Method for improving smelting stability of converter based on flue gas information

By monitoring the CO content of the flue gas in the converter smelting and adjusting the oxygen gun height and oxygen supply strength, the problems of overflow and splashing in the high-speed rail consumption smelting mode are solved, the stability and production efficiency of the converter smelting are improved, and the efficient dephosphorization effect is achieved .

CN118910492AActive Publication Date: 2024-11-08SHOUGANG GROUP CO LTD +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410819590.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-08
Estimated Expiration
2044-06-24

AI Technical Summary

Technical Problem

In converter smelting, under the high-speed rail consumption mode, the heat in the furnace is unbalanced, resulting in frequent overflow or splashing. The traditional monitoring methods have subjectivity and hysteresis, which affects the stability and safety of smelting.

Method used

By monitoring the flue gas CO content output from the converter smelting, adjusting the oxygen gun height and oxygen supply intensity, controlling the oxygen gun height and ore feeding speed in stages, dynamically adjusting the smelting process, reducing the melt pool temperature and promoting dephosphorization reaction.

Benefits of technology

It effectively reduces the occurrence of overflow and splashing, improves smelting stability, and achieves efficient production, with a dephosphorization rate of 95.2%, and a terminal phosphorus content of less than 0.005%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910492A_ABST
    Figure CN118910492A_ABST
Patent Text Reader

Abstract

The invention provides a method for improving converter smelting stability based on flue gas information, and belongs to the field of converter smelting. The method comprises the steps that waste steel, first ore and molten iron are sequentially mixed, and a steelmaking raw material is obtained; the steelmaking raw materials are subjected to converter smelting, and the CO content of converter smelting output flue gas is obtained; when the oxygen blowing amount of converter smelting is within a set oxygen blowing amount range, the height of an oxygen lance is adjusted according to the CO content; the set oxygen blowing amount range is larger than 65% and smaller than or equal to 85%. When the oxygen blowing amount is larger than 65% and smaller than or equal to 85%, the situation of unstable smelting, such as spilled slag splashing or drying, easily occurs, the proceeding degree of physical and chemical reactions in the furnace can be directly reflected according to the mass fraction of CO in flue gas information, the height of the oxygen lance is dynamically controlled in a staged mode, and therefore the reaction process is controlled, and the oxygen blowing amount is controlled to be larger than 65% and smaller than or equal to 85%. And therefore, the smelting stability of the converter is improved, and spilled slag splashing or drying is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of converter smelting, and in particular to a method for improving converter smelting stability based on flue gas information. Background Art

[0002] According to the previous research results on the scrap steel ratio and the benefit per ton of steel, although increasing the scrap steel ratio can reduce environmental pollution, reduce comprehensive energy consumption and improve productivity, when the scrap steel price is high, significantly increasing the scrap steel ratio will not only increase the converter smelting cost, but also cause problems such as low converter terminal temperature hit rate, long smelting cycle, large slag volume and high post-blowing rate. Therefore, from the perspective of low converter smelting cost, the optimal scrap steel ratio is often no more than 20%, that is, the converter needs to adopt a high iron consumption smelting mode. When the converter adopts the high iron consumption smelting mode, due to the small amount of scrap steel added, the abundant heat in the furnace needs to be balanced by slag-making agents, which makes the molten pool temperature rise faster, and ultimately causes the carbon-oxygen reaction in the furnace to develop unevenly, and eventually leads to slag overflow or splashing.

[0003] The converter is a high-temperature, high-pressure, multi-element and multi-phase reaction vessel. During the normal smelting process, only a certain degree of splashing occurs in the furnace, which usually does not cause a large amount of metal loss or dangerous accidents. However, when the splashing of slag or metal droplets exceeds the controllable range in the furnace, it violently impacts the furnace lining and flies out of the furnace mouth. In severe cases, it will surge out of the furnace mouth in large quantities, causing dangerous accidents, which is often called converter splashing. Slag overflow and splashing during the blowing process are the most frequent types of accidents. This phenomenon is the overflow of slag and metal liquid in the furnace caused by the impact of the oxygen stream in the blowing process and the gas escape of the decarburization reaction, which has a significant impact on the safety and economy of converter smelting. In the traditional converter steelmaking process, operators usually judge the occurrence of slag overflow or splashing by observing the furnace mouth flame or using sonar slag removal. Among them, the observation method has a strong subjectivity, and sonar slag removal not only has a certain hysteresis, but also its monitoring signal is greatly affected by the stability of smelting in the furnace. Therefore, the probability of slag overflow or splashing is high. In this context, the stable operation of the converter's high iron consumption smelting mode has become a technical difficulty, seriously affecting the efficient production of the converter. Summary of the invention

[0004] The present application provides a method for improving the stability of converter smelting based on flue gas information to solve the following technical problem: how to improve the stability of converter smelting to reduce the occurrence of slag overflow, splashing or back drying during the smelting process.

