Preparation process of Zn-Mg-Cu aluminum alloy
By adjusting the elemental composition and optimizing the heat treatment process, the cracking and deformation problems of 7075 aluminum alloy during processing were solved, and its tensile strength, yield strength and corrosion resistance were improved, thus meeting the requirements for high performance.
Patent Information
- Application Number
- CN202411112477.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-08
AI Technical Summary
The existing 7075 aluminum alloy is prone to cracking or deformation during processing, and its performance is difficult to meet the growing demand for high performance.
By adjusting the composition of elements such as Fe, Si, Cu, Mg and Zn in 7075 aluminum alloy, optimizing the ratio of Cu, Mg and Zn, adding mixed rare earth elements Er-Sc-Ce, and adopting multi-stage homogenization and heat treatment processes, including solution treatment, water quenching and multi-stage aging treatment, the microstructure of the alloy is optimized.
It significantly improves the tensile strength, yield strength and elongation at break of aluminum alloys, achieves the EA level for exfoliation corrosion, solves the problems of cracking and deformation during processing, and broadens the application range.
Smart Images

Figure CN118910481A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy materials, and in particular to a preparation process of a Zn-Mg-Cu series aluminum alloy. Background Art
[0002] Aluminum alloy is the most widely used type of nonferrous metal material in industry, and has been widely used in aviation, aerospace, automobile, machinery manufacturing, shipbuilding and chemical industries. Al-Zn-Mg-Cu aluminum alloy belongs to the 7 series ultra-high strength aluminum alloy. This series of alloys has a high yield ratio and specific strength, and is widely used in the fields of aerospace and transportation. At present, a series of ultra-high strength aluminum alloys such as 7050, 7055, 7068, and 7150 have been developed at home and abroad. However, with the rapid development of science and technology and society, and the continuous growth of demand for aluminum alloys in related industries, it has become the focus of attention in the industry to meet higher performance requirements through reasonable processing technology. As a heat-treatable aging-strengthening alloy, heat and aging treatment play a key role in improving the performance of 7xxx series high-strength aluminum alloys. This application aims to further develop and optimize the formula of 7075 aluminum alloy and the preparation aging heat treatment process, so that the excellent properties of the alloy such as high strength, high toughness, and corrosion resistance can be fully utilized, and solve the problem that 7075 aluminum alloy is prone to cracks or deformation during processing. Summary of the invention
[0003] In view of the problems existing in the prior art, the embodiment of the present application proposes a preparation process of a Zn-Mg-Cu aluminum alloy, aiming to improve the mechanical properties and corrosion resistance of the aluminum alloy material and solve the problem of easy cracking or deformation.
[0004] In order to achieve the above object, the preparation process proposed by the present invention specifically comprises the following steps:
[0005] Step 1: Take a 7075 aluminum alloy ingot, use anhydrous ethanol to high-pressure wash the surface of the aluminum alloy ingot to remove impurities, then place the 7075 aluminum alloy ingot after impurities removal in a pre-baking furnace and heat it to 325℃~345℃, then put it into a melting furnace, heat it to 695℃~715℃ at a rate of 20℃ / min to melt it into molten metal, and after the raw materials in the melting furnace are completely melted, perform electromagnetic stirring for 75min, and the stirring speed is 80~100r / min;
[0006] Step 2: Adjust the temperature of the smelting furnace to 735°C to 755°C, and perform refining treatment on the aluminum alloy melt. The refining agent adopts the introduction of N2-Cl2-Co mixed gas to achieve the combined refining treatment of the aluminum alloy melt. The refining time is set to 12 minutes. During the refining, electromagnetic stirring is performed and the scum on the surface is removed.
