900MPa-grade magnetic pole steel for pumped storage hydroelectric generating set and production method of 900MPa-grade magnetic pole steel
By producing 900MPa grade magnetic pole steel through specific chemical composition and process, the problems of insufficient strength and magnetic induction performance in the existing technology have been solved, and high-strength, low-cost magnetic pole steel manufacturing has been achieved.
Patent Information
- Application Number
- CN202410971449.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Existing technologies make it difficult to produce magnetic pole steel for pumped storage hydroelectric generators with a yield strength ≥900MPa, elongation A ≥12%, magnetic induction performance B50 ≥1.6T, and thickness ≤2.0mm, and the cost is relatively high.
By employing specific chemical compositions and processes, including controlling the homogenization temperature of the billet, the cooling rate of hot rolling, and the annealing temperature, 900MPa grade magnetic pole steel is produced, avoiding the use of expensive alloying elements.
Magnetic pole steel with a yield strength ≥900MPa, elongation A ≥12%, and magnetic induction performance B50 ≥1.6T, with a thickness ≤2.0mm, has been achieved, reducing production costs.
Smart Images

Figure BDA0004953346170000061 
Figure BDA0004953346170000062 
Figure BDA0004953346170000071
Abstract
Description
Technical Field
[0001] The present invention relates to a steel for motor and a production method, specifically to a 900MPa grade magnetic pole steel for pumped storage hydroelectric generator set and a production method. Background Art
[0002] Pumped-storage power stations are the green, low-carbon, clean and flexible power sources in the power system with the most mature technology, the best economy and the best conditions for large-scale development. They work well with wind power, solar power generation, nuclear power and thermal power.
[0003] Magnetic pole steel is used for the rotor magnetic pole part of the pumped storage generator structure. It is the main component of the hydro-turbine generator to generate the magnetic field. It is a rotating component and requires good electromagnetic and mechanical properties. The thickness is generally ≤2.0mm. As the rated speed of the unit increases, the strength requirements of the required magnetic pole steel plate also increase. Therefore, for the pumped storage hydro-turbine generator unit with a rated speed of 600r / min, the demand for extremely thin magnetic pole steel with a yield strength of ≥900MPa and a thickness of ≤2.0mm is proposed.
[0004] After searching:
[0005] The document with Chinese patent application number CN201210165348.7 discloses "A method for manufacturing high magnetic induction and low cost 250MPa cold-rolled magnetic pole steel", whose process includes: heating the slab to 1200-1260℃ and keeping it warm; hot rolling: the final rolling temperature is 850-900℃, the coiling temperature is 550-630℃, and the cooling method is jet water cooling; cooling to 60-80℃ for pickling, and the cooling method is air cooling; cold rolling: the cold rolling reduction rate is 50-75%; continuous annealing: the soaking section temperature is 720-780℃, and the soaking time is 60-200s; flattening is performed with a flattening elongation of 0.8-1.4%, and a 250MPa cold-rolled magnetic pole steel is produced. However, the yield strength of the produced magnetic pole steel is only 250MPa.
[0006] The document with Chinese patent application number CN200910049782.7 discloses "A method for manufacturing 500MPa grade cold-rolled magnetic pole steel", and the weight percentages of the main chemical components of the slab are: C: 0.07-0.10%, Si: 0.18-0.31%, Mn: 1.00-1.50%, P: ≤0.02%, S: ≤0.007%, O≤0.004%, N≤0.004%, Nb: 0.046-0.060%, Ti: ≤0.003%, V: 0.050-0.070%, and the remainder is Fe and unavoidable impurities. The process is as follows: (1) heating the slab to 1200-1260°C, rolling the slab into a thin steel plate, the final rolling temperature is 830-890°C, cooling to 550-600°C by laminar cooling for coiling; (2) air cooling and pickling; (3) cold rolling; (4) continuous annealing: the temperature of the annealing furnace soaking section is controlled at 740-760°C, the speed of the annealing process section is controlled at 120-125 m / min, and the soaking section time is controlled at 230-239s; (5) flattening. However, the yield strength of the product can only reach 570MPa.
