Nickel-zinc battery positive electrode and preparation method and application thereof
By using bismuth oxide and spherical nickel hydroxide and cobalt coating in the positive electrode coating of nickel zinc batteries, the electrolyte corrosion problem is solved, the corrosion resistance and conductivity of nickel zinc batteries are improved, and the cycle stability and capacity are significantly improved.
Patent Information
- Application Number
- CN202411326179.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-29
AI Technical Summary
During the cycling operation of nickel-zinc batteries, the positive electrode and/or negative electrode are easily eroded by electrolyte, resulting in problems such as flatulence and dendrites, affecting their cycling and electrochemical properties.
Use bismuth oxide as the additive for the positive electrode coating to replace zinc powder, and add part of bismuth oxide to the original formula to increase the slurry density and load, reduce gas extraction phenomenon, combine spherical nickel hydroxide and cobalt coating to improve conductivity and corrosion resistance.
It improves the corrosion resistance and conductivity of the positive electrode of nickel-zinc battery, improves cycling stability and capacity, has a flat surface, and enhances electrochemical performance.
Smart Images

Figure CN119050286A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new energy technology, and in particular to a nickel-zinc battery positive electrode and a preparation method and application thereof. Background Art
[0002] Nickel-zinc battery is a new energy battery, which consists of a positive electrode, a negative electrode, a separator arranged between the positive electrode and the negative electrode, and an electrolyte. Usually, the active materials of the positive electrode include nickel and nickel hydroxide, the active materials of the negative electrode include zinc and zinc oxide, and the electrolyte is an alkaline aqueous solution. Nickel-zinc batteries have many advantages such as high-rate operation, high specific energy, low cost and low environmental cost. However, during the cycle operation of nickel-zinc batteries, the positive electrode and / or the negative electrode are easily corroded by the electrolyte, which in turn causes problems such as flatulence and dendrite growth, which leads to the need to improve its cycle performance and related electrochemical performance.
[0003] In order to solve the above technical problems, the relevant technologies have made many optimizations to the coating ingredients of the positive and negative electrodes, for example, mixing anti-corrosion materials into the negative electrode coating, or coating / mixing the positive electrode active materials with transition metal oxides or precious metal oxides.
[0004] However, for the modification of the positive electrode, if precious metal oxides are used as raw materials, the cost will increase to a certain extent, and if transition metal oxides are used as raw materials, the performance improvement will not be obvious. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a nickel-zinc battery positive electrode, which can effectively improve the corrosion resistance and conductivity of the nickel-zinc battery positive electrode, thereby improving its cycle stability and capacity.
[0006] The invention also provides a method for preparing the positive electrode of the nickel-zinc battery.
[0007] The invention also provides application of the positive electrode of the nickel-zinc battery.
[0008] According to an embodiment of the first aspect of the present invention, there is provided a nickel-zinc battery positive electrode, the nickel-zinc battery positive electrode comprising a positive electrode current collector and a positive electrode coating covering a surface of the positive electrode current collector;
[0009] The raw materials for preparing the positive electrode coating include, by weight:
[0010] 52-92 parts of positive electrode active material;
[0011] Positive electrode additive 0.51 to 20.1 parts;
[0012] 0.6 to 4.8 parts of positive electrode binder;
[0013] The positive electrode additive includes bismuth oxide.
[0014] The nickel-zinc battery positive electrode according to the embodiment of the present invention has at least the following beneficial effects:
[0015] In traditional technology, zinc powder is usually added to the positive electrode coating as an auxiliary additive to reduce the expansion of the positive electrode active material (inhibit the formation of γ-NiOOH) and improve the initial electronic conductivity of the positive electrode coating. However, the solvent used for homogenization in the preparation of the positive electrode of the nickel-zinc battery is water, and zinc powder has gas evolution in water. Therefore, during the homogenization process, the zinc powder will react with water or other positive electrode additives to produce gas, and the surface of the produced nickel-zinc battery positive electrode sheet has obvious large shrinkage holes.
