strength and plasticity.

[0013] In the present invention, the aperture of the stripping die during stripping is smaller than the diameter of the drawn wire by 0.01 mm.

[0014] The above-mentioned method for preparing a high-strength and tough ultra-light magnesium-lithium alloy wire suitable for arc additive manufacturing is characterized in that the smelting in step one is carried out under argon protection, the smelting power is 7kW to 10kW, and the time is 5min to 10min. The present invention uses a vacuum induction melting furnace to smelt and strictly control the impurity elements such as Fe, Ni, Cu, etc. in the smelted cast alloy, effectively overcoming the problem of reduced strength and toughness of the magnesium alloy wire caused by impurity elements; at the same time, the cast alloy obtained by vacuum smelting has a uniform structure, equiaxed grains, less grain boundary segregation, and effectively inhibits the influence of magnesium alloy grain boundaries and the second phase in the grain on the mechanical and corrosion properties of the magnesium alloy wire.

[0015] The above-mentioned method for preparing a high-strength and tough ultra-light magnesium-lithium alloy wire suitable for arc additive manufacturing is characterized in that the temperature of the homogenization treatment in step 2 is 250°C to 350°C, the time is 5h to 10h, and the homogenization treatment is followed by water cooling to room temperature. The present invention ensures that the grain boundary and intracrystalline precipitation phases are melted back to form a supersaturated magnesium-based solid solution through homogenization treatment, realizes the maximum degree of alloying elements melting back into the magnesium matrix, avoids the existence of coarse grain boundary precipitation phases, and is beneficial to improving the strength and plasticity of the magnesium alloy.

[0016] The above-mentioned method for preparing a high-strength and tough ultra-light magnesium-lithium alloy wire suitable for arc additive manufacturing is characterized in that the extrusion deformation process described in step three is: preheating the homogenized ingot to 250°C to 350°C and keeping it warm for 15min to 30min, then preheating the extrusion die to the same temperature as the homogenized ingot, and then extruding at an extrusion temperature of 250°C to 350°C, an extrusion speed of 1mm / s to 5mm / s, and an extrusion ratio of 16:1 for extrusion deformation, followed by cooling to room temperature, and finally recrystallization annealing at 200°C to 300°C for 1h to 2h. The present invention controls the parameters of extrusion deformation, performs an extrusion deformation with a large extrusion ratio and combines it with recrystallization annealing, reduces the diameter, and provides an extruded deformed bar with grain refinement and excellent mechanical properties for subsequent rotary forging deformation, effectively avoiding microcracks inside the material due to excessive stress during rotary forging.

[0017] The above-mentioned method for preparing a high-strength and tough ultra-light magnesium-lithium alloy wire suitable for arc additive manufacturing is characterized in that the rotary forging temperature of the multi-pass rotary forging deformation in step three is 300°C to 350°C, the holding time between rotary forging passes is 10min to 15min, the diameter reduction amount per pass is 0.5mm, and the number of rotary forging deformation passes is 8 to 10 times. The present invention controls the parameters of the multi-pass rotary forging deformation, and further reduces the diameter by using the rotary forging deformation with multiple passes of small deformation accumulation, which helps to accumulate dislocation density inside the alloy, gradually refine the grain size and the second phase, increase the deformation dislocation in the alloy, and combine the short-time recrystallization annealing heat treatment between each pass to eliminate residual stress, prevent wire breakage and cracks, induce dynamic recrystallization to refine grains, and homogenize the microstructure.

[0018] The above-mentioned method for preparing a high-strength and tough ultra-light magnesium-lithium alloy wire suitable for arc additive manufacturing is characterized in that the process of drawing deformation described in step 4 is: first, drawing at a drawing speed of 2mm / s~4mm / s, a reduction of 0.1mm~0.5mm between each pass, and preheating at 250℃~300℃ for 5min~7min between each pass to obtain a drawing blank with a diameter of less than 1.5mm, and then drawing at a drawing speed of 2mm / s~4mm / s, a reduction of 0.03mm~0.05mm between each pass, and preheating at 250℃~300℃ for 1min~2min between each pass. The graded drawing deformation used in the present invention is conducive to the preparation of alloy wires with long length and uniform structure.