[0007] The document with Chinese patent application number ZL202110575161.3 discloses "Magnetic yoke steel with excellent fatigue resistance and tensile strength ≥850MPa", whose chemical composition and weight percentage are: C: 0.03-0.07%, Si: ≤0.15%, Mn: 0.5-1.0%, P: ≤0.015%, S: ≤0.002%, Nb: 0.075-0.095%, V: 0.015-0.025%, Mo: 0.20-0.30%, Als: 0.02-0.10%, N: ≤0.010%, and the rest is Fe and unavoidable impurities. Its yield strength is ≥800MPa, but there are also precious metals such as Mo and Nb, and the alloy cost is high. Summary of the invention
[0008] The present invention aims to overcome the shortcomings of the prior art and provide a magnetic field having a yield strength of ≥900MPa, an elongation of A ≥12%, and a magnetic field performance of B 50 900MPa grade magnetic pole steel for pumped storage hydroelectric units with a diameter of ≥1.6T and a product thickness of ≤2.0mm and a production method thereof.
[0009] Measures to achieve the above objectives:
[0010] A 900MPa grade magnetic pole steel for a pumped storage hydroelectric generator set, the components and weight percentage contents of which are: C: 0.25-0.30%, Si: 0.10-0.20%, Mn: 1.1-1.5%, Cr: 0.3-0.4%, Ti: 0.2-0.3%, B: 0.0025-0.0030%, P: ≤0.015%, S: ≤0.010%, Als: 0.02-0.10%, and the rest are Fe and unavoidable inclusions.
[0011] Preferably, the weight percentage of Cr is 0.33-0.37%.
[0012] Preferably, the weight percentage of Ti is 0.20-0.25%.
[0013] A method for producing 900MPa grade magnetic pole steel for a pumped storage hydroelectric generator set, comprising the following steps:
[0014] 1) After conventional smelting, the billet is cast into a billet, during which the billet thickness is controlled to be 60-85 mm;
[0015] 2) Heat the ingot, control the soaking temperature at 1150-1200°C, and control the soaking time to be no less than 30 minutes;
[0016] 3) Use 7 passes of hot rolling to the product thickness: control the starting rolling temperature to be no less than 1050°C, and the final rolling temperature to be between 850 and 900°C;
[0017] 4) laminar cooling with a cooling rate of 70-90°C / s to the coiling temperature;
[0018] 5) Coil the steel sheet and control the coiling temperature at 300-400°C.
[0019] 6) Annealing, controlling the annealing heating temperature to 550-600°C and the holding time to 3-6h;
[0020] 7) Perform straightening.
[0021] Preferably, the soaking temperature of the casting is between 1157°C and 1192°C.
[0022] Preferably, the starting rolling temperature is not less than 1058°C, and the final rolling temperature is between 868°C and 892°C.
[0023] Preferably, the coiling temperature is between 340 and 390°C.
[0024] Functions and mechanisms of each element and main process in the present invention
[0025] The carbon (C) content of the present invention is 0.25% to 0.30%, and carbon is the most economical strengthening element. However, if the carbon content is between 0.07% and 0.15%, the molten steel will undergo peritectic reaction during the casting process, increasing the risk of continuous casting leakage, and too high a carbon content will reduce the magnetic induction performance. Therefore, limiting the carbon content to 0.25% to 0.30% can not only improve the strength of the steel, but also ensure the magnetic induction performance of the steel, while greatly reducing the addition of alloy elements and reducing costs.
[0026] The manganese (Mn) content of the present invention is 1.1% to 1.5%. Manganese can reduce the phase transition temperature of austenite to ferrite, expand the hot working temperature range, and is conducive to refining the ferrite grain size and improving the yield strength of steel.
