Method for improving interlaminar shear performance of carbon fiber reinforced aluminum matrix composite

By growing silicon carbide nanowires in situ in carbon fiber reinforced aluminum-based composite materials and improving interface bonding through pressure impregnation, the problems of poor interlayer bonding force and insufficient shear performance of the material are solved, and the mechanical properties are significantly improved and Reduced production costs.

CN118910519APending Publication Date: 2024-11-08HARBIN INST OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410990164.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The carbon fiber reinforced aluminum-based composite has anisotropy and poor interlayer bonding force, which is prone to cracking and delamination, resulting in insufficient shear performance.

Method used

By heating high-purity silicon powder and carbon fibers in a vacuum air atmosphere furnace, the silicon carbide nanowires are grown in situ in carbon fibers, the interlayer bonding force of the material is enhanced, and the interface bonding between the matrix and the reinforcement is improved through the pressure immersion method.

Benefits of technology

The interlayer shear strength of carbon fiber reinforced aluminum matrix composite materials has been significantly improved, and the problem of poor interlayer bonding force is solved. The nanowire structure of the reinforcement body is controllable, the production cost is low, the environment is friendly, and the mechanical properties are greatly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910519A_ABST
    Figure CN118910519A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving interlaminar shear performance of a carbon fiber reinforced aluminum-based composite material, and relates to the field of preparation methods of high-strength light-weight structural composite materials. The technical problems that an existing carbon fiber reinforced aluminum matrix composite is anisotropic, poor in interlayer binding force and prone to cracking and layering are solved. The method comprises the following steps: 1, weighing; 2, pretreating the carbon fibers; 3, preparing a reinforcing body; 4, molding the composite material; and 5, heat treatment. The method is simple, the preparation period is short, the high-purity SiC nanowires can grow on the carbon fibers in situ, and the reaction is controllable. The method can be applied to the preparation process of the carbon fiber reinforced aluminum-based composite material, the interlaminar shear strength of the carbon fiber reinforced aluminum-based composite material is improved, and the problems that the interlaminar bonding force is poor and layering is prone to occurring are solved. The method is used for improving the interlaminar shear performance of the carbon fiber reinforced aluminum matrix composite.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation methods of high-strength lightweight structural composite materials. Background Art

[0002] Carbon fiber reinforced aluminum matrix composites have the advantages of high specific strength and high specific modulus, and have broad application prospects in the fields of aerospace, military industry and automobile. Silicon carbide has excellent properties such as high strength, high hardness, small thermal expansion coefficient, strong oxidation resistance and good wear resistance, and is widely used as a reinforcement in metal matrix composites. However, silicon carbide particles are brittle and have poor toughness like ceramic materials. Silicon carbide nanowires have been widely studied due to their unique one-dimensional structure, high aspect ratio and large specific surface area. Their surface effects and quantum effects will significantly improve their performance. While retaining the various excellent properties of the original silicon carbide, the mechanical properties such as strength and toughness are much higher than those of silicon carbide particles or silicon carbide whiskers.

[0003] Carbon fiber reinforced aluminum matrix composites are anisotropic due to the different texture directions of carbon fiber. Although the fiber-dominated in-plane performance is excellent, it can only rely on the matrix to play the role of bonding and load transfer in the interlayer area. The fracture toughness is poor and it is easy to crack and delaminate, which becomes the weak link of the composite material performance. Therefore, improving the interlayer bonding ability of carbon fiber reinforced aluminum matrix composites is an important part of expanding its application range. Summary of the invention

[0004] In order to solve the technical problems of anisotropy, poor interlayer bonding and easy cracking and delamination in existing carbon fiber reinforced aluminum-based composite materials, the present invention provides a method for improving the interlayer shear performance of carbon fiber reinforced aluminum-based composite materials.