[0007] Step 3: After refining, the material composition is analyzed by spectral analysis, and mixed rare earth elements (Er-Sc-Ce) are added according to the actual composition of the material, and the alloy is melted at a melting temperature of 705°C to 725°C. After melting, the alloy liquid is slightly stirred without breaking the covering agent on the surface of the alloy liquid. Then, the alloy liquid composition is checked by spectral analysis and the material composition is adjusted until the following requirements are met;
[0008] Silicon ≤ 0.15%, iron ≤ 0.2%, copper 1.3% to 1.8%, manganese ≤ 0.1%, magnesium 2.21% to 3.06%, chromium 0.18% to 0.28%, zinc 5.2% to 7.2%, titanium 0.4%, mixed rare earth 0.35% and the balance Al;
[0009] Step 4: After the composition is qualified, the alloy melt is subjected to static treatment by a dynamic temperature control high temperature and long time process. Specifically, the alloy melt is first heated to 760°C at a rate of 6°C / min and kept at this temperature for 5 minutes; then the alloy melt is heated to 780°C at a rate of 4°C / min and kept at this temperature for 12 minutes; then the alloy melt is cooled to 755°C at a rate of 5°C / min and kept at this temperature for 8 minutes; finally, the alloy melt is cooled to 715°C at a rate of 3°C / min and kept at this temperature for 15 minutes;
[0010] Step 5: The obtained alloy melt is gravity casted, the casting temperature is controlled at 675-685℃, the mold temperature is 315-325℃, and the casting speed is 25mm / min. During casting, the aluminum liquid should be poured into the mold gate evenly and stably, and the flow should not be interrupted in the middle. After casting, wait for the aluminum liquid at the riser to solidify, cool it for 15 minutes before opening the mold to avoid damage to the test rod caused by opening the mold at high temperature;
[0011] Step 6: homogenizing the alloy ingot;
[0012] Step 7: removing the surface layer of the alloy ingot and forging it into a billet, and the forging temperature is set at 396°C to 404°C;
[0013] Step 8: heat treating the prepared alloy billet.
[0014] Furthermore, in step 1, when the aluminum alloy ingot is gradually melted, the pre-configured covering agent is added to the melting furnace in three equal portions, and the temperatures of the melting furnace are 420° C., 560° C. and 680° C. during the three additions.
[0015] Preferably, the covering agent comprises the following components by weight: 32 parts of sodium chloride, 40 parts of potassium chloride, 5 parts of calcium fluoride, 3 parts of aluminum chloride and 43 parts of Na3AIF.
[0016] Furthermore, in step 2, the volume ratio of each gas component in the N2-Cl2-Co mixed gas, V(N2):V(Cl2):V(Co), is 7:2:1.
[0017] Furthermore, in the step three, the mixed rare earth includes Sc, Ce and Er, and the weight ratio between the three is 4:2:1.
[0018] Furthermore, in the step three, the weight ratio of Cu:Mg:Zn is 1:1.7:4.
[0019] Furthermore, in step 6, the homogenization process includes the following stages in sequence:
[0020] Ⅰ. Homogenization temperature is 358℃~362℃, and the holding time is 8h;
[0021] Ⅱ. The homogenization temperature is 444℃~448℃, and the holding time is 16h;
[0022] III. The homogenization temperature is 536℃~542℃ and the holding time is 24h;
[0023] IV. Air cool to room temperature; before stage I, the heating rate of the alloy ingot is 120°C / h; during stages I to II, the heating rate of the alloy ingot is 80°C / h; during stages II to III, the heating rate of the alloy ingot is 60°C / h.
[0024] Furthermore, in step eight, the heat treatment comprises the following steps in sequence:
[0025] Solution treatment: treatment temperature 458℃~462℃, holding time 2.5h;
[0026] Water quenching: Use room temperature water to quench the blank, cool it to room temperature, and pre-compress the blank with 2.75% permanent cold deformation;
[0027] Primary aging: treatment temperature 126℃~132℃, insulation time 12h;
[0028] Secondary aging: treatment temperature 188℃~194℃, holding time 1.5h;
[0029] Level 3 aging: keep in liquid nitrogen at -196℃ for 25min;
[0030] Fourth-level aging: treatment temperature is 126℃~132℃, holding time is 8h; and before solution treatment, the heating rate of the alloy billet is 120℃ / h; during water quenching from room temperature to first-level aging, the heating rate of the alloy billet is 60℃ / h;
[0031] During the primary aging to secondary aging process, the heating rate of the alloy billet is 80℃ / h;
[0032] During the secondary aging to the tertiary aging, the cooling rate of the alloy billet is 150℃ / h;
[0033] From the third-stage aging process to the fourth-stage aging process, the heating rate of the alloy billet is 100℃ / h.