[0027] The chromium (Cr) content of the present invention is 0.3% to 0.4%: chromium is a carbide-forming element, has a strong affinity with carbon, and can hinder the diffusion of carbon atoms. Cr is beneficial to refine ferrite grains and improve the strength of steel plates, but too high a content is detrimental to magnetic properties. In the present invention, the chromium content is controlled at 0.3% to 0.4%, preferably: the weight percentage content of Cr is 0.30% to 0.35%.
[0028] The titanium (Ti) content of the present invention is 0.2% to 0.3%. Ti is a strong carbide and nitride forming element. The carbon and nitride particles formed can prevent the austenite grains from growing during the reheating of steel and the rough rolling in the high-temperature austenite zone, play a role in refining the grains and improving the toughness of the steel. The fine dispersed TiC precipitated in the coiling stage can have a significant precipitation strengthening effect, thereby effectively improving the strength of the steel plate. The present invention selects a Ti content of 0.2% to 0.3%, preferably: the weight percentage content of Ti is 0.20% to 0.25%.
[0029] The silicon (Si) content of the present invention is 0.10% to 0.20%. Si has a solid solution strengthening effect, which can improve the strength of steel and is beneficial to magnetic properties. When the silicon content exceeds a certain range, it will be detrimental to the surface quality. Therefore, the present invention controls the Si content to 0.10% to 0.20%.
[0030] The phosphorus (P) content of the present invention is ≤0.015%, and the sulfur (S) content is ≤0.010%. Phosphorus in steel has adverse effects such as easily causing segregation and reducing magnetic induction performance. Sulfur is easily combined with manganese to form MnS inclusions, which affect the magnetic induction performance and plasticity of steel. Therefore, the present invention should minimize the adverse effects of phosphorus and sulfur elements on steel properties, and control the phosphorus and sulfur contents by means of deep desulfurization pretreatment of molten iron, thereby reducing their adverse effects.
[0031] The boron (B) content of the present invention is 0.0025% to 0.0030%. The main function of B is to act as a surface active element, adsorb on the austenite grain boundary, delay the transformation of austenite to ferrite, thereby refining the final structure and achieving a strengthening effect. In addition, B is extremely cheap and has a significant effect on cost control. However, if the B content is too high, a low melting point eutectic will be formed, which is concentrated on the grain boundary, thereby causing hot brittleness. Therefore, the boron content of the present invention is in the range of 0.0025% to 0.0030%.
[0032] The reason why the present invention controls the soaking temperature of the casting billet at 1150-1200°C is to ensure complete solid solution and sufficient austenitization of the alloy elements, while improving the uniformity of the slab temperature, reducing deformation resistance and rolling load, and facilitating the rolling of thin-gauge yoke steel.
[0033] The reason why the final rolling temperature is controlled at 850-900°C, the cooling rate is 70-90°C / s, and the coiling temperature is 300-400°C is to obtain a bainite structure by a high cooling rate, give full play to the structure strengthening and fine grain strengthening effects, and at the same time, through the annealing temperature of 550-600°C, TiC particles are fully precipitated, give full play to the precipitation strengthening effect, and improve the strength of the steel plate.
[0034] The present invention does not contain precious alloy elements such as Nb and Mo, and has a yield strength of ≥900MPa, an elongation A of ≥12%, and a magnetic induction performance B 50 ≥1.60T, which can fully meet the demand for 900MPa grade magnetic pole steel for pumped storage turbine generator rotors at a rated speed of 600r / min, with a product thickness not exceeding 2mm and a cost that can be reduced by 600 to 900 yuan / ton of steel compared to the existing technology. DETAILED DESCRIPTION
[0035] The present invention is described in detail below:
[0036] Table 1 is a list of component values of various embodiments and comparative examples of the present invention;
[0037] Table 2 is a table of process parameter values and performance tests for various embodiments and comparative examples of the present invention.