[0005] The present application provides a method for improving converter smelting stability based on flue gas information, the method comprising:

[0006] Mixing scrap steel, first ore and molten iron in sequence to obtain steelmaking raw materials;

[0007] The steel-making raw material is subjected to converter smelting, and the CO content of the output flue gas of the converter smelting is obtained;

[0008] When the oxygen blowing amount of the converter smelting is within the set oxygen blowing amount range, the oxygen lance height is adjusted according to the CO content; the set oxygen blowing amount range is >65% and ≤85%.

[0009] Optionally, adjusting the oxygen lance height according to the CO content includes:

[0010] According to the CO content, the oxygen lance height is adjusted; wherein,

[0011] In terms of mass fraction, if 48% < the CO content < 55%, the oxygen lance height is adjusted to the reference height;

[0012] If the CO content is ≤48% by mass fraction, the oxygen lance height is adjusted to be lowered by 0.15m to 0.25m from the base height;

[0013] In terms of mass fraction, if 55% ≤ the CO content < 60%, the oxygen lance height is adjusted to be increased by 0.15m to 0.25m on the basis of the reference height;

[0014] If the CO content is ≥ 60% by mass fraction, the oxygen lance height is adjusted to be increased by 0.25 m to 0.35 m based on the reference height.

[0015] Optionally, the reference height satisfies the following relationship:

[0016] When 65%<oxygen blowing amount≤70%, the reference height is 2.0m;

[0017] When 70%<oxygen blowing amount≤78%, the reference height is 2.25m;

[0018] When 78%<oxygen blowing amount≤85%, the reference height is 2.1m.

[0019] Optionally, the scrap steel accounts for 10% to 20% by mass of the steelmaking raw material; the temperature of the molten iron is ≥1360°C; and the Si content of the molten iron is ≥0.25% by mass fraction.

[0020] Optionally, the method further comprises: controlling the oxygen lance height in stages during the converter smelting process; wherein,

[0021] When 0≤oxygen blowing amount≤6%, the oxygen lance height is 2.2m;

[0022] When 6%<oxygen blowing amount≤28%, the oxygen lance height is 2.0m;

[0023] When 28%<oxygen blowing amount≤65%, the oxygen lance height is 1.8m;

[0024] When 85%<oxygen blowing amount≤100%, the height of the oxygen lance is 1.9m.

[0025] Optionally, the method further comprises: controlling the oxygen supply intensity in stages during the converter smelting process; wherein,

[0026] When 0≤oxygen blowing amount≤40%, the oxygen supply intensity is slowly increased to 2.7Nm 3 / (t·min)~2.9Nm 3 / (t·min);

[0027] When the oxygen blowing amount is greater than 40%, the oxygen supply intensity is slowly increased to 3.0 Nm 3 / (t·min)~3.2Nm 3 / (t·min).

[0028] Optionally, the method also includes: during the converter smelting process, when the oxygen blowing amount is 4% to 6%, adding a second ore; the feeding rate of the second ore is 0.8t / min to 1.2t / min, the total amount of the first ore and the second ore added is 26kg / t·steel to 40kg / t·steel, and the ratio of the first ore added to the total amount added is 40% to 50%.

[0029] Optionally, the method further comprises: adding limestone, lime and light-burned dolomite into the converter in stages during the converter smelting process; wherein,

[0030] When 4%≤oxygen blowing amount≤6%, limestone, lime and light-burned dolomite with the first-stage addition amount are added into the furnace; the first-stage addition amount of the limestone is 11kg / t·steel to 12kg / t·steel; the first-stage addition amount of the lime is 12.5kg / t·steel to 15kg / t·steel; the first-stage addition amount of the light-burned dolomite is 8.5kg / t·steel to 9.5kg / t·steel;

[0031] When 20%≤oxygen blowing amount≤23%, limestone, lime and light-burned dolomite with second-stage addition amount are added into the furnace; the second-stage addition amount of limestone is 6kg / t·steel to 8kg / t·steel; the second-stage addition amount of lime is 12.5kg / t·steel to 15kg / t·steel; the second-stage addition amount of light-burned dolomite is 8.5kg / t·steel to 9.5kg / t·steel.

[0032] Optionally, the bottom blowing gas supply intensity of the converter smelting is 0.03Nm 3 / (t·min)~0.09Nm 3 / (t·min).

[0033] Optionally, measured by mass fraction, the P content of the final molten steel of the converter smelting is ≤0.0080%, and the O content is ≤0.06%; the temperature of the final molten steel of the converter smelting is 1620°C~1660°C; the final slag basicity of the converter smelting is 3.2~3.8, and measured by mass fraction, the TFe content of the final slag is 14%~18%, and the MgO content of the final slag is 8%~12%.