[0034] Compared with the prior art, the present invention has at least the following beneficial effects: on the basis of the original formula of 7075 aluminum alloy, the embodiment of the present application adjusts the elemental components such as Fe, Si, Cu, Mg and Zn in the alloy, optimizes the ratio between Cu, Mg and Zn, adds mixed rare earth and the selection and ratio of its elemental components, and optimizes the homogenization and heat treatment of the alloy, so that the aluminum alloy material prepared in the embodiment of the present application has higher tensile strength, yield strength and elongation at break, and the exfoliation corrosion grade of the alloy material reaches EA level, and solves the problem that the 7075 aluminum alloy is prone to cracks or deformation during the processing process, significantly improves the performance of the aluminum alloy material, broadens its application occasions and fields, and meets the growing social and scientific and technological development needs. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.
[0036] Figure 1 This is a process flow chart of a preparation process of a Zn-Mg-Cu aluminum alloy provided in an embodiment of the present application; DETAILED DESCRIPTION
[0037] The specific implementation modes of the present invention are further described below in conjunction with examples. The following examples are only used to more clearly illustrate the technical solutions of the present invention, and are not intended to limit the protection scope of the present invention.
[0038] Example 1
[0039] Example 1 of the present application discloses a preparation process of a Zn-Mg-Cu aluminum alloy, comprising the following steps:
[0040] Step 1: Take a 7075 aluminum alloy ingot, use anhydrous ethanol to high-pressure wash the surface of the aluminum alloy ingot to remove impurities, then place the 7075 aluminum alloy ingot after impurities removal in a pre-baking furnace and heat it to 335°C, then put it into a melting furnace, heat it to 705°C at a rate of 20°C / min to melt it into molten metal, and after the raw materials in the melting furnace are completely melted, perform electromagnetic stirring for 75 minutes, and the stirring speed is 80-100r / min;
[0041] In the process of gradually melting the aluminum alloy ingot, the pre-configured covering agent is added to the melting furnace in three equal portions, wherein the temperatures of the melting furnace are 420° C., 560° C. and 680° C. during the three additions, respectively. The formula composition (by weight) of the covering agent is shown in Table 1 below:
[0042] Table 1:
[0043]
[0044] Step 2: adjusting the temperature of the smelting furnace to 745°C, refining the aluminum alloy melt, using a refining agent to pass a N2-Cl2-Co mixed gas to achieve a combined refining treatment of the aluminum alloy melt, the refining setting time is 12 minutes, electromagnetic stirring is performed during refining to remove surface scum, and the volume ratio of each gas component in the N2-Cl2-Co mixed gas is 7:2:1 [V(N2):V(Cl2):V(Co)];
[0045] Step 3: After refining, the material composition is analyzed by spectral analysis, and according to the actual composition of the material, a mixed rare earth element component (Er-Sc-Ce) is added, and the alloy is melted at a melting temperature of 715°C. After melting, the alloy liquid is slightly stirred without breaking the covering agent on the surface of the alloy liquid, and then the alloy liquid composition is spectrally analyzed and checked and the material composition is adjusted (the adjustment includes adjusting the ratio between the contents of Cu-Mg-Zn and the contents of silicon, iron, and manganese, etc.) until the content requirements of each element component in Table 2 below are met;
[0046] Table 2: Element composition of Zn-Mg-Cu aluminum alloy in the present embodiment
[0047]
[0048]
[0049] Step 4: After the composition is qualified, the alloy melt is subjected to static treatment using a dynamic temperature control high temperature and long time process. Specifically, the alloy melt is first heated to 760°C at a rate of 6°C / min and kept warm for 5 minutes; then the alloy melt is heated to 780°C at a rate of 4°C / min and kept warm for 12 minutes; then the alloy melt is cooled to 755°C at a rate of 5°C / min and kept warm for 8 minutes; finally, the alloy melt is cooled to 715°C at a rate of 3°C / min and kept warm for 15 minutes.
[0050] Step 5: The obtained alloy melt is gravity casted, the casting temperature is controlled at 680℃, the mold temperature is 320℃, and the casting speed is 25mm / min. During casting, the molten aluminum should be poured into the mold gate evenly and stably, and the flow should not be interrupted in the middle. After casting, wait for the riser aluminum liquid to solidify, cool it for 15 minutes and then open the mold to avoid damage to the test rod caused by opening the mold at high temperature.