[0016] The present invention replaces zinc powder with bismuth oxide, or adds part of bismuth oxide on the basis of the original basic formula. The bismuth oxide will not react with other positive electrode additives, the gas evolution phenomenon in the slurry is much less, the slurry density is also improved, the load capacity of the positive electrode of the nickel-zinc battery is increased, the shrinkage holes on the surface are also small, and the surface is flat and smooth, which is more conducive to the area utilization efficiency of the surface of the positive electrode sheet of the nickel-zinc battery.
[0017] Furthermore, bismuth oxide increases from trivalent to pentavalent during the charging process, and in a specific environment may form compounds with the positive electrode active material, or enhance conductivity, ultimately improving the overall electrochemical performance of the resulting nickel-zinc battery.
[0018] On the whole, the present invention improves the capacity and cycle stability of the obtained nickel-zinc battery positive electrode to a certain extent by adjusting the raw materials for preparing the nickel-zinc battery positive electrode and the amount of the raw materials used in preparing the nickel-zinc battery positive electrode.
[0019] According to some embodiments of the present invention, the positive electrode active material comprises spherical nickel hydroxide.
[0020] The spherical nickel hydroxide is doped with zinc and coated with cobalt, wherein the weight percentage of zinc doping is 2-3%, and the weight percentage of cobalt coating is 4-5%.
[0021] According to some embodiments of the present invention, the positive electrode additive further comprises nickel powder. Thus, the electronic conductivity of the positive electrode of the nickel-zinc battery can be improved, its polarization can be reduced, and its initial charge and discharge capacity in the formation stage can be increased.
[0022] The particle size of the nickel powder is 1-5 μm, for example, about 2 μm or about 3 μm. The nickel powder includes carbonyl nickel powder.
[0023] According to some embodiments of the present invention, the mass ratio of the nickel powder to the positive electrode active material is 1-7:51-85.
[0024] According to some embodiments of the present invention, the mass ratio of the nickel powder to the positive electrode active material is 1:10 to 20. For example, it may be about 1:14, 1:15, 1:16, 1:17 or about 1:18.
[0025] According to some embodiments of the present invention, the positive electrode additive further comprises yttrium oxide. According to some embodiments of the present invention, the mass ratio of bismuth oxide to yttrium oxide is 0.5-20:0.01-0.1.
[0026] According to some embodiments of the present invention, the mass ratio of bismuth oxide to yttrium oxide is 25 to 200:1, for example, about 30:1, 50:1, 70:1, 80:1, 100:1, 120:1, 130:1 or about 150:1.
[0027] According to some embodiments of the present invention, the bismuth oxide has a spherical structure.
[0028] According to some embodiments of the present invention, the particle size of the bismuth oxide is between 0.1 and 1 μm.
[0029] According to some embodiments of the present invention, the positive electrode binder includes PTFE.
[0030] According to some embodiments of the present invention, the raw materials for preparing the positive electrode coating further include a thickener.
[0031] According to some embodiments of the present invention, the thickener comprises CMC.
[0032] According to some embodiments of the present invention, the mass ratio of the thickener to the binder is 0.5-5:0.6-4.8.
[0033] According to some embodiments of the present invention, the mass ratio of the thickener to the binder is 1:5 to 9. For example, it may be about 1:6 or about 1:8.
[0034] According to some embodiments of the present invention, the mass ratio of the binder to the positive electrode active material is 1:15 to 18, for example, about 1:16 or about 1:17.
[0035] According to some embodiments of the present invention, the raw materials for preparing the positive electrode coating include, by weight:
[0036]
[0037] According to some embodiments of the present invention, the raw material for preparing the positive electrode current collector includes foamed nickel.
[0038] According to some embodiments of the present invention, the thickness of the positive electrode of the nickel-zinc battery is 0.6-0.7 mm, for example, about 0.65 mm, 0.66 mm, 0.67 mm or about 0.68 mm.
[0039] According to an embodiment of the second aspect of the present invention, a method for preparing a positive electrode of a nickel-zinc battery is provided, and the preparation method comprises the following steps:
[0040] S1. Providing a slurry comprising raw materials for preparing the positive electrode of the nickel-zinc battery;
[0041] S2. The slurry is coated on the surface of the positive electrode current collector precursor, and then rolled after drying.
[0042] Since the preparation method adopts all the technical solutions of the nickel-zinc battery positive electrode of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment.