[0038] Each embodiment of the present invention is produced according to the following steps:
[0039] 1) After conventional smelting, the billet is cast into a billet, during which the billet thickness is controlled to be 60-85 mm;
[0040] 2) Heat the ingot, control the soaking temperature at 1150-1200°C, and control the soaking time to be no less than 30 minutes;
[0041] 3) Use 7 passes of hot rolling to the product thickness: control the starting rolling temperature to be no less than 1050°C, and the final rolling temperature to be between 850 and 900°C;
[0042] 4) laminar cooling with a cooling rate of 70-90°C / s to the coiling temperature;
[0043] 5) Coil the steel sheet and control the coiling temperature at 300-400°C.
[0044] 6) Annealing, controlling the annealing heating temperature to 550-600°C and the holding time to 3-6h;
[0045] 7) Perform straightening.
[0046] Table 1 Chemical composition list of various embodiments and comparative examples of the present invention (wt%)
[0047]
[0048] Table 2 List of main process parameters of various embodiments of the present invention and comparative examples
[0049]
[0050]
[0051] Table 3 List of mechanical properties test results of various embodiments of the present invention and comparative examples
[0052]
[0053] It can be seen from Table 3 that embodiments 1 to 8 meet the requirements of yield strength ≥ 900 MPa, elongation A ≥ 12%, and magnetic induction performance B 50 Under the requirement of ≥1.60T, the thickness of hot-rolled plate is ≤2.0mm, which fully meets the market demand.
[0054] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.
Claims
1. A 900MPa grade magnetic pole steel for a pumped storage hydroelectric unit, wherein the components and weight percentage contents are: C: 0.25-0.30%, Si: 0.10-0.20%, Mn: 1.1-1.5%, Cr: 0.3-0.4%, Ti: 0.2-0.3%, B: 0.0025~0.0030%, P: ≤0.015%, S: ≤0.010%, Als: 0.02~0.10%, the rest is Fe and unavoidable inclusions.
2. The 900MPa grade magnetic pole steel for a pumped storage hydroelectric generator set as claimed in claim 1, Features: The weight percentage of Cr is 0.33-0.37%.
3. The 900MPa grade magnetic pole steel for a pumped storage hydroelectric generator set as claimed in claim 1, Features: The weight percentage content of Ti is 0.20-0.25%.
4. A method for producing a 900MPa grade magnetic pole steel for a pumped storage hydroelectric generator set as claimed in claim 1, comprising the following steps: 1) After conventional smelting, the billet is cast into a billet, during which the billet thickness is controlled to be 60-85 mm; 2) Heat the ingot, control the soaking temperature at 1150-1200°C, and control the soaking time to be no less than 30 minutes; 3) Use 7 passes of hot rolling to the product thickness: control the starting rolling temperature to be no less than 1050°C, and the final rolling temperature to be between 850 and 900°C; 4) laminar cooling with a cooling rate of 70-90°C / s to the coiling temperature; 5) Coil the steel sheet and control the coiling temperature at 300-400°C. 6) Annealing, controlling the annealing heating temperature to 550-600°C and the holding time to 3-6h; 7) Perform straightening.
5. The method for producing a 900MPa grade magnetic pole steel for a pumped storage hydroelectric generator set as claimed in claim 4, Features: The uniform heating temperature of the ingot is between 1157 and 1192°C.
6. The method for producing a 900MPa grade magnetic pole steel for a pumped storage hydroelectric generator set as claimed in claim 4, Features: The starting rolling temperature is not lower than 1058°C, and the final rolling temperature is between 868 and 892°C.
7. The method for producing a 900MPa grade magnetic pole steel for a pumped storage hydroelectric generator set as claimed in claim 4, Features: The coiling temperature is between 340 and 390°C.
Citation Information
Patent Citations
Manufacturing method of 500Mpa-grade cold-rolled magnetic steel
CN101871076A
Manufacturing method for high-magnetic induction low-cost 250 MPa cold-rolled magnetic pole steel
CN102650016A
Magnet yoke steel with tensile strength larger than or equal to 850 MPa and excellent anti-fatigue performance and production method
CN113373373A
Hot rolled steel in C-Mn-Ti series with high intensity magnetic induction performance
CN101003879A
Hot-rolled pole sheet steel and manufacturing method thereof
CN105624556A