[0051] Step 6: The alloy ingot is homogenized. The process is divided into four stages, as shown in Table 3 below:
[0052] Table 3: Ingot homogenization
[0053]
[0054] Step 7: removing the surface layer of the alloy ingot and forging it into a billet, and the forging temperature is set at 400°C;
[0055] Step 8: heat treating the obtained alloy billet, which includes the following stages, as shown in Table 4 below:
[0056] Table 4: Heat treatment of blanks
[0057]
[0058]
[0059] Example 2
[0060] Embodiment 2 of the present application discloses a preparation process of a Zn-Mg-Cu aluminum alloy, comprising the following steps:
[0061] Step 1: Take a 7075 aluminum alloy ingot, use anhydrous ethanol to high-pressure wash the surface of the aluminum alloy ingot to remove impurities, then place the 7075 aluminum alloy ingot after impurities removal in a pre-baking furnace and heat it to 325°C, then put it into a melting furnace, heat it to 695°C at a rate of 20°C / min to melt it into molten metal, and after the raw materials in the melting furnace are completely melted, perform electromagnetic stirring for 75 minutes, and the stirring speed is 80-100r / min;
[0062] In the process of gradually melting the aluminum alloy ingot, the pre-configured covering agent is added to the melting furnace in three equal portions, wherein the temperatures of the melting furnace are 420° C., 560° C. and 680° C. during the three additions, respectively. The formula composition of the covering agent is shown in Table 1 above:
[0063] Step 2: adjusting the temperature of the smelting furnace to 735°C, refining the aluminum alloy melt, using a refining agent to pass a N2-Cl2-Co mixed gas to achieve a combined refining treatment of the aluminum alloy melt, the refining setting time is 12 minutes, electromagnetic stirring is performed during refining, and the scum on the surface is removed, and the volume ratio of each gas component in the N2-Cl2-Co mixed gas is 7:2:1 [V(N2):V(Cl2):V(Co)];
[0064] Step 3: After refining, the material composition is analyzed by spectral analysis, and according to the actual composition of the material, a mixed rare earth element component (Er-Sc-Ce) is added, and the alloy is melted at a melting temperature of 705°C. After melting, the alloy liquid is slightly stirred without breaking the covering agent on the surface of the alloy liquid, and then the alloy liquid composition is checked by spectral analysis and the material composition is adjusted (the adjustment includes adjusting the ratio between the contents of Cu-Mg-Zn, etc.) until the content requirements of each element component in Table 5 below are met;
[0065] Table 5: Element composition of Zn-Mg-Cu aluminum alloy in the present embodiment
[0066] Elemental composition Mass% silicon 0.1% iron 0.15% copper 1.5% manganese 0.05% magnesium 2.55% chromium 0.18% Zinc 6% titanium 0.4% Mixed rare earth Sc0.2%, Ce0.1%, Er0.05% other The balance is Al, and impurities ≤ 0.15%
[0067] Step 4: After the composition is qualified, the alloy melt is subjected to static treatment using a dynamic temperature control high temperature and long time process. Specifically, the alloy melt is first heated to 760°C at a rate of 6°C / min and kept warm for 5 minutes; then the alloy melt is heated to 780°C at a rate of 4°C / min and kept warm for 12 minutes; then the alloy melt is cooled to 755°C at a rate of 5°C / min and kept warm for 8 minutes; finally, the alloy melt is cooled to 715°C at a rate of 3°C / min and kept warm for 15 minutes.
[0068] Step 5: The obtained alloy melt is gravity casted, the casting temperature is controlled at 675℃, the mold temperature is 315℃, and the casting speed is 25mm / min. During casting, the molten aluminum should be poured into the mold gate evenly and stably, and the flow should not be interrupted in the middle. After casting, wait for the riser aluminum liquid to solidify, cool it for 15 minutes and then open the mold to avoid damage to the test rod caused by opening the mold at high temperature.