[0043] Furthermore, the preparation method is simple, easy to implement, and convenient for large-scale industrial promotion.
[0044] According to some embodiments of the present invention, in step S1, the method for preparing the slurry includes preparing the positive electrode binder into a positive electrode binder slurry, and then mixing it with other prepared raw materials and water.
[0045] According to some embodiments of the present invention, the solid content of the positive electrode binder slurry is 55-65%, for example, about 60%.
[0046] According to some embodiments of the present invention, the density of the slurry is 2 to 2.5 g / cm 3 For example, it can be about 2.1 g / cm 3 , 2.2g / cm 3 or about 2.3g / cm 3 .
[0047] According to some embodiments of the present invention, in step S1, the components of the slurry include, by mass percentage:
[0048]
[0049]
[0050] According to some embodiments of the present invention, in step S1, the components of the slurry include, by mass percentage:
[0051]
[0052] According to some embodiments of the present invention, in the positive electrode binder slurry, the solid content of the positive electrode binder is 55-65%, for example, specifically about 60%.
[0053] According to some embodiments of the present invention, the positive electrode binder slurry is an aqueous slurry.
[0054] According to some embodiments of the present invention, in step S2, the thickness of the positive electrode current collector precursor is 0.9-1.6 mm, for example, about 1.0 mm or about 1.5 mm.
[0055] According to some embodiments of the present invention, in step S2, the step further includes pre-pressing the positive electrode current collector precursor before coating; obtaining a positive electrode current collector semi-finished product for subsequent coating; and obtaining the positive electrode current collector after coating and rolling. The thickness of the positive electrode current collector semi-finished product is 0.9 to 1.0 mm. For example, it can be about 0.95 mm.
[0056] According to some embodiments of the present invention, in step S2, the positive electrode current collector precursor is nickel foam.
[0057] According to some embodiments of the present invention, the pore density of the nickel foam is 100-120 PPI, for example, about 110 PPI.
[0058] According to some embodiments of the present invention, the porosity of the nickel foam is 95-97%, for example, about 96 or about 96.5%.
[0059] According to some embodiments of the present invention, in step S2, the thickness of the wet coating obtained by coating (also referred to as slurry drawing thickness) is 1 to 1.05 mm, for example, about 1.03 mm or about 1.04 mm.
[0060] According to an embodiment of the third aspect of the present invention, there is provided a nickel-zinc battery, the nickel-zinc battery comprising a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte that infiltrates the positive electrode, the negative electrode and the separator;
[0061] The positive electrode is the positive electrode of the nickel-zinc battery.
[0062] Since the nickel-zinc battery adopts all the technical solutions of the nickel-zinc battery positive electrode of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment, that is, the energy density and cycle stability of the nickel-zinc battery are improved to a certain extent.
[0063] According to some embodiments of the present invention, the negative electrode includes a negative electrode current collector and a negative electrode coating disposed on a surface of the negative electrode current collector.
[0064] According to some embodiments of the present invention, the raw materials for preparing the negative electrode coating include negative electrode active materials, inorganic oxide additives, organic additives, surfactants and negative electrode binders.
[0065] According to some embodiments of the present invention, the raw materials for preparing the negative electrode coating include, by weight:
[0066] 60-90 parts of negative electrode active material;
[0067] 3.5-15 parts of inorganic oxide additive;
[0068] Organic additives 0.01-0.1 parts;
[0069] Surfactant 0.01-0.1 part;
[0070] Negative electrode binder 0.75 to 8 parts.
[0071] According to some embodiments of the present invention, the raw materials for preparing the negative electrode coating include, by weight:
[0072] 70-75 parts of negative electrode active material;
[0073] 3.5-4 parts of inorganic oxide additive;
[0074] Organic additives 0.01-0.1 parts;
[0075] Surfactant 0.01-0.1 part;
[0076] 2 to 3 parts of negative electrode binder.
[0077] According to some embodiments of the present invention, the negative electrode active material includes zinc and zinc oxide. The mesh size of the zinc is between 200 and 1000 meshes. The D50 particle size of the zinc oxide is between 0.5 and 1 μm, for example, about 0.7 μm or about 0.8 μm.