[0034] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0035] The present application provides a method for improving the stability of converter smelting based on flue gas information, comprising: mixing scrap steel, first ore and molten iron in sequence to obtain steelmaking raw materials; subjecting the steelmaking raw materials to converter smelting and obtaining the CO content of the converter smelting output flue gas; when the oxygen blowing amount of the converter smelting is within the set oxygen blowing amount range, adjusting the oxygen lance height according to the CO content; the set oxygen blowing amount range is greater than 65% and less than or equal to 85%. By adding ore to the smelting raw materials, the temperature of the molten pool in the early stage of smelting is reduced, which is conducive to the dephosphorization reaction and promotes the early slag; when the oxygen blowing amount reaches the oxygen blowing amount range greater than 65% and less than or equal to 85%, unstable smelting is prone to occur, such as slag overflow, splashing or back drying. The mass fraction of CO in the flue gas information can directly reflect the degree of decarburization reaction in the reactor, and the oxygen lance height is dynamically controlled in stages to control the reaction process, thereby improving the stability of converter smelting and reducing the occurrence of slag overflow or splashing. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0037] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0038] Figure 1 A flow chart of a method for improving converter smelting stability based on flue gas information provided in an embodiment of the present application. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0040] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0041] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.

[0042] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0043] Figure 1A flow chart of a method for improving converter smelting stability based on flue gas information provided in an embodiment of the present application.

[0044] See also Figure 1 The present application provides a method for improving converter smelting stability based on flue gas information, which is applicable to 180-300 ton converters. The method comprises:

[0045] S1, mixing scrap steel, a first ore and molten iron in sequence to obtain steelmaking raw materials;

[0046] In some embodiments, the scrap steel accounts for 10% to 20% by mass of the steelmaking raw material; the temperature of the molten iron is ≥1360°C; and the Si content of the molten iron is ≥0.25% by mass.

[0047] In some embodiments, step S1 may specifically include: adding scrap steel and the first ore into a converter, and then filling molten iron into the converter to obtain steelmaking raw materials.

[0048] The mass proportion of scrap steel in steelmaking raw materials is 10% to 20%, that is, the scrap steel ratio entering the furnace accounts for 10% to 20% of the total loading amount. The reason for adopting this loading system is that the price of scrap steel is relatively high at present. If a larger scrap steel loading system is adopted, it is not conducive to the benefit of ton steel; the reason for adding ore into the converter before adding iron is that it reduces the temperature of the molten pool in the early stage of smelting, which is conducive to the dephosphorization reaction and promotes the early slag. Exemplarily, the mass proportion of scrap steel in steelmaking raw materials can be 10%, 12%, 14%, 16%, 18%, 20%, etc.; the temperature of molten iron can be 1360℃, 1365℃, 1370℃, 1375℃, 1380℃, etc.; in terms of mass fraction, the Si content of molten iron can be 0.25%, 0.26%, 0.27%, 0.28%, 0.30%, etc.

[0049] S2, smelting the steelmaking raw material in a converter, and obtaining the CO content of the flue gas output from the converter smelting;

[0050] In recent years, with the continuous improvement of computer computing power and monitoring capabilities of detection equipment, it is increasingly conducive to the development of flue gas steelmaking models. The application of flue gas steelmaking models in production can not only predict and dynamically adjust the reaction and slag state in the furnace, but also realize full closed-loop dynamic control. This feature has become a key research direction for improving the stability of converter smelting. During the converter smelting process, the information of converter smelting output flue gas is obtained in real time.

[0051] S3. When the oxygen blowing amount of the converter smelting is within the set oxygen blowing amount range, the oxygen lance height is adjusted according to the CO content; the set oxygen blowing amount range is >65% and ≤85%.

[0052] It should be noted that the oxygen blowing amount in the present application refers to the volume fraction of the top blowing oxygen supply to the total oxygen supply.

[0053] Based on flue gas analysis, the converter blowing process can be carried out efficiently and stably; this invention can not only avoid the human error brought by empirical steelmaking, but also avoid the long delay effect of sonar slagging, and can predict slag overflow or splashing in the furnace, reducing the occurrence of slag overflow and splashing during the blowing process; under this loading condition, through the control of dynamic gun position, not only can the occurrence of slag overflow or splashing during the blowing process be effectively avoided, but also the dephosphorization reaction in the converter can be promoted. The dephosphorization rate can reach 95.2%, and the final phosphorus content can reach 0.0044%, thereby realizing efficient and stable production of the converter.

[0054] When the oxygen blowing amount reaches the oxygen blowing amount range of >65% and ≤85%, smelting instability is likely to occur, such as slag overflow or splashing. After a lot of research, it was found that the oxygen lance height can be dynamically controlled in stages according to the flue gas information, thereby reducing the occurrence of slag overflow or splashing.