[0069] Step 6: The alloy ingot is homogenized. The process is divided into four stages, as shown in Table 6 below:
[0070] Table 6: Ingot homogenization
[0071]
[0072]
[0073] Step 7: removing the surface layer of the alloy ingot and forging it into a billet, and the forging temperature is set at 396°C;
[0074] Step 8: heat treating the obtained alloy billet, which includes the following stages, as shown in Table 7 below:
[0075] Table 7: Heat treatment of blanks
[0076]
[0077] Example 3
[0078] Example 3 of the present application discloses a preparation process of a Zn-Mg-Cu aluminum alloy, comprising the following steps:
[0079] Step 1: Take a 7075 aluminum alloy ingot, use anhydrous ethanol to high-pressure wash the surface of the aluminum alloy ingot to remove impurities, then place the 7075 aluminum alloy ingot after impurities removal in a pre-baking furnace and heat it to 345°C, then put it into a melting furnace, heat it to 715°C at a rate of 20°C / min to melt it into molten metal, and after the raw materials in the melting furnace are completely melted, perform electromagnetic stirring for 75 minutes, and the stirring speed is 80-100r / min;
[0080] In the process of gradually melting the aluminum alloy ingot, the pre-configured covering agent is added to the melting furnace in three equal portions, wherein the temperatures of the melting furnace are 420° C., 560° C. and 680° C. respectively during the three additions, and the formula composition of the covering agent is shown in Table 1:
[0081] Step 2: adjusting the temperature of the smelting furnace to 755°C, refining the aluminum alloy melt, using a refining agent to pass a N2-Cl2-Co mixed gas to achieve a combined refining treatment of the aluminum alloy melt, the refining setting time is 12 minutes, electromagnetic stirring is performed during refining, and the scum on the surface is removed, and the volume ratio of each gas component in the N2-Cl2-Co mixed gas is 7:2:1 [V(N2):V(Cl2):V(Co)];
[0082] Step 3: After refining, the material composition is analyzed by spectral analysis, and according to the actual composition of the material, a mixed rare earth element component (Er-Sc-Ce) is added, and the alloy is melted at a melting temperature of 725°C. After melting, the alloy liquid is slightly stirred without breaking the covering agent on the surface of the alloy liquid, and then the alloy liquid composition is checked by spectral analysis and the material composition is adjusted (the adjustment includes adjusting the ratio between the contents of Cu-Mg-Zn, etc.) until the content requirements of each element component in Table 8 below are met;
[0083] Table 8: Element composition of Zn-Mg-Cu aluminum alloy in the present embodiment
[0084] Elemental composition Mass% silicon 0.08% iron 0.1% copper 1.8% manganese 0.1% magnesium 3.06% chromium 0.28% Zinc 7.2% titanium 0.4% Mixed rare earth Sc0.2%, Ce0.1%, Er0.05% other The balance is Al, and impurities ≤ 0.15%
[0085] Step 4: After the composition is qualified, the alloy melt is subjected to static treatment using a dynamic temperature control high temperature and long time process. Specifically, the alloy melt is first heated to 760°C at a rate of 6°C / min and kept warm for 5 minutes; then the alloy melt is heated to 780°C at a rate of 4°C / min and kept warm for 12 minutes; then the alloy melt is cooled to 755°C at a rate of 5°C / min and kept warm for 8 minutes; finally, the alloy melt is cooled to 715°C at a rate of 3°C / min and kept warm for 15 minutes.
[0086] Step 5: The obtained alloy melt is gravity casted, the casting temperature is controlled at 685℃, the mold temperature is 325℃, and the casting speed is 25mm / min. During casting, the molten aluminum should be poured into the mold gate evenly and stably, and the flow should not be interrupted in the middle. After casting, wait for the riser aluminum liquid to solidify, cool it for 15 minutes and then open the mold to avoid damage to the test rod caused by opening the mold at high temperature.
[0087] Step 6: The alloy ingot is homogenized. The process is divided into four stages, as shown in Table 9 below:
[0088] Table 9: Ingot homogenization
[0089]
[0090] Step 7: removing the surface layer of the alloy ingot and forging it into a billet, and the forging temperature is set at 404°C;
[0091] Step 8: The obtained alloy billet is heat treated, and the treatment includes the following stages, as shown in Table 10 below:
[0092] Table 10: Heat treatment of blanks
[0093]
[0094]
[0095] Comparative Example 1
[0096] Comparative Example 1 is a 7075 aluminum alloy without improvement treatment, and the 7075 aluminum alloy contains the element components (by weight percentage) shown in Table 11 below:
[0097] Table 11: 7075 aluminum alloy composition
[0098]
[0099] Comparative Example 2
[0100] The difference between Comparative Example 2 and Example 1 is that the 7075 aluminum alloy T6 heat treatment process is adopted, that is, solution treatment (quenching) + complete artificial aging.