[0078] According to some embodiments of the present invention, the inorganic oxide additive includes bismuth oxide and indium hydroxide, wherein the D50 particle size of the bismuth oxide is 1-2 μm, for example, specifically about 1.1 μm; and the particle size of the indium hydroxide is in the range of 20-70 nm.
[0079] According to some embodiments of the present invention, the organic additive includes PAAK.
[0080] According to some embodiments of the invention, the surfactant comprises SDBS.
[0081] According to some embodiments of the present invention, the negative electrode binder includes at least one of PTFE and PVA.
[0082] According to some embodiments of the present invention, the negative electrode current collector is a punched tin-plated copper strip.
[0083] According to some embodiments of the present invention, the thickness of the punched tinned copper strip is 0.04-0.06 mm of the base material, for example, it may be about 0.05 mm.
[0084] According to some embodiments of the present invention, the size of the punched hole on the negative electrode current collector is 1×1 mm. The closest distance between two adjacent through holes is 0.8-1.2 mm; for example, it can be about 1 mm, the rough thickness of the punched hole is 1.05-1.15 mm; for example, it can be about 1.1 mm, and the pre-pressed thickness is 0.7-0.9 mm; for example, it can be about 0.8 mm.
[0085] According to some embodiments of the present invention, the preparation process of the negative electrode comprises the following steps:
[0086] D1. preparing the raw materials for preparing the negative electrode coating into a negative electrode slurry;
[0087] D2. coating the negative electrode slurry on the surface of the negative electrode current collector and then drying.
[0088] According to some embodiments of the present invention, in step D1, the preparation method of the negative electrode slurry includes first preparing the surfactant, the negative electrode binder, and the organic additive into corresponding slurries respectively, and then mixing them with other preparation raw materials and water. This can improve the uniformity of the texture of the negative electrode slurry and reduce the time required for preparing the negative electrode slurry.
[0089] According to some embodiments of the present invention, when the negative electrode binder is selected from PTFE, the solid content of the negative electrode binder slurry is 55-65%, for example, about 60%.
[0090] When the negative electrode binder is selected from PVA, the solid content of the negative electrode binder slurry is 3-8%, for example, about 5%.
[0091] The negative electrode binder slurry is an aqueous slurry.
[0092] According to some embodiments of the present invention, the solid content of the surfactant slurry is 8-12%, for example, about 10%. The surfactant slurry is an aqueous slurry.
[0093] According to some embodiments of the present invention, the slurry of the organic additive has a solid content of 0.3-0.8%, for example, about 0.5%.
[0094] According to some embodiments of the present invention, the components of the negative electrode slurry include, by mass percentage:
[0095]
[0096] According to some embodiments of the present invention, the electrolyte includes potassium hydroxide, lithium hydroxide, zinc oxide and solvent water.
[0097] The mass concentration of the potassium hydroxide in the electrolyte is 20-30%, for example, about 25% or about 26%.
[0098] The mass concentration of the lithium hydroxide in the electrolyte is 0.01-0.05%, for example, about 0.02% or about 0.03%.
[0099] The concentration of the zinc oxide in the electrolyte is its saturation concentration.
[0100] According to some embodiments of the present invention, the material of the diaphragm includes at least one of PP and PE.
[0101] According to some embodiments of the present invention, the membrane is a melt-mixed hydrophilic membrane.
[0102] In more detail, the separator has a bag-like structure. The positive electrode and the negative electrode are placed in the separator respectively. Then, the positive electrode and the separator are composed of components, and the negative electrode and the separator are composed of components.
[0103] According to some embodiments of the present invention, the thickness of a single layer of the separator is 150-200 μm, for example, about 170 μm, 180 μm or about 190 μm.
[0104] In actual production, a suitable diaphragm can be selected according to needs, cost, etc., as long as it has suitable hydrophilicity; the present invention does not make strict limitations.
[0105] According to an embodiment of the fourth aspect of the present invention, there is provided a nickel-zinc battery positive electrode, or an application of the nickel-zinc battery in the field of power batteries, energy storage batteries and batteries for 3C small household appliances.
[0106] Since the application adopts all the technical solutions of the nickel-zinc battery positive electrode or nickel-zinc battery of the above-mentioned embodiments, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiments.