[0055] In some embodiments, adjusting the oxygen lance height according to the CO content includes: adjusting the oxygen lance height according to the CO content; wherein, in terms of mass fraction, if 48% < the CO content < 55%, the oxygen lance height is adjusted to a reference height; in terms of mass fraction, if the CO content ≤ 48%, the oxygen lance height is adjusted to be reduced by 0.15 m to 0.25 m based on the reference height; in terms of mass fraction, if 55% ≤ the CO content < 60%, the oxygen lance height is adjusted to be increased by 0.15 m to 0.25 m based on the reference height; in terms of mass fraction, if the CO content ≥ 60%, the oxygen lance height is adjusted to be increased by 0.25 m to 0.35 m based on the reference height.

[0056] In some embodiments, the reference height satisfies the following relationship: when 65%<oxygen blowing amount≤70%, the reference height is 2.0m; when 70%<oxygen blowing amount≤78%, the reference height is 2.25m; when 78%<oxygen blowing amount≤85%, the reference height is 2.1m.

[0057] During the converter blowing process, the oxygen lance height is controlled according to the CO mass fraction in the flue gas information; the reason for adopting this lance position control strategy is that the CO mass fraction in the flue gas information directly reflects the degree of decarburization reaction in the furnace. Therefore, after determining the standard value range of the CO mass fraction, adjusting the lance position height based on the benchmark lance position is more instructive for controlling the degree of reaction in the furnace.

[0058] According to the mass fraction of CO in the flue gas information, which directly reflects the degree of decarbonization reaction in the furnace, the oxygen lance height is dynamically adjusted based on the reference oxygen lance height. If the CO mass fraction is within the standard value range (48% to 55%), no intervention is required. If it is not within the standard range, intervention is performed. The CO mass fraction is restored to the standard value range and the dynamic oxygen lance height is restored to the reference height value.

[0059] Exemplarily, when the oxygen blowing amount is in the range of >65% and <70%, the mass fraction of CO in the flue gas information is in the standard value range, and the oxygen lance height is 2.0m at this time; when the oxygen blowing amount reaches 70%, the mass fraction of CO in the flue gas information increases to 58%, the oxygen lance height is adjusted to 2.45m, and the mass fraction of CO in the flue gas information decreases. When the oxygen blowing amount reaches 75%, the mass fraction of CO in the flue gas information returns to the standard value range, and the oxygen lance height is adjusted to 2.25m. When the oxygen blowing amount is in the range of 75% to 78%, the oxygen lance height is fixed at 2.25m; when the oxygen blowing amount is >78% and ≤85%, the mass fraction of CO in the flue gas information is in the standard value range, and the oxygen lance height is fixed at 2.1m.

[0060] In some embodiments, the method also includes: controlling the oxygen lance height in stages during the converter smelting process; wherein, when 0≤oxygen blowing amount≤6%, the oxygen lance height is 2.2m; when 6%<oxygen blowing amount≤28%, the oxygen lance height is 2.0m; when 28%<oxygen blowing amount≤65%, the oxygen lance height is 1.8m; when 85%<oxygen blowing amount≤100%, the oxygen lance height is 1.9m.

[0061] The oxygen lance height control in the present application is specifically as follows: the oxygen lance height is controlled in stages. When the oxygen blowing amount is [0-65]% and (85-100]%, the oxygen lance height is fixedly controlled; when the oxygen blowing amount is (65-85]%, the oxygen lance height is dynamically controlled in stages, that is, according to the flue gas information, it is dynamically adjusted on the basis of the reference oxygen lance height.

[0062] In some embodiments, the method further comprises: controlling the oxygen supply intensity in stages during the converter smelting process; wherein, when 0 ≤ oxygen blowing amount ≤ 40%, the oxygen supply intensity is slowly increased to 2.7 Nm 3 / (t·min)~2.9Nm 3 / (t·min); When the oxygen blowing amount is greater than 40%, the oxygen supply intensity is slowly increased to 3.0Nm 3 / (t·min)~3.2Nm 3 / (t·min).