[0101] The solution treatment temperature is 495-505°C. After solution treatment for 2-3 hours, aging is performed at 120 degrees for 6 hours, and finally aging is performed at 160 degrees for 3 hours.
[0102] Comparative Example 3
[0103] The difference between Comparative Example 3 and Example 2 is that:
[0104] The silicon content is 0.4%.
[0105] Comparative Example 4
[0106] The difference between Comparative Example 4 and Example 2 is that:
[0107] The iron content is 0.5%.
[0108] Comparative Example 5
[0109] The difference between Comparative Example 5 and Example 3 is that:
[0110] The copper content is 1.2%, the magnesium content is 2.1%, and the zinc content is 5.1%.
[0111] Comparative Example 6
[0112] The difference between Comparative Example 6 and Example 3 is that:
[0113] No mixed rare earth is added to the element composition.
[0114] Comparative Example 7
[0115] The difference between Comparative Example 7 and Example 1 is that:
[0116] The mixed rare earth is only Sc0.35%.
[0117] Comparative Example 8
[0118] The difference between Comparative Example 8 and Example 1 is that:
[0119] The mixed rare earth is only Ce0.35%.
[0120] Comparative Example 9
[0121] The difference between Comparative Example 9 and Example 1 is that:
[0122] The mixed rare earth is only Er0.35%.
[0123] Comparative Example 10
[0124] The difference between Comparative Example 10 and Example 1 is that:
[0125] The mixed rare earth is Sc0.2% and Ce0.15%.
[0126] Comparative Example 11
[0127] The difference between Comparative Example 11 and Example 1 is that:
[0128] The mixed rare earth is Sc0.25% and Er0.1%.
[0129] Comparative Example 12
[0130] The difference between Comparative Example 12 and Example 1 is that:
[0131] The mixed rare earth is Ce0.25% and Er0.1%.
[0132] Comparative Example 13
[0133] The difference between Comparative Example 13 and Example 1 is that:
[0134] The mixed rare earth is Sc0.15%, Ce0.1%, Er0.1%.
[0135] Test example
[0136] The performance of the aluminum alloys obtained in the above comparative examples 4-13 was tested by the same testing method as in Examples 1-3. The results are shown in Table 12.
[0137] Table 12: Performance test results
[0138]
[0139]
[0140] Combined with the test data in Table 12, it should be noted that:
[0141] (1) The performance of the aluminum alloy prepared in the embodiment of the present application is significantly better than the existing 7075 aluminum alloy on the market, and is also better than other comparative examples set in the present application. By setting these comparative examples, it can be seen that if the content of each element component is not within the protection scope of the present application, or some components are out of the formula, or the aging heat treatment method is changed, the mechanical properties, corrosion resistance and material quality of the aluminum alloy cannot be taken into account, resulting in a decline in the above-mentioned properties to varying degrees;
[0142] (2) In the embodiments of the present application, based on the performance parameters in Table 12, it can be seen that the solution of Embodiment 1 is the best example, and the solutions of Embodiments 2 and 3 are relatively good examples;
[0143] (3) Compared with the existing 7075 aluminum alloy on the market, the tensile strength of the aluminum alloy prepared in the embodiment of the present application is increased by 17.9%, the yield strength is increased by 20.7%, the elongation at break is increased by three percentage points, and the exfoliation corrosion level is increased by two levels. In addition, the aluminum alloy prepared in the embodiment of the present application solves the problem of cracks or deformation that are easy to occur during processing;
[0144] (4) Compared with the conventional T6 heat treatment process, the multi-stage homogenization + solution quenching + multi-stage aging adopted in the embodiment of the present application has a more complicated process procedure, but it makes the strength, toughness, corrosion resistance, etc. of the alloy material optimally matched. Specifically, the above-mentioned process adopted in the embodiment of the present application can better make the grain size and distribution, composition and performance inside the aluminum alloy uniform and stable, and produce elongation phase and dispersed phase inside the alloy crystal, better eliminate the defects such as grain boundary, non-equilibrium crystallization low melting point phase, internal stress, intergranular oxidation, casting, etc. inside the material, achieve the purpose of spacing reduction and grain refinement, stabilize the organizational state of the alloy body, and at the same time improve the plastic deformation ability of the alloy, making it easier to process and shape, thereby improving the quality of the aluminum alloy material.