[0005] A method for improving the interlaminar shear performance of a carbon fiber reinforced aluminum-based composite material, specifically comprising the following steps:

[0006] 1. Weighing materials: Weigh high-purity silicon powder and carbon fiber as raw materials, and use hydrofluoric acid solution to wash away the oxide layer on the surface of the high-purity silicon powder;

[0007] 2. Carbon fiber pretreatment: put the carbon fiber weighed in step 1 into an ultrasonic cleaning machine filled with deionized water, ultrasonically treat for 5 to 15 minutes, clean it with anhydrous ethanol, and dry it in a drying oven at 60 to 80°C;

[0008] 3. Preparation of reinforcement: Spread the high-purity silicon powder treated in step 1 into a crucible, place a pad in the crucible, place the carbon fiber obtained in step 2 on the pad, and then install a mold, seal the crucible and put it into a vacuum atmosphere furnace; after the vacuum atmosphere furnace is evacuated, fill it with a protective atmosphere, heat it to 1000-2000°C, keep it warm for 0.5-6h, and then cool it with the furnace to obtain a reinforcement of carbon fiber in-situ grown silicon carbide nanowires;

[0009] 4. Composite material molding: stacking the reinforcement obtained in step 3, loading it into a mold and preheating it, then pouring the molten aluminum alloy into the mold and performing pressure infiltration to obtain an aluminum-based composite material reinforced with in-situ grown carbon fiber silicon carbide nanowires;

[0010] 5. Heat treatment: heat the carbon fiber in-situ grown silicon carbide nanowire reinforced aluminum matrix composite material obtained in step 4 to 300-600° C., keep it warm for 0.5-2 hours, and cool it to room temperature in the furnace.

[0011] The present invention utilizes the thermodynamic principle to realize in-situ growth of silicon carbide nanowires on carbon fibers by thermal evaporation. The preparation method of the reinforcement follows the gas-solid (VS) mechanism, which is more likely to occur at a certain temperature according to thermodynamic calculations. At a certain temperature, a small amount of oxygen in the furnace reacts with the evaporated silicon powder to form SiO gas, and at the same time reacts with C on the carbon fibers to generate CO. The SiO gas reacts with CO and C to generate SiC.

[0012] Beneficial effects of the present invention:

[0013] The method of the invention is simple, has a short preparation cycle, and the carbon fiber can grow high-purity SiC nanowires in situ, and the reaction is controllable. The method can be applied to the preparation process of carbon fiber reinforced aluminum-based composite materials, improve the interlaminar shear strength of carbon fiber reinforced aluminum-based composite materials, and solve the problems of poor interlaminar bonding and easy delamination.

[0014] Compared with the traditional method, the silicon carbide nanowires prepared by the present invention have the advantages of being less susceptible to pollution, better dispersibility, low production cost, simple process, environmental friendliness, and controllable nanowire structure, and have broad application prospects;

[0015] The present invention controls the volume fraction of the reinforcement by controlling the reaction degree of silicon carbide nanowires by controlling the holding time and the heating temperature, thereby controlling the content of the nanowires; pressurizing the reinforcement of silicon carbide grown in situ on carbon fiber, and using metallic aluminum liquid to improve the interface bonding between the reinforcement and the matrix.

[0016] The silicon carbide nanowires introduced into the composite material of the present invention are relatively small in size and can play a role of dispersion strengthening, hinder the movement of dislocations, and store dislocations to achieve a satisfactory material strengthening effect. The hardening area caused by the silicon carbide nanowires is small and dispersed, which can reduce the stress concentration of the composite material. The SiC nanowires on the carbon fiber construct a nano-scale mechanical interlocking between the carbon fiber and the Al matrix, which can effectively inhibit crack propagation, greatly improve the load transfer efficiency of the interface, and improve the shear resistance.

[0017] The composite material of the present invention uses an aluminum alloy as a matrix and carbon fiber in-situ grown silicon carbide nanowires as a reinforcement. The matrix and the reinforcement are composited by a pressure infiltration method. The obtained carbon fiber reinforced aluminum-based composite material has greatly improved shear resistance compared with the carbon fiber reinforced aluminum-based composite material without the addition of silicon carbide nanowires. The interlaminar shear performance of the composite material of the present invention is improved by up to 100%. The mechanical properties of the carbon fiber in-situ grown silicon carbide nanowire reinforced aluminum-based composite material prepared by the method of the present invention are greatly improved.