[0063] The oxygen supply intensity is controlled in stages: when the oxygen blowing volume is 0-40%, the oxygen flow rate increases slowly; when the oxygen blowing volume is 40%, the oxygen supply intensity is controlled to 2.7Nm3 / (t·min)~2.9Nm 3 / (t·min), when the oxygen supply is greater than 40%, slowly increase the oxygen supply intensity to 3.0Nm 3 / (t·min)~3.2Nm 3 / (t·min). During the converter blowing process, the top blowing oxygen supply intensity is controlled according to the oxygen supply amount; the reason for adopting this oxygen supply system is that since a certain amount of ore is added before iron addition, there are more iron oxides in the molten pool, which is conducive to the early slag reduction. Therefore, the oxygen supply intensity does not need to be too large in the initial stage of smelting. If the oxygen supply intensity is too large during this period, it will cause the molten pool to heat up too fast, and eventually lead to incomplete dephosphorization, slag overflow or splashing. When 0≤oxygen blowing amount≤40%, the oxygen supply intensity can be slowly increased to 2.7Nm 3 / (t·min),2.75m 3 / (t·min),2.8m 3 / (t·min),2.85m 3 / (t·min),2.9Nm 3 / (t·min), etc.; when the oxygen blowing amount is greater than 40%, the oxygen supply intensity can be slowly increased to 3.0Nm 3 / (t·min),3.05m 3 / (t·min),3.1m 3 / (t·min),3.15m 3 / (t·min),3.2Nm 3 / (t·min), etc.

[0064] In some embodiments, the method further includes: during the converter smelting process, when the oxygen blowing amount is 4% to 6%, adding a second ore; the feeding rate of the second ore is 0.8t / min to 1.2t / min, the total amount of the first ore and the second ore added is 26kg / t·steel to 40kg / t·steel, and the ratio of the first ore added to the total amount added is 40% to 50%.

[0065] During the converter blowing process, the feeding rate of iron ore is controlled; the reason for adopting this ore feeding rate is: on the one hand, the heating rate of the molten pool can be suppressed, and on the other hand, the temperature of the molten pool can be maintained within a certain range, which has no adverse effect on the reaction rate in the furnace. Exemplarily, the feeding rate of the second ore is 0.8t / min, 0.9t / min, 1.0t / min, 1.1t / min, 1.2t / min, etc., the total amount of the first ore and the second ore added is 26kg / t·steel, 30kg / t·steel, 32kg / t·steel, 35kg / t·steel, 40kg / t·steel, etc., and the ratio of the amount of the first ore added to the total amount added can be 40%, 42%, 44%, 46%, 48%, 50%, etc.

[0066] In some embodiments, the method further comprises: adding limestone, lime and light-burned dolomite into the furnace in stages during the converter smelting process; wherein, when 4%≤oxygen blowing amount≤6%, adding the limestone, lime and light-burned dolomite with the first-stage addition amount into the furnace; the first-stage addition amount of the limestone is 11kg / t·steel to 12kg / t·steel; the first-stage addition amount of the lime is 12.5kg / t·steel to 15kg / t·steel; the first-stage addition amount of the light-burned dolomite is 10 ... The first stage addition amount is 8.5kg / t·steel to 9.5kg / t·steel; when 20%≤oxygen blowing amount≤23%, limestone, lime and light-burned dolomite with the second stage addition amount are added into the furnace; the second stage addition amount of the limestone is 6kg / t·steel to 8kg / t·steel; the second stage addition amount of the lime is 12.5kg / t·steel to 15kg / t·steel; the second stage addition amount of the light-burned dolomite is 8.5kg / t·steel to 9.5kg / t·steel.

[0067] The reason for adding limestone, lime and light-burned dolomite into the converter in stages during the converter blowing process is that the thermal state in the converter is different at different blowing stages. Adding limestone, lime and light-burned dolomite in stages not only helps the formation of slag, but also helps to control the thermal state in the furnace and improve the blowing stability.

[0068] In some embodiments, the bottom blowing gas supply intensity of the converter smelting is 0.03Nm 3 / (t·min)~0.09Nm 3 / (t·min).

[0069] During the converter blowing process, controlling the bottom blowing gas supply intensity can ensure that the molten pool has good dynamic conditions and promote the chemical reaction in the molten pool. For example, the bottom blowing gas supply intensity of the converter smelting can be 0.03Nm 3 / (t·min), 0.04Nm 3 / (t·min), 0.05Nm 3 / (t·min), 0.06Nm 3 / (t·min), 0.08Nm 3 / (t·min), 0.09Nm 3 / (t·min), etc.

[0070] In some embodiments, the P content of the final molten steel of the converter smelting is ≤0.0080%, and the O content is ≤0.06%, calculated by mass fraction; the temperature of the final molten steel of the converter smelting is 1620°C~1660°C; the final slag basicity of the converter smelting is 3.2~3.8, and the final slag TFe content is 18%~24%, and the final slag MgO content is 8%~12%, calculated by mass fraction.