[0107] If there is no special explanation, the actual meaning of “about” in the present invention is that the error is allowed to be within the range of ±2%, for example, about 100 is actually 100±2%×100.
[0108] Unless otherwise specified, “between” in the present invention includes the number itself, for example, “between 2 and 3” includes the endpoint values 2 and 3.
[0109] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be obvious from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0110] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0111] Figure 1 This is the apparent morphology of the nickel-zinc battery positive electrode obtained in Example 1 of the present invention.
[0112] Figure 2 This is the apparent morphology of the positive electrode of the nickel-zinc battery obtained in Comparative Example 1 of the present invention.
[0113] Figure 3 This is the cycle performance result of the nickel-zinc battery obtained in the application example of the present invention.
[0114] Figure 4 is a SEM image of bismuth oxide used in the examples of the present invention. DETAILED DESCRIPTION
[0115] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0116] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0117] If there is no special explanation, in the specific implementation manner, the positive electrode of the nickel-zinc battery is:
[0118] Nickel hydroxide, model FC05Ⅲ, has a quasi-spherical structure, in which about 2.5% zinc is doped and about 4.5% cobalt is coated (the percentages are the mass percentages of the nickel hydroxide).
[0119] The D50 particle size of the nickel powder is about 2.5 μm; specifically, it is carbonyl nickel powder.
[0120] The particle size distribution of yttrium oxide is between 20nm and 150nm.
[0121] Example 1
[0122] In this example, a nickel-zinc battery positive electrode was prepared, and the designed capacity of the nickel-zinc battery positive electrode was 2.5Ah / piece; the specific preparation raw materials are shown in Table 1, and the specific preparation process is as follows:
[0123] S1. The positive electrode binder PTFE is formulated into a positive electrode binder slurry having a solid content of 60%;
[0124] The positive electrode active material spherical nickel hydroxide, positive electrode binder slurry, positive electrode additive bismuth oxide (morphology as Figure 4 As shown, it has a spherical structure and a particle size of about 0.1 to 1 μm), yttrium oxide and nickel powder, thickener CMC and pure water are mixed according to the proportions in Table 1 to prepare a slurry;
[0125] S2. Coat the slurry obtained in step S1 on the surface of the positive electrode current collector precursor nickel foam, and roll-press after drying.
[0126] The precursor nickel foam used has a pore number of 110PPI and a porosity of 96.5%; the thickness is about 1.6mm; after pre-pressing, the thickness is obtained as shown in Table 2, that is, between 0.9 and 1mm, and is used as a positive electrode collector semi-finished product for later coating; after coating, roller pressing is performed to obtain the final electrode sheet and positive electrode collector thickness as shown in Table 2.
[0127] The density of the slurry, the thickness of the nickel foam, the wet film thickness obtained by slurry coating, the thickness between rollers during rolling, and the thickness of the obtained nickel-zinc battery positive electrode are shown in Table 2.
[0128] Table 1 Composition of slurry used for preparing positive electrode of nickel-zinc battery in Examples and Comparative Examples (by mass percentage)
[0129]
[0130] Table 2 Process parameters for preparing positive electrodes for nickel-zinc batteries in Examples and Comparative Examples
[0131]
[0132] In Table 2, the pole piece weight is the weight of a single pole piece, including the coating area of 76.5×94 mm and the reserved welding edge of 6×76.5 mm.
[0133] Examples 2 to 4 and Comparative Example 1 respectively prepared a nickel-zinc battery positive electrode, which differed from Example 1 in that:
[0134] The preparation raw materials are slightly different, and the specific preparation raw materials are shown in Table 1.
[0135] Due to the differences in the above-mentioned raw materials, there are slight differences in the process parameters, and the specific differences are shown in Table 2.
[0136] Application Examples
[0137] This example provides a nickel-zinc battery, specifically:
[0138] A positive electrode, which is a positive electrode of a nickel-zinc battery from an embodiment or a comparative example;
[0139] The preparation process of the negative electrode is:
[0140] With reference to the ratio in Table 3, the negative electrode slurry was prepared, and the negative electrode slurry was coated on the surface of the negative electrode current collector pre-pressed to a thickness of 0.8 mm, and the scraper gap was controlled to be 0.85 mm and then dried.