[0019] Compared with the prior art, the present invention has the following advantages:

[0020] 1. The high-strength and ultra-light magnesium-lithium alloy wire prepared by the present invention through smelting, homogenization, extrusion deformation, rotary forging deformation, drawing deformation and peeling treatment has equal diameter and slenderness, smooth surface and good formability, which can reach hundreds of meters. At the same time, it has fine grains, uniform microstructure and good mechanical properties, and can be used for arc additive manufacturing of lightweight and high-performance complex structural parts with different wall thicknesses.

[0021] 2. The present invention realizes the coexistence of α-Mg and β-Li dual-phase structures in the magnesium-lithium alloy by controlling the content of each component in the magnesium-lithium alloy wire, effectively realizes the coordinated improvement of alloy strength and plasticity, realizes the precipitation of the second phase in the alloy in nanometer size, and can maintain the coordination of alloy strength and plasticity to a certain extent.

[0022] 3. The density of the magnesium-lithium alloy wire obtained by the present invention is lower than 1.6 g / cm 2 At the same time, the tensile strength is greater than 175MPa and the elongation is greater than 10%, which is more conducive to the additive manufacturing of lightweight magnesium-lithium alloy samples and has a wider range of uses for some non-load-bearing structural parts.

[0023] 4. The vacuum induction melting method of the present invention is used to prepare the ingot. By this method, the impurity elements such as Fe, Ni, Cu, etc. in the molten cast alloy can be strictly controlled, effectively overcoming the problem of decreased strength and toughness of the magnesium alloy wire caused by the impurity elements; at the same time, the cast alloy obtained by vacuum melting has a uniform structure, equiaxed grains, less grain boundary segregation, and effectively inhibits the influence of the magnesium alloy grain boundary and the second phase in the crystal on the mechanical and corrosion properties of the magnesium alloy wire. The preparation process is simple, the energy consumption is low, and the purity of the obtained magnesium alloy ingot is good.

[0024] 5. The present invention prepares ultra-light magnesium-lithium alloy wire by a method of multi-step continuous plastic processing deformation combined with annealing heat treatment between passes, wherein the extrusion deformation performs a large extrusion ratio extrusion deformation combined with recrystallization annealing, which provides a grain-refined, mechanically excellent extruded deformed bar for subsequent rotary forging deformation, effectively avoiding microcracks inside the material due to excessive stress during rotary forging, and using rotary forging deformation with multiple passes of small deformation accumulation to help accumulate dislocation density inside the alloy, gradually refine the grain size and the second phase, and increase the deformation dislocation in the alloy. Combined with short-time recrystallization annealing heat treatment between each pass, residual stress is eliminated, wire breakage and cracks are prevented, dynamic recrystallization is induced to refine grains, and microstructure is homogenized. The use of graded drawing deformation is conducive to the preparation of alloy wires with long length and uniform organization, thereby obtaining light magnesium-lithium alloy wires with excellent toughness. The room temperature tensile strength of the magnesium-lithium alloy wire can reach up to 212MPa, and the elongation can reach up to 10.2%, which is conducive to ensuring the mechanical properties of complex components manufactured by rear-end arc additive manufacturing.

[0025] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A longitudinal cross-sectional microstructure morphology of the high-strength, tough, ultra-light magnesium-lithium alloy wire prepared in Example 2 of the present invention.

[0027] Figure 2 Cross-sectional microstructure morphology of the high-strength, tough, ultra-light magnesium-lithium alloy wire prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0028] Example 1

[0029] This embodiment includes the following steps:

[0030] Step 1, magnesium-lithium alloy smelting: Mg, Li, Zn and Mg-30wt.%Y master alloy are placed in a crucible of a vacuum induction melting furnace, heated and melted at a melting power of 8kW under argon protection, and kept warm for 7 minutes before cooling with the furnace, and the surface oxide scale and impurities are polished to obtain an ingot;

[0031] Step 2: homogenization treatment: the ingot obtained in step 1 is placed in a muffle furnace, and then homogenized at a temperature of 350° C. for 5 hours, and then water-cooled to room temperature at a temperature of 30° C. to 80° C. to obtain a homogenized ingot;