[0145] (5) According to Comparative Example 3, the silicon content in the embodiment of the present application cannot be too high. When the silicon content reaches 0.4% of the 7075 aluminum alloy, coarse block or needle-shaped eutectic silicon will be formed, resulting in pores and crystallization of aluminum silicide in the aluminum alloy, which will cause the alloy material to have a more obvious decline in mechanical properties, corrosion resistance, processing performance and material quality.
[0146] (6) According to Comparative Example 4, it can be seen that the iron content in the embodiment of the present application cannot be too high. When the iron content reaches 0.5% of the 7075 aluminum alloy, the iron atoms in the solid solution will precipitate to form iron compounds and form polycrystals at the grain boundaries, resulting in a decrease in the strength of the alloy material and affecting the stability of the grain boundaries, which can easily lead to fractures and voids. In addition, excessive addition of Fe will generate Al-Fe-Si compounds, and Fe-Si compounds will significantly reduce the ductility of the aluminum alloy. In addition, excessive iron elements will also form a metastable phase similar to ψ(FeAl3) together with elements such as copper and magnesium, resulting in a decrease in the corrosion resistance of the aluminum alloy material.
[0147] (7) In the embodiments of the present application, the weight ratio of Cu, Mg and Zn is limited to 1:1.7:4. When the three elements are in the above weight ratio, copper, magnesium and zinc can better combine with each other to form a strengthening phase and form a solid solution phase with Al. If the above weight ratio is not adopted, it will lead to insufficient lack of strengthening phase and solid solution phase and / or formation of excess phase between grains, thereby causing the strength at the grain boundary to decrease, the alloy to become brittle, and the toughness to decrease.
[0148] (8) In the embodiment of the present application, by adding mixed rare earth elements Sc, Ce and Er (the total content is less than 0.35wt%) in a weight ratio of 4:2:1, it is helpful to better remove harmful impurities in the alloy, refine impurities or change their morphology, so that the grains are refined and evenly distributed. When the content of the mixed rare earth is 0.35%, the grains of the α (Al) phase are the smallest, which plays a good role in refining the grains. As the amount of rare earth increases further, the grains gradually become larger. Therefore, the rare earth content in the aluminum alloy material of the embodiment of the present application is not easy to exceed 0.35%. In addition, experimental studies have found that there is a latent period for the modification of rare earth on aluminum alloys. The embodiment of the present application adopts a high-temperature and long-term process with dynamic temperature control and heat treatment operations to enable the rare earth elements to play the most effective modification effect.
[0149] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A process for preparing a Zn-Mg-Cu aluminum alloy, characterized in that: The following steps are involved: Step 1: Take a 7075 aluminum alloy ingot, use anhydrous ethanol to high-pressure wash the surface of the aluminum alloy ingot to remove impurities, then place the 7075 aluminum alloy ingot after impurities removal in a pre-baking furnace and heat it to 325℃~345℃, then put it into a melting furnace, heat it to 695℃~715℃ at a rate of 20℃ / min to melt it into molten metal, and after the raw materials in the melting furnace are completely melted, perform electromagnetic stirring for 75min, and the stirring speed is 80~100r / min; Step 2: Adjust the temperature of the smelting furnace to 735°C to 755°C, and perform refining treatment on the aluminum alloy melt. The refining agent adopts the introduction of N2-Cl2-Co mixed gas to achieve the combined refining treatment of the aluminum alloy melt. The refining time is set to 12 minutes. During the refining, electromagnetic stirring is performed and the scum on the surface is removed. Step 3: After refining, the material composition is analyzed by spectral analysis, and mixed rare earth elements (Er-Sc-Ce) are added according to the actual composition of the material, and the alloy is melted at a melting temperature of 705°C to 725°C. After melting, the alloy liquid is slightly stirred without breaking the covering agent on the surface of the alloy liquid. Then, the alloy liquid composition is checked by spectral analysis and the material composition