[0141] The parameters of the negative electrode current collector are as follows: tin-plated punched burr copper strip, substrate 0.05 mm, burr thickness after punching 1.1 mm, hole size 1×1 mm, hole spacing 1 mm, and 0.8 mm after pre-pressing.
[0142] Table 3 Composition of the negative electrode slurry of nickel-zinc battery used in the application example (by mass percentage)
[0143]
[0144] In Table 3, the D50 particle size of zinc oxide is about 0.75 μm. The mesh size of zinc is between 400 and 500 mesh, which means it can pass through a 400 mesh sieve, but not a 500 mesh sieve. The D50 particle size of bismuth oxide is about 1.05 μm. The particle size of indium hydroxide is distributed between 20 and 70 nm.
[0145] Diaphragm: A bag is made of a non-woven diaphragm made of 180μm thick PP / PE spray-melt fiber after sulfonation. The positive electrode is placed in the bag. The microporous membrane extruded from the PP / PE mixture of Ceagard in the United States is hydrophilically treated and wrapped with two layers for the negative electrode, and then the positive and negative electrodes are stacked.
[0146] Electrolyte: 26% potassium hydroxide as the main component, 0.02% lithium hydroxide added, saturated zinc oxide.
[0147] Assembly: 8 pieces of nickel-zinc battery positive electrodes, 9 pieces of nickel-zinc battery negative electrodes and separators are stacked and arranged, and the battery capacity is set to 20Ah, and the battery dry weight is obtained as shown in Table 4. The nickel-zinc battery is obtained after liquid injection, packaging and formation. In this example, some process parameters of the nickel-zinc battery are shown in Table 4 and below.
[0148] The charge is divided into three stages: the first stage is 0.4A charging for 0.5h, standing for 0.1h, 4A charging for 3h, with the cut-off voltage set to 1.95V, standing for 0.1h, 2A charging for 4h, standing for 0.1h, 4A discharging cut-off voltage at 1.4V, standing for 0.1h; the second stage is 4A charging for 3.5h, with the cut-off voltage set to 1.95V, standing for 0.1h, 2A charging for 2h, standing for 0.1h, 1A charging for 4h, standing for 0.1h, 4A discharging cut-off voltage at 1.4V, standing for 0.1h; the third stage is 2A charging for 3h, standing for 0.1h, and 1A charging for 6h.
[0149] Table 4 Some process parameters of nickel-zinc batteries
[0150]
[0151] Combined with the parameters in Table 1, it can be seen that the ratio of positive electrode additives to positive electrode active materials has changed in different embodiments. The amount of positive electrode additives used will affect the polarization of the nickel-zinc battery to a certain extent, and may also affect the charge and discharge mechanism of the positive electrode to a certain extent, and then affect the capacity of the positive electrode of the nickel-zinc battery in the first stage of formation to a certain extent. With the subsequent formation and the progress of charge and discharge, the above differences are narrowed, but there are still differences, and in the continued cycle process, the above differences will be widened again.
[0152] Test Case
[0153] In the first aspect of this example, the appearance of the positive electrode of the nickel-zinc battery obtained in the embodiment and the comparative example was observed. The results showed that compared with the positive electrode of the nickel-zinc battery obtained in comparative example 1, the surface of the nickel-zinc battery obtained in the embodiment had fewer pore structures, smaller pores, and a smoother surface. The specific results are as follows: Figures 1-2 shown.
[0154] The second aspect of this example tests the capacity (100% capacity is planned to be 20Ah) and cycle performance of the battery obtained in the application example. The specific test method is: cycle at 90% DOD (18Ah), and the cycle current is planned to be 4A; if the capacity is less than 60% (12Ah), use 0.2C (limited to 1C current density is 20A) deep charge and discharge once or more; if the capacity is restored and is not less than 60% DOD, continue to cycle at 90% DOD, otherwise stop cycling; record the cycle capacity after 210 cycles. The test results are shown in Table 5 and Figure 3 shown.