[0018] The method of the invention is used to improve the interlaminar shearing performance of carbon fiber reinforced aluminum-based composite materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a scanning electron microscope photograph of the in-situ grown silicon carbide nanowires on carbon fiber obtained in step 3 of the embodiment;

[0020] Figure 2 The XRD spectrum of the in-situ grown silicon carbide nanowires on carbon fiber obtained in step 3 of the embodiment;

[0021] Figure 3 It is the interlaminar shear displacement curve diagram of the composite materials prepared in the embodiment and the comparative example. DETAILED DESCRIPTION

[0022] Specific implementation method 1: This implementation method is a method for improving the interlaminar shear performance of carbon fiber reinforced aluminum-based composite materials, which is specifically carried out in the following steps:

[0023] 1. Weighing materials: Weigh high-purity silicon powder and carbon fiber as raw materials, and use hydrofluoric acid solution to wash away the oxide layer on the surface of the high-purity silicon powder;

[0024] 2. Carbon fiber pretreatment: put the carbon fiber weighed in step 1 into an ultrasonic cleaning machine filled with deionized water, ultrasonically treat for 5 to 15 minutes, clean it with anhydrous ethanol, and dry it in a drying oven at 60 to 80°C;

[0025] 3. Preparation of reinforcement: Spread the high-purity silicon powder treated in step 1 into a crucible, place a pad in the crucible, place the carbon fiber obtained in step 2 on the pad, and then install a mold, seal the crucible and put it into a vacuum atmosphere furnace; after the vacuum atmosphere furnace is evacuated, fill it with a protective atmosphere, heat it to 1000-2000°C, keep it warm for 0.5-6h, and then cool it with the furnace to obtain a reinforcement of carbon fiber in-situ grown silicon carbide nanowires;

[0026] 4. Composite material molding: stacking the reinforcement obtained in step 3, loading it into a mold and preheating it, then pouring the molten aluminum alloy into the mold and performing pressure infiltration to obtain an aluminum-based composite material reinforced with in-situ grown carbon fiber silicon carbide nanowires;

[0027] 5. Heat treatment: heat the carbon fiber in-situ grown silicon carbide nanowire reinforced aluminum matrix composite material obtained in step 4 to 300-600° C., keep it warm for 0.5-2 hours, and cool it to room temperature in the furnace.

[0028] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the carbon fiber in step 1 is M40J carbon fiber or T700 carbon fiber. The rest is the same as specific implementation method 1.

[0029] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that: the purity of the high-purity silicon powder in step 1 is 99% or above. The rest is the same as specific implementation method 1 or 2.

[0030] Specific implementation method 4: This implementation method is different from one of the specific implementation methods 1 to 3 in that: the vacuum pumping in step 3 is pumped to 10 -2 ~10 -1 Pa. The rest is the same as that of the first to third embodiments.

[0031] Specific implementation method 5: This implementation method is different from specific implementation methods 1 to 4 in that the protective atmosphere in step 3 is argon or argon gas, and the gas purity is 99% or above. The rest is the same as specific implementation methods 1 to 4.

[0032] Specific embodiment 6: This embodiment is different from specific embodiments 1 to 5 in that the heating rate when heating to 1000-2000° C. in step 3 is 2-10° C. / min. The rest is the same as specific embodiments 1 to 5.

[0033] Specific implementation method 7: This implementation method is different from specific implementation methods 1 to 6 in that: Step 3 is to raise the temperature to 1200° C. and keep the temperature for 1 hour. The rest is the same as specific implementation methods 1 to 6.

[0034] Specific implementation eight: This implementation differs from specific implementations one to seven in that: step three is to raise the temperature to 1200° C. and keep the temperature for 2 hours. The rest is the same as specific implementations one to seven.

[0035] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that: in step 3, the temperature is raised to 1300° C. and kept at this temperature for 0.5 h. The rest is the same as specific embodiments 1 to 8.

[0036] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that: step 3 is to raise the temperature to 1300° C. and keep the temperature for 2 hours. The rest is the same as specific embodiments 1 to 9.

[0037] Specific implementation eleven: This implementation is different from specific implementations one to ten in that: step three is to raise the temperature to 1400° C. and keep the temperature for 1 hour. The rest is the same as specific implementations one to ten.

[0038] Specific embodiment 12: This embodiment differs from specific embodiments 1 to 11 in that: step 3 raises the temperature to 1400° C. and keeps the temperature for 4 hours. The rest is the same as specific embodiments 1 to 11.

[0039] Specific implementation 13: This implementation is different from specific implementations 1 to 12 in that: step 3 is heating to 1500-1600° C. and keeping the temperature for 1 hour. The rest is the same as specific implementations 1 to 12.