[0032] Step 3, extrusion, rotary forging deformation: the homogenized ingot obtained in step 2 is cut into cylindrical blocks of 40 mm × 50 mm (diameter × length) and polished and peeled, and then the polished and peeled cylindrical blocks are preheated to 320 ° C and kept warm for 30 minutes, the extrusion die is preheated to the same temperature as the homogenized ingot, and then extrusion deformation is performed at an extrusion temperature of 320 ° C, an extrusion speed of 3 mm / s, and an extrusion ratio of 16:1, and then cooled to room temperature, and finally recrystallized annealed at 300 ° C for 1 hour to obtain an extruded billet with a diameter of 7 mm, and the extruded billet is subjected to 8 rotary forging deformations at a rotary forging temperature of 300 ° C, a holding time of 15 minutes between rotary forging passes, and a diameter reduction of 0.5 mm per pass to obtain a rotary forging wire with a diameter of 3 mm;

[0033] Step 4, drawing deformation: the rotary forging wire obtained in step 3 is first drawn at a drawing speed of 2 mm / s, a reduction of 0.1 mm between each pass, and preheated at 300°C for 6 minutes between each pass to obtain an intermediate wire with a diameter of 1.5 mm, and then drawn at a drawing speed of 2 mm / s, a reduction of 0.05 mm between each pass, and preheated at 300°C for 1 minute between each pass to obtain a drawn wire;

[0034] Step 5: Stripping: The drawn wire obtained in step 4 is wound on the pay-off assembly, stripped through a stripping die, and then retracted through a wire drawing drum to obtain a high-strength, tough, and ultra-light magnesium-lithium alloy wire with a diameter of 0.9 mm.

[0035] After testing, the magnesium-lithium alloy wire prepared in this embodiment is composed of the following components by mass fraction: Li 5.02%, Zn 5.79%, Y 1.61%, and the remainder is Mg and inevitable impurities with a total mass fraction of less than 0.2%.

[0036] Example 2

[0037] This embodiment includes the following steps:

[0038] Step 1, magnesium-lithium alloy smelting: Mg, Li, Zn and Mg-30wt.%Y master alloy are placed in a crucible of a vacuum induction melting furnace, heated and melted at a melting power of 7kW under argon protection, and kept warm for 10 minutes before cooling with the furnace, and the surface oxide scale and impurities are polished to obtain an ingot;

[0039] Step 2: homogenization treatment: the ingot obtained in step 1 is placed in a muffle furnace, and then homogenized at a temperature of 320° C. for 7 hours, and then water-cooled to room temperature at a temperature of 30° C. to 80° C. to obtain a homogenized ingot;

[0040] Step 3, extrusion, rotary forging deformation: the homogenized ingot obtained in step 2 is cut into cylindrical blocks of 40 mm × 50 mm (diameter × length) and polished and peeled, and then the polished and peeled cylindrical blocks are preheated to 310 ° C and kept warm for 30 minutes, the extrusion die is preheated to the same temperature as the homogenized ingot, and then extrusion deformation is performed at an extrusion temperature of 310 ° C, an extrusion speed of 3 mm / s, and an extrusion ratio of 16:1, and then cooled to room temperature, and finally recrystallized annealed at 300 ° C for 1 hour to obtain an extruded billet with a diameter of 7 mm, and the extruded billet is subjected to 8 rotary forging deformation at a rotary forging temperature of 350 ° C, a holding time of 10 minutes between rotary forging passes, and a diameter reduction of 0.5 mm per pass to obtain a rotary forging wire with a diameter of 3 mm;

[0041] Step 4, drawing deformation: the rotary forging wire obtained in step 3 is first drawn for 5 times at a drawing speed of 3 mm / s and a reduction amount of 0.3 mm between each pass, and each pass needs to be preheated at 300°C for 5 minutes to obtain an intermediate wire with a diameter of 1.5 mm, and then drawn for 20 times at a drawing speed of 3 mm / s and a reduction amount of 0.03 mm between each pass, and each pass needs to be preheated at 300°C for 1 minute to obtain a drawn wire;

[0042] Step 5: Stripping: The drawn wire obtained in step 4 is wound on the pay-off assembly, stripped through a stripping die, and then retracted through a wire drawing drum to obtain a magnesium-lithium alloy wire with a diameter of 0.9 mm.

[0043] After testing, the magnesium-lithium alloy wire prepared in this embodiment is composed of the following components by mass fraction: Li 8.49%, Zn 5.95%, Y 1.51%, and the remainder is Mg and inevitable impurities with a total mass fraction of less than 0.2%.