[0155] Table 5 Cycling performance of nickel-zinc batteries obtained in application examples
[0156]
[0157]
[0158] According to the results in Tables 4 and 5, under the same conditions, as the amount of bismuth oxide added to the positive electrode of the nickel-zinc battery increases, its discharge capacity shows a trend of first increasing and then decreasing, with a peak at about 8% (the amount of bismuth oxide in the slurry, the corresponding mass percentage in the positive electrode coating is about 10%); at the same time, the internal resistance of the battery before and after formation also reached the lowest point at about 8%. This shows that adding bismuth oxide to the positive electrode can not only improve the conductivity of the positive electrode of the nickel-zinc battery, but also improve the capacity of the nickel-zinc battery.
[0159] Furthermore, according to Table 5 and Figure 3 The results show that the cycle stability of the nickel-zinc batteries of Examples 1 to 4 is also significantly better than that of Comparative Example 1, and among the examples, the result of Example 3 is the best. It can be seen that adding bismuth oxide to the positive electrode can also improve the corrosion resistance of the positive electrode of the nickel-zinc battery, thereby improving the cycle stability.
[0160] In summary, the nickel-zinc battery positive electrode provided by the present invention or the nickel-zinc battery including the above-mentioned nickel-zinc battery positive electrode has lower internal resistance, higher capacity, and more stable cycle performance; therefore, it is expected to be widely used in the field of power batteries, energy storage batteries or 3C small household appliance batteries.
[0161] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A nickel-zinc battery positive electrode, characterized in that: The positive electrode of the nickel-zinc battery includes a positive electrode current collector and a positive electrode coating covering the surface of the positive electrode current collector; The raw materials for preparing the positive electrode coating include, by weight: 52-92 parts of positive electrode active material; Positive electrode additive 0.51 to 20.1 parts; 0.6 to 4.8 parts of positive electrode binder; The positive electrode additive includes bismuth oxide.
2. The nickel-zinc battery positive electrode according to claim 1, characterized in that: The positive electrode active material includes spherical nickel hydroxide.
3. The nickel-zinc battery positive electrode according to claim 1, characterized in that: The positive electrode additive also includes yttrium oxide and nickel powder; preferably, the mass ratio of bismuth oxide to yttrium oxide is 0.5-20:0.01-0.10; preferably, the mass ratio of nickel powder to the positive electrode active material is 1-7:51-85.
4. The nickel-zinc battery positive electrode according to claim 1, characterized in that: The raw materials for preparing the positive electrode coating further include a thickener; preferably, the mass ratio of the thickener to the binder is 0.5-5:0.6-4.
8.
5. The nickel-zinc battery positive electrode according to any one of claims 1 to 4, characterized in that: The raw material for preparing the positive electrode current collector includes foamed nickel.
6. A method for preparing a positive electrode for a nickel-zinc battery as claimed in any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: S1. Providing a slurry comprising raw materials for preparing the positive electrode of the nickel-zinc battery; S2. The slurry is coated on the surface of the positive electrode current collector precursor, and then rolled after drying.
7. A nickel-zinc battery, characterized in that: The nickel-zinc battery comprises a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte that soaks the positive electrode, the negative electrode and the separator; The positive electrode is the nickel-zinc battery positive electrode as claimed in any one of claims 1 to 5.
8. The nickel-zinc battery according to claim 7, characterized in that: The negative electrode comprises a negative electrode current collector and a negative electrode coating disposed on the surface of the negative electrode current collector; and / or, raw materials for preparing the negative electrode coating include negative electrode active materials, inorganic oxide additives, organic additives, surfactants and negative electrode binders.
9. The nickel-zinc battery according to claim 8, characterized in that: The negative electrode active material includes zinc and zinc oxide; preferably, the inorganic oxide additive includes bismuth oxide and indium hydroxide; preferably, the organic additive includes PAAK; preferably, the surfactant is SDBS; preferably, the negative electrode binder is PVA and / or PTFE.
10. Use of a nickel-zinc battery positive electrode as claimed in any one of claims 1 to 5, or a nickel-zinc battery as claimed in any one of claims 7 to 9 in the fields of power batteries, energy storage batteries and batteries for 3C small household appliances.
Citation Information
Cited By
Preparation method of zinc-nickel battery negative electrode
CN119864377A
A method for preparing a negative electrode of a zinc-nickel battery
CN119864377B