[0040] Specific embodiment 14: This embodiment differs from specific embodiments 1 to 13 in that the aluminum alloy in step 4 is a 5xxx aluminum alloy, a 6xxx aluminum alloy or a 7xxx aluminum alloy. The rest is the same as specific embodiments 1 to 13.

[0041] Specific embodiment 15: This embodiment differs from specific embodiments 1 to 14 in that: in step 4, the preheating temperature is controlled to be 500-550° C., and the preheating time is 1-2 hours. The rest is the same as specific embodiments 1 to 14.

[0042] Specific embodiment 16: This embodiment differs from specific embodiments 1 to 15 in that the infiltration pressure in step 4 is controlled to be 25-50 MPa. The rest is the same as specific embodiments 1 to 15.

[0043] Specific embodiment 17: This embodiment differs from specific embodiments 1 to 16 in that the heating rate in step 5 is 2 to 10°C / min. The rest is the same as specific embodiments 1 to 16.

[0044] The content of the present invention is not limited to the content of the above-mentioned embodiments. The combination of one or several specific embodiments can also achieve the purpose of the invention.

[0045] Example:

[0046] A method for improving the interlaminar shear performance of a carbon fiber reinforced aluminum-based composite material, specifically comprising the following steps:

[0047] 1. Weighing materials: Weigh 99.99% pure silicon powder and M40J carbon fiber as raw materials, and use hydrofluoric acid solution to wash away the surface oxide layer of high-purity silicon powder;

[0048] 2. Carbon fiber pretreatment: put the M40J carbon fiber weighed in step 1 into an ultrasonic cleaning machine filled with deionized water, ultrasonically treat for 15 minutes, clean it with anhydrous ethanol, and put it into a drying oven at 70°C for drying;

[0049] 3. Preparation of reinforcement: Spread the high-purity silicon powder processed in step 1 into a crucible, place a pad in the crucible, and place the M40J carbon fiber cut into a suitable size obtained in step 2 on the pad, so that there is a gap between the powder and the carbon fiber, then install the mold, seal the crucible and put it into a vacuum atmosphere furnace; wait until the vacuum atmosphere furnace is evacuated to 10 -2 After the temperature reaches 1000 Pa, argon gas with a purity of 99.99% is filled in, and the temperature is raised to 1400°C at a controlled heating rate of 10°C / min, kept at that temperature for 1 hour, and then cooled with the furnace to obtain a reinforcement of carbon fiber in-situ grown silicon carbide nanowires;

[0050] 4. Composite material molding: the reinforcement obtained in step 3 is stacked and loaded into a mold and preheated at a temperature of 500°C for 1 hour, and then the molten 5056 aluminum alloy heated to 880°C and melted at a constant temperature is poured into the mold for pressure infiltration, and the infiltration pressure is controlled to be 30 MPa to obtain an aluminum-based composite material reinforced with in-situ growth of carbon fiber and silicon carbide nanowires;

[0051] 5. Heat treatment: heat the carbon fiber in-situ grown silicon carbide nanowire reinforced aluminum matrix composite material obtained in step 4 to 300°C, control the heating rate to 10°C / min, keep warm for 1 hour, and cool the furnace to room temperature.

[0052] Comparative Example:

[0053] This comparative example is a method for improving the mechanical properties of a carbon fiber reinforced aluminum-based composite material, which is carried out according to the following steps:

[0054] 1. Weighing materials: weigh 5056 aluminum alloy and M40J carbon fiber;

[0055] 2. Melting: heating the 5056 aluminum alloy weighed in step 1 to 880° C. and melting at a constant temperature for 30 minutes to obtain an aluminum alloy melt;

[0056] 3. Composite material molding: After stacking the carbon fiber layers, load them into a mold and preheat them. The preheating temperature is 500°C and the preheating time is 1 hour. Pour the aluminum alloy melt obtained in step 2 into the mold and perform pressure infiltration. Control the infiltration pressure to be 30MPa to obtain a carbon fiber reinforced aluminum-based composite material. During the pressure infiltration process, pour the aluminum alloy melt obtained in step 2 into the mold and then load a graphite indenter. Apply pressure through a press to infiltrate the alloy melt into the carbon fiber preform to obtain a carbon fiber reinforced aluminum-based composite material.