is adjusted until the following requirements are met; Silicon ≤ 0.15%, iron ≤ 0.2%, copper 1.3% to 1.8%, manganese ≤ 0.1%, magnesium 2.21% to 3.06%, chromium 0.18% to 0.28%, zinc 5.2% to 7.2%, titanium 0.4%, mixed rare earth 0.35% and the balance Al; Step 4: After the composition is qualified, the alloy melt is subjected to static treatment by a dynamic temperature control high temperature and long time process. Specifically, the alloy melt is first heated to 760°C at a rate of 6°C / min and kept at this temperature for 5 minutes; then the alloy melt is heated to 780°C at a rate of 4°C / min and kept at this temperature for 12 minutes; then the alloy melt is cooled to 755°C at a rate of 5°C / min and kept at this temperature for 8 minutes; finally, the alloy melt is cooled to 715°C at a rate of 3°C / min and kept at this temperature for 15 minutes; Step 5: The obtained alloy melt is gravity casted, the casting temperature is controlled at 675-685℃, the mold temperature is 315-325℃, and the casting speed is 25mm / min. During casting, the aluminum liquid should be poured into the mold gate evenly and stably, and the flow should not be interrupted in the middle. After casting, wait for the aluminum liquid at the riser to solidify, cool it for 15 minutes before opening the mold to avoid damage to the test rod caused by opening the mold at high temperature; Step 6: homogenizing the alloy ingot; Step 7: removing the surface layer of the alloy ingot and forging it into a billet, and the forging temperature is set at 396°C to 404°C; Step 8: heat treating the prepared alloy billet.
2. The preparation process according to claim 1, characterized in that: In the step 1, when the aluminum alloy ingot is gradually melted, the pre-configured covering agent is added into the melting furnace in three equal portions, and the temperatures of the melting furnace are 420° C., 560° C. and 680° C. during the three additions.
3. The preparation process according to claim 2, characterized in that: The covering agent comprises the following components by weight: 32 parts of sodium chloride, 40 parts of potassium chloride, 5 parts of calcium fluoride, 3 parts of aluminum chloride and 43 parts of Na3AIF.
4. The preparation process according to claim 1, characterized in that: In step 2, the volume ratio of each gas component in the N2-Cl2-Co mixed gas V(N2):V(Cl2):V(Co) is 7:2:
1.
5. The preparation process according to claim 1, characterized in that: In the step 3, the mixed rare earth includes Sc, Ce and Er, and the weight ratio of the three is 4:2:
1.
6. The preparation process according to claim 1, characterized in that: In the step three, the weight ratio of Cu:Mg:Zn is 1:1.7:
4.
7. The preparation process according to claim 1, characterized in that: In step 6, the homogenization process includes the following stages in sequence: Ⅰ. Homogenization temperature is 358℃~362℃, and the holding time is 8h; Ⅱ. The homogenization temperature is 444℃~448℃, and the holding time is 16h; III. The homogenization temperature is 536℃~542℃, and the holding time is 24h; IV. Air cool to room temperature.
8. The preparation process according to claim 7, characterized in that: Before stage I, the heating rate of the alloy ingot was 120°C / h; during stage I to II, the heating rate of the alloy ingot was 80°C / h; during stage II to III, the heating rate of the alloy ingot was 60°C / h.
9. The preparation process according to claim 1, characterized in that: In the step eight, the heat treatment comprises the following steps in sequence: Solution treatment: treatment temperature 458℃~462℃, holding time 2.5h; Water quenching: Use room temperature water to quench the blank, cool it to room temperature, and pre-compress the blank with 2.75% permanent cold deformation; Primary aging: treatment temperature 126℃~132℃, insulation time 12h; Secondary aging: treatment temperature 188℃~194℃, holding time 1.5h; Level 3 aging: keep in liquid nitrogen at -196℃ for 25min; Level 4 aging: treatment temperature 126℃~132℃, holding time 8h.
10. The preparation process according to claim 9, characterized in that: Before solution treatment, the alloy billet was heated at a rate of 120°C / h; during water quenching from room temperature to primary aging, the alloy billet was heated at a rate of 60°C / h; During the primary aging to secondary aging process, the heating rate of the alloy billet is 80℃ / h; During the secondary aging to the tertiary aging, the cooling rate of the alloy billet is 150℃ / h; From the third-stage aging process to the fourth-stage aging process, the heating rate of the alloy billet is 100℃ / h.