[0071] Controlling the temperature of the molten steel after tapping to 1620-1660°C is helpful to control the phosphorus mass fraction of the molten steel at the end point; controlling the oxygen mass fraction after tapping to ≤0.06% can not only ensure the reaction in the furnace, but also help reduce the consumption of alloy in the subsequent process and the control of inclusions; controlling the basicity of the final slag to 3.2-3.8 can not only ensure the control of the phosphorus content in the final molten steel, but also help to slow down the erosion of the slag on the furnace lining; controlling the final slag TFe to 14%-18% can not only ensure the chemical reaction in the furnace, but also help to reduce the consumption of metal materials; controlling the final slag MgO to 8-12% is helpful to adjust the slag viscosity and facilitate the implementation of the subsequent slag splashing furnace protection process.

[0072] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.

[0073] The following examples and comparative examples all adopt a 210-ton top and bottom blown converter for smelting.

[0074] Example 1

[0075] This embodiment provides a method for improving converter smelting stability based on flue gas information, comprising the following steps:

[0076] S11, mixing scrap steel, the first ore and molten iron in sequence to obtain steelmaking raw materials; the scrap steel ratio charged into the furnace accounts for 11.7% of the total charge amount, the molten iron temperature is 1375° C., and the silicon content of the molten iron is 0.342%; the addition amount of the first ore is 15 kg / t·steel;

[0077] S21, subjecting the steel-making raw materials to converter smelting, and obtaining the CO content of the flue gas output from the converter smelting; during the converter smelting process, when the oxygen blowing amount is 4-6%, the addition amounts of lime, limestone and light-burned dolomite are 15kg / t·steel, 11.5kg / t·steel and 8.5kg / t·steel respectively, and when the oxygen blowing amount is 20-23%, the addition amounts of lime, limestone and light-burned dolomite are 14.8kg / t·steel, 6.5kg / t·steel and 9kg / t·steel respectively; when the oxygen blowing amount is 4-6%, the second ore is added at a feeding speed of 1t / min, and the addition amount of the second ore is 18.4kg / t·steel;

[0078] S31. When the oxygen blowing amount of the converter smelting is within the set oxygen blowing amount range, the oxygen lance height is adjusted according to the CO content; the set oxygen blowing amount range is >65% and ≤85%, when 65<oxygen blowing amount≤70, the CO content is 52%, and the corresponding lance position is 2.0m, when 70<oxygen blowing amount≤78, the CO content is 58%, and the corresponding lance position is 2.4m, when 78<oxygen blowing amount≤85, the CO content is 51%, and the corresponding lance position is 2.1m;

[0079] The temperature of the molten steel after tapping is 1626°C; the oxygen mass fraction after tapping is 0.041%; the final slag basicity is 3.76; the final slag TFe is 19.0%; the final slag MgO is 10.1%; slag overflow or splashing occurs during the entire smelting process, and the dephosphorization rate and final phosphorus content are 95.2% and 0.0044% respectively.

[0080] Example 2

[0081] This embodiment provides a method for improving converter smelting stability based on flue gas information, comprising the following steps:

[0082] S11, mixing scrap steel, the first ore and molten iron in sequence to obtain steelmaking raw materials; the scrap steel ratio charged into the furnace accounts for 10.3% of the total charge amount, the molten iron temperature is 1366° C., and the silicon content of the molten iron is 0.286%; the addition amount of the first ore is 17.5 kg / t·steel;

[0083] S21, subjecting the steel-making raw materials to converter smelting, and obtaining the CO content of the flue gas output from the converter smelting; during the converter smelting process, when the oxygen blowing amount is 4-6%, the addition amounts of lime, limestone and light-burned dolomite are 14kg / t·steel, 11.5kg / t·steel and 9kg / t·steel respectively, and when the oxygen blowing amount is 20-23%, the addition amounts of lime, limestone and light-burned dolomite are 16kg / t·steel, 6.7kg / t·steel and 9.5kg / t·steel respectively; when the oxygen blowing amount is 4-6%, the second ore is added at a feeding rate of 1t / min, and the addition amount of the second ore is 18kg / t·steel;

[0084] S31. When the oxygen blowing amount of the converter smelting is within the set oxygen blowing amount range, the oxygen lance height is adjusted according to the CO content; the set oxygen blowing amount range is >65% and ≤85%, when 65<oxygen blowing amount≤70, the CO content is 57%, and the corresponding lance position is 2.15m, when 70<oxygen blowing amount≤78, the CO content is 56%, and the corresponding lance position is 2.45m, when 78<oxygen blowing amount≤85, the CO content is 50%, and the corresponding lance position is 2.1m;

[0085] The temperature of the molten steel after tapping is 1638℃; the oxygen mass fraction after tapping is 0.0524%; the final slag basicity is 3.51; the final slag TFe is 20.3%; the final slag MgO is 8.04%. Slag overflow or splashing occurs during the entire smelting process, and the dephosphorization rate and final phosphorus content are 94.0% and 0.0057% respectively.