[0044] Figure 1 The longitudinal section microstructure morphology of the high-strength and ultra-light magnesium-lithium alloy wire prepared in this embodiment is as follows: Figure 1 It can be seen that the α-Mg phase is distributed in an elongated state in the pulling direction, with a relatively small aspect ratio and good microstructure uniformity.

[0045] Figure 2 The cross-sectional microstructure of the high-strength and ultra-light magnesium-lithium alloy wire prepared in this embodiment is shown in FIG. Figure 2 It can be seen that the dual-phase structure is evenly distributed, and the cross-section of the α-Mg phase is approximately circular, which can provide good strength and plasticity contribution.

[0046] Example 3

[0047] This embodiment includes the following steps:

[0048] Step 1, magnesium-lithium alloy smelting: Mg, Li, Zn and Mg-30wt.%Y master alloy are placed in a crucible of a vacuum induction melting furnace, heated and melted at a melting power of 10kW under argon protection, and then cooled with the furnace after keeping warm for 5 minutes, and the surface oxide scale and impurities are polished to obtain an ingot;

[0049] Step 2: homogenization treatment: the ingot obtained in step 1 is placed in a muffle furnace, and then homogenized at a temperature of 250° C. for 10 hours, and then water-cooled to room temperature at a temperature of 30° C. to 80° C. to obtain a homogenized ingot;

[0050] Step 3, extrusion, rotary forging deformation: the homogenized ingot obtained in step 2 is cut into cylindrical blocks of 40 mm × 50 mm (diameter × length) and polished and peeled, and then the polished and peeled cylindrical blocks are preheated to 320 ° C and kept warm for 30 minutes, the extrusion die is preheated to the same temperature as the homogenized ingot, and then extrusion deformation is performed at an extrusion temperature of 320 ° C, an extrusion speed of 3 mm / s, and an extrusion ratio of 16:1, and then cooled to room temperature, and finally recrystallized annealed at 300 ° C for 1 hour to obtain an extruded billet with a diameter of 7 mm, and the extruded billet is subjected to 8 rotary forging deformation at a rotary forging temperature of 350 ° C, a holding time of 10 minutes between rotary forging passes, and a diameter reduction of 0.5 mm per pass to obtain a rotary forging wire with a diameter of 3 mm;

[0051] Step 4, drawing deformation: the rotary forging wire obtained in step 3 is first drawn for 3 times at a drawing speed of 4 mm / s and a reduction of 0.5 mm between each pass, and each pass needs to be preheated at 300°C for 7 minutes, and then drawn for 10 times at a drawing speed of 4 mm / s and a reduction of 0.04 mm between each pass, and each pass needs to be preheated at 300°C for 1 minute to obtain a drawn wire;

[0052] Step 5: Stripping: The drawn wire obtained in step 4 is wound on the pay-off assembly, stripped through a stripping die, and then retracted through a wire drawing drum to obtain a high-strength, tough, and ultra-light magnesium-lithium alloy wire with a diameter of 1.1 mm.

[0053] After testing, the magnesium-lithium alloy wire prepared in this embodiment is composed of the following components by mass fraction: Li 10.51%, Zn 6.08%, Y 1.58%, and the remainder is Mg and inevitable impurities with a total mass fraction of less than 0.2%.

[0054] Example 4

[0055] This embodiment includes the following steps:

[0056] Step 1, magnesium-lithium alloy smelting: Mg, Li, Zn and Mg-30wt.%Y master alloy are placed in a crucible of a vacuum induction melting furnace, heated and melted at a melting power of 10kW under argon protection, and then cooled with the furnace after keeping warm for 5 minutes, and the surface oxide scale and impurities are polished to obtain an ingot;

[0057] Step 2: homogenization treatment: the ingot obtained in step 1 is placed in a muffle furnace, and then homogenized at a temperature of 350° C. for 8 hours, and then water-cooled to room temperature at a temperature of 30° C. to 80° C. to obtain a homogenized ingot;

[0058] Step 3, extrusion, rotary forging deformation: the homogenized ingot obtained in step 2 is cut into cylindrical blocks of 40 mm × 50 mm (diameter × length) and polished and peeled, and then the polished and peeled cylindrical blocks are preheated to 350 ° C and kept warm for 15 minutes, the extrusion die is preheated to the same temperature as the homogenized ingot, and then extrusion deformation is performed at an extrusion temperature of 350 ° C, an extrusion speed of 5 mm / s, and an extrusion ratio of 16:1, and then cooled to room temperature, and finally recrystallized annealed at 200 ° C for 2 hours to obtain an extruded billet with a diameter of 7 mm, and the extruded billet is subjected to 10 rotary forging deformations at a rotary forging temperature of 340 ° C, a holding time of 12 minutes between rotary forging passes, and a diameter reduction of 0.5 mm per pass to obtain a rotary forging wire with a diameter of 2 mm;

[0059] Step 4, drawing deformation: the rotary forging wire obtained in step 3 is first drawn for 5 times at a drawing speed of 4 mm / s and a reduction amount of 0.1 mm between each pass, and each pass needs to be preheated at 250°C for 6 minutes, and then drawn for 10 times at a drawing speed of 4 mm / s and a reduction amount of 0.05 mm between each pass, and each pass needs to be preheated at 270°C for 2 minutes to obtain a drawn wire;

[0060] Step 5: Stripping: The drawn wire obtained in step 4 is wound on the pay-off assembly, stripped through a stripping die, and then retracted through a wire drawing drum to obtain a high-strength, tough, and ultra-light magnesium-lithium alloy wire with a diameter of 1 mm.

[0061] After testing, the magnesium-lithium alloy wire prepared in this embodiment is composed of the following components in mass fraction: Li 3.12%, Zn 6.97%, Y 1.12%, and the remainder is Mg and inevitable impurities with a total mass fraction of less than 0.2%.

[0062] Example 5

[0063] This embodiment includes the following steps:

[0064] Step 1, magnesium-lithium alloy smelting: Mg, Li, Zn and Mg-30wt.%Y master alloy are placed in a crucible of a vacuum induction melting furnace, heated and melted at a melting power of 10kW under argon protection, and then cooled with the furnace after keeping warm for 5 minutes, and the surface oxide scale and impurities are polished to obtain an ingot;

[0065] Step 2: homogenization treatment: the ingot obtained in step 1 is placed in a muffle furnace, and then homogenized at a temperature of 350° C. for 10 hours, and then water-cooled to room temperature at a temperature of 30° C. to 80° C. to obtain a homogenized ingot;

[0066] Step 3, extrusion, rotary forging deformation: the homogenized ingot obtained in step 2 is cut into cylindrical blocks of 40 mm × 50 mm (diameter × length) and polished and peeled, and then the polished and peeled cylindrical blocks are preheated to 250 ° C and kept warm for 20 minutes, the extrusion die is preheated to the same temperature as the homogenized ingot, and then extrusion deformation is performed at an extrusion temperature of 250 ° C, an extrusion speed of 1 mm / s, and an extrusion ratio of 16:1, and then cooled to room temperature, and finally recrystallized annealed at 250 ° C for 1.5 hours to obtain an extruded billet with a diameter of 7 mm, and the extruded billet is subjected to 9 rotary forging deformation at a rotary forging temperature of 320 ° C, a holding time of 14 minutes between rotary forging passes, and a diameter reduction of 0.5 mm per pass to obtain a rotary forging wire with a diameter of 2 mm;

[0067] Step 4, drawing deformation: the rotary forging wire obtained in step 3 is first drawn at a drawing speed of 3 mm / s, a reduction of 0.1 mm between each pass, and preheated at 270°C for 6 min between each pass, and then drawn at a drawing speed of 3 mm / s, a reduction of 0.05 mm between each pass, and preheated at 250°C for 1.5 min between each pass to obtain a drawn wire;

[0068] Step 5: Stripping: The drawn wire obtained in step 4 is wound on the pay-off assembly, stripped through a stripping die, and then retracted through a wire drawing drum to obtain a high-strength, tough, and ultra-light magnesium-lithium alloy wire with a diameter of 0.8 mm.

[0069] After testing, the magnesium-lithium alloy wire prepared in this embodiment is composed of the following components in mass fraction: Li 11.87%, Zn 5.11%, Y 2.92%, and the remainder is Mg and inevitable impurities with a total mass fraction of less than 0.2%.

[0070] The high-strength and tough ultra-light magnesium-lithium alloy wires prepared in Examples 1 to 5 were tested for tensile strength, yield strength and elongation. The results are shown in Table 1.