[0086] Example 3

[0087] This embodiment provides a method for improving converter smelting stability based on flue gas information, comprising the following steps:

[0088] S11, mixing scrap steel, the first ore and molten iron in sequence to obtain steelmaking raw materials; the scrap steel ratio charged into the furnace accounts for 11% of the total charge amount, the molten iron temperature is 1367° C., and the silicon content of the molten iron is 0.259%; the addition amount of the first ore is 12.5 kg / t·steel;

[0089] S21, subjecting the steel-making raw materials to converter smelting, and obtaining the CO content of the flue gas output from the converter smelting; during the converter smelting process, when the oxygen blowing amount is 4-6%, the addition amounts of lime, limestone and light-burned dolomite are 13kg / t·steel, 11.3kg / t·steel and 8.6kg / t·steel respectively, and when the oxygen blowing amount is 20-23%, the addition amounts of lime, limestone and light-burned dolomite are 12.2kg / t·steel, 8.3kg / t·steel and 8.6kg / t·steel respectively; when the oxygen blowing amount is 4-6%, the second ore is added at a feeding rate of 1t / min, and the addition amount of the second ore is 14.2kg / t·steel;

[0090] S31. When the oxygen blowing amount of the converter smelting is within the set oxygen blowing amount range, the oxygen lance height is adjusted according to the CO content; the set oxygen blowing amount range is >65% and ≤85%, when 65<oxygen blowing amount≤70, the CO content is 52%, and the corresponding lance position is 2.0m, when 70<oxygen blowing amount≤78, the CO content is 62%, and the corresponding lance position is 2.55m, when 78<oxygen blowing amount≤85, the CO content is 56%, and the corresponding lance position is 2.25m;

[0091] The temperature of the molten steel after tapping is 1640°C; the oxygen mass fraction after tapping is 0.0575%; the final slag basicity is 3.44; the final slag TFe is 19.1%; the final slag MgO is 9.51%; slag overflow or splashing occurs during the entire smelting process, and the dephosphorization rate and final phosphorus content are 94.0% and 0.0065% respectively.

[0092] Comparative Example 1

[0093] This comparative example provides a method for improving converter smelting stability, comprising the following steps:

[0094] S11, mixing scrap steel and molten iron to obtain steelmaking raw materials; the scrap steel ratio into the furnace accounts for 10.6% of the total charge amount, the molten iron temperature is 1375° C., and the silicon content of the molten iron is 0.198%;

[0095] S21, subjecting the steel-making raw materials to converter smelting, during the converter smelting process, when the oxygen blowing amount is 4-6%, the addition amounts of lime, limestone, light-burned dolomite and cooling slag-forming agent are 17.3kg / t·steel, 10.6kg / t·steel, 8.3kg / t·steel and 6.4kg / t·steel respectively, and when the oxygen blowing amount is 20-23%, the addition amounts of lime, limestone, light-burned dolomite and cooling slag-forming agent are 15.2kg / t·steel, 6.6kg / t·steel, 8kg / t·steel and 3.4kg / t·steel respectively; when the oxygen blowing amount is 4-6%, ore is added at a feeding speed of 1t / min, and the addition amount of ore is 15.4kg / t·steel;

[0096] The temperature of the molten steel after tapping is 1688℃; the oxygen mass fraction after tapping is 0.0450%; the final slag basicity is 3.09; the final slag TFe is 16.4%; the final slag MgO is 11.1%; a certain degree of slag overflow occurs in the early stage of smelting, and the slag overflow time lasts for 1.2 minutes, and slight splashing occurs in the later stage. The dephosphorization rate and final phosphorus content are 82.1% and 0.0175% respectively.

[0097] In addition, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:

[0098] In the embodiments of the present invention, the occurrence of slag overflow or splashing during the production process of a converter with high iron consumption can be solved.

[0099] In the embodiment of the present invention, based on the flue gas analysis, the converter blowing process can be carried out efficiently and stably; the invention can not only avoid the human error brought by the experience of steelmaking, but also avoid the long delay effect of sonar slagging, and can predict the slag overflow or splashing in the furnace, thereby reducing the occurrence of slag overflow and splashing during the blowing process; under this loading condition, through the control of the dynamic gun position, not only can the occurrence of slag overflow or splashing during the blowing process be effectively avoided, but also the dephosphorization reaction in the converter can be promoted, the dephosphorization rate can reach 95.2%, and the final phosphorus content can reach 0.0044%, thereby realizing efficient and stable production of the converter.

[0100] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for improving converter smelting stability based on flue gas information, It is characterized in that The method comprises: Mixing scrap steel, first ore and molten iron in sequence to obtain steelmaking raw materials; The steel-making raw material is subjected to converter smelting, and the CO content of the output flue gas of the converter smelting is obtained; When the oxygen blowing amount of the converter smelting is within the set oxygen blowing amount range, the oxygen lance height is adjusted according to the CO content; the set oxygen blowing amount range is >65% and ≤85%.