[0071] Table 1

[0072] Example Tensile strength(MPa) Yield strength (MPa) Elongation(%) Example 1 212 157 10.2 Example 2 194 141 11.5 Example 3 175 132 20.6 Example 4 202 143 14.2 Example 5 199 161 17.2 Pure magnesium wire 181 123 7.1

[0073] It can be seen from Table 1 that, compared with pure magnesium alloy wires, the high-strength and tough ultra-light magnesium-lithium alloy wires prepared in Examples 1 to 5 of the present invention have good performance in strength and elongation.

[0074] After testing, the high-strength and tough ultra-light magnesium-lithium alloy wires prepared in Examples 1 to 5 of the present invention not only have lower density than pure magnesium wires, but also have finer micro-scale grain sizes, and the wire diameter can reach less than 1 mm, with a smooth surface and good formability.

[0075] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a high-strength and ultra-light magnesium-lithium alloy wire suitable for arc additive manufacturing, characterized in that: The method comprises the following steps: Step 1, smelting of magnesium-lithium alloy: smelting Mg, Li, Zn and Mg-Y master alloy in a vacuum induction melting furnace, and grinding after cooling in the furnace to obtain an ingot; Step 2: homogenization: homogenizing the ingot obtained in step 1 to obtain a homogenized ingot; Step 3: extrusion and rotary forging deformation: the homogenized ingot obtained in step 2 is subjected to extrusion deformation, and then subjected to multiple passes of rotary forging deformation to obtain a rotary forging wire; Step 4: Drawing and deformation: drawing and deforming the rotary forging wire obtained in step 3 to obtain a drawn wire; Step 5: peeling: peel the drawn wire obtained in step 4 to obtain a high-strength and ultra-light magnesium-lithium alloy wire; the magnesium-lithium alloy wire is composed of the following components by mass fraction: Li 3% to 12%, Zn 5% to 7%, Y 1% to 3%, and the remainder is Mg and unavoidable impurities, and the total mass of the unavoidable impurities is less than 0.2%; the density of the magnesium-lithium alloy wire is less than 1.6 g / cm 2 , tensile strength is greater than 175MPa and elongation is greater than 10%.

2. The method for preparing a high-strength and ultra-light magnesium-lithium alloy wire suitable for arc additive manufacturing according to claim 1, characterized in that: The smelting in step 1 is carried out under argon protection, the smelting power is 7kW to 10kW, and the time is 5min to 10min.

3. The method for preparing a high-strength and ultra-light magnesium-lithium alloy wire suitable for arc additive manufacturing according to claim 1, characterized in that: The temperature of the homogenization treatment in step 2 is 250° C. to 350° C., and the time is 5 h to 10 h. After the homogenization treatment, the mixture is water-cooled to room temperature.

4. The method for preparing a high-strength and ultra-light magnesium-lithium alloy wire suitable for arc additive manufacturing according to claim 1, characterized in that: The extrusion deformation process described in step three is: preheating the homogenized ingot to 250°C to 350°C and keeping it warm for 15min to 30min, then preheating the extrusion die to the same temperature as the homogenized ingot, and then extruding at an extrusion temperature of 250°C to 350°C, an extrusion speed of 1mm / s to 5mm / s, and an extrusion ratio of 16:1, followed by cooling to room temperature, and finally recrystallization annealing at 200°C to 300°C for 1h to 2h.

5. The method for preparing a high-strength and ultra-light magnesium-lithium alloy wire suitable for arc additive manufacturing according to claim 1, characterized in that: The rotary forging temperature of the multi-pass rotary forging deformation in step 3 is 300° C. to 350° C., the holding time between rotary forging passes is 10 min to 15 min, the diameter reduction amount of each pass is 0.5 mm, and the number of rotary forging deformation passes is 8 to 10 times.

6. The method for preparing a high-strength and ultra-light magnesium-lithium alloy wire suitable for arc additive manufacturing according to claim 1, characterized in that: The drawing deformation process described in step 4 is: first, drawing is performed for 3 to 15 times at a drawing speed of 2 mm / s to 4 mm / s, and the reduction between each pass is 0.1 mm to 0.5 mm, and each pass needs to be preheated at 250°C to 300°C for 5 min to 7 min to obtain a drawn billet with a diameter less than 1.5 mm, and then drawing is performed for 4 to 20 times at a drawing speed of 2 mm / s to 4 mm / s, and the reduction between each pass is 0.03 mm to 0.05 mm, and each pass needs to be preheated at 250°C to 300°C for 1 min to 2 min.