2. The method according to claim 1, It is characterized in that The step of adjusting the oxygen lance height according to the CO content includes: According to the CO content, the oxygen lance height is adjusted; wherein, In terms of mass fraction, if 48% < the CO content < 55%, the oxygen lance height is adjusted to the reference height; If the CO content is ≤48% by mass fraction, the oxygen lance height is adjusted to be lowered by 0.15m to 0.25m from the base height; In terms of mass fraction, if 55% ≤ the CO content < 60%, the oxygen lance height is adjusted to be increased by 0.15m to 0.25m on the basis of the reference height; If the CO content is ≥ 60% by mass fraction, the oxygen lance height is adjusted to be increased by 0.25 m to 0.35 m based on the reference height.

3. The method according to claim 2, It is characterized in that The reference height satisfies the following relationship: When 65%<oxygen blowing amount≤70%, the reference height is 2.0m; When 70%<oxygen blowing amount≤78%, the reference height is 2.25m; When 78%<oxygen blowing amount≤85%, the reference height is 2.1m.

4. The method according to claim 1, It is characterized in that The scrap steel accounts for 10% to 20% of the steelmaking raw materials by mass; the temperature of the molten iron is ≥1360°C; and the Si content of the molten iron is ≥0.25% by mass.

5. The method according to claim 1, It is characterized in that The method further comprises: controlling the oxygen lance height in stages during the converter smelting process; wherein, When 0≤oxygen blowing amount≤6%, the oxygen lance height is 2.2m; When 6%<oxygen blowing amount≤28%, the oxygen lance height is 2.0m; When 28%<oxygen blowing amount≤65%, the oxygen lance height is 1.8m; When 85%<oxygen blowing amount≤100%, the height of the oxygen lance is 1.9m.

6. The method according to claim 1, It is characterized in that The method further comprises: controlling the oxygen supply intensity in stages during the converter smelting process; wherein, When 0≤oxygen blowing amount≤40%, the oxygen supply intensity is slowly increased to 2.7Nm 3 / (t·min)~2.9Nm 3 / (t·min); When the oxygen blowing amount is greater than 40%, the oxygen supply intensity is slowly increased to 3.0 Nm 3 / (t·min)~3.2Nm 3 / (t·min).

7. The method according to claim 1, It is characterized in that The method also includes: during the converter smelting process, when the oxygen blowing amount is 4% to 6%, adding a second ore; the feeding speed of the second ore is 0.8t / min to 1.2t / min, the total amount of the first ore and the second ore added is 26kg / t·steel to 40kg / t·steel, and the ratio of the amount of the first ore added to the total amount added is 40% to 50%.

8. The method according to claim 1, It is characterized in that The method further comprises: adding limestone, lime and light-burned dolomite into the converter in stages during the converter smelting process; wherein, When 4%≤oxygen blowing amount≤6%, limestone, lime and light-burned dolomite with the first-stage addition amount are added into the furnace; the first-stage addition amount of the limestone is 11kg / t·steel to 12kg / t·steel; the first-stage addition amount of the lime is 12.5kg / t·steel to 15kg / t·steel; the first-stage addition amount of the light-burned dolomite is 8.5kg / t·steel to 9.5kg / t·steel; When 20%≤oxygen blowing amount≤23%, limestone, lime and light-burned dolomite with second-stage addition amount are added into the furnace; the second-stage addition amount of limestone is 6kg / t·steel to 8kg / t·steel; the second-stage addition amount of lime is 12.5kg / t·steel to 15kg / t·steel; the second-stage addition amount of light-burned dolomite is 8.5kg / t·steel to 9.5kg / t·steel.

9. The method according to claim 1, It is characterized in that The bottom blowing gas supply intensity of the converter smelting is 0.03Nm 3 / (t·min)~0.09Nm 3 / (t·min).

10. The method according to claim 1, It is characterized in that Calculated by mass fraction, the P content of the final molten steel in the converter smelting is ≤0.0080%, and the O content is ≤0.06%; the temperature of the final molten steel in the converter smelting is 1620°C~1660°C; the final slag basicity of the converter smelting is 3.2~3.8, and calculated by mass fraction, the TFe content of the final slag is 14%~18%, and the MgO content of the final slag is 8%~12%.

Citation Information

Patent Citations

  • Iron bath-type melting furnace

    CN102066584A

  • Method, device and system for controlling furnace conditions of convertor steelmaking

    CN102363825A

  • Method for dynamically judging state in converter based on CO volume percentage content curve

    CN111172346A

  • Converter flame splashing state monitoring method, device and equipment and storage medium

    CN117496429A

  • Control method of converter operation model based on high scrap ratio condition

    CN117512250A