[0057] 4. Heat treatment: Heat the carbon fiber reinforced aluminum-based composite material obtained in step 3 to 300°C at a heating rate of 10°C / min, keep warm for 1 hour, and cool the furnace to room temperature to obtain the Cf / 5056Al-based composite material.

[0058] Figure 1 This is a scanning electron microscope photograph of the in-situ grown silicon carbide nanowires on carbon fiber obtained in step 3 of the embodiment. It can be seen from the figure that the SiC nanowires have uniform morphology, a length of about several hundred nanometers, and an average diameter of about 120 nm.

[0059] Figure 2 This is the XRD spectrum of the in-situ grown silicon carbide nanowires on carbon fiber obtained in step 3 of Example 1. It can be seen from the figure that there are no other impurity peaks except the carbon fiber diffraction peak, indicating that the obtained nanowires have the characteristics of high purity.

[0060] Figure 3 It is the interlaminar shear displacement curve diagram of the composite materials prepared in the embodiment and the comparative example.

[0061] pass Figure 3 It can be seen that the reinforcement of the carbon fiber in-situ grown silicon carbide nanowire reinforced aluminum-based composite material prepared in the embodiment was prepared at 1400°C for 1 hour. From the interlaminar shear displacement curve of the composite material, it can be concluded that the interlaminar shear strength of the Cf / Al composite material without silicon carbide nanowires reached 67.07MPa, and the interlaminar shear strength of the Cf-SiC NWs / Al composite material prepared by the present invention reached 90.35MPa. Compared with the comparative example, the interlaminar shear strength of the composite material of the embodiment is increased by 32.6%.

Claims

1. A method for improving the interlaminar shear performance of carbon fiber reinforced aluminum matrix composite materials, characterized in that The method is specifically carried out in the following steps:

1. Weighing materials: Weigh high-purity silicon powder and carbon fiber as raw materials, and use hydrofluoric acid solution to wash away the oxide layer on the surface of the high-purity silicon powder; 2. Carbon fiber pretreatment: put the carbon fiber weighed in step 1 into an ultrasonic cleaning machine filled with deionized water, ultrasonically treat for 5 to 15 minutes, clean it with anhydrous ethanol, and dry it in a drying oven at 60 to 80°C; 3. Preparation of reinforcement: Spread the high-purity silicon powder treated in step 1 into a crucible, place a pad in the crucible, place the carbon fiber obtained in step 2 on the pad, and then install a mold, seal the crucible and put it into a vacuum atmosphere furnace; after the vacuum atmosphere furnace is evacuated, fill it with a protective atmosphere, heat it to 1000-2000°C, keep it warm for 0.5-6h, and then cool it with the furnace to obtain a reinforcement of carbon fiber in-situ grown silicon carbide nanowires; 4. Composite material molding: stacking the reinforcement obtained in step 3, loading it into a mold and preheating it, then pouring the molten aluminum alloy into the mold and performing pressure infiltration to obtain an aluminum-based composite material reinforced with in-situ grown carbon fiber silicon carbide nanowires; 5. Heat treatment: heat the carbon fiber in-situ grown silicon carbide nanowire reinforced aluminum matrix composite material obtained in step 4 to 300-600° C., keep it warm for 0.5-2 hours, and cool it to room temperature in the furnace.

2. The method for improving the interlaminar shear performance of carbon fiber reinforced aluminum-based composite materials according to claim 1, wherein the carbon fiber described in step 1 is M40J carbon fiber or T700 carbon fiber.

3. The method for improving the interlaminar shear performance of carbon fiber reinforced aluminum matrix composite materials according to claim 1, characterized in that The purity of the high-purity silicon powder in step 1 is 99% or above.

4. The method for improving the interlaminar shear performance of carbon fiber reinforced aluminum matrix composite materials according to claim 1, characterized in that Step 3: Vacuum to 10 -2 ~10 -1 Pa.

5. The method for improving the interlaminar shear performance of carbon fiber reinforced aluminum matrix composite materials according to claim 1, characterized in that The protective atmosphere in step 3 is argon or argon, and the gas purity is 99% or above.

6. The method for improving the interlaminar shear performance of carbon fiber reinforced aluminum matrix composite materials according to claim 1, characterized in that The heating rate when heating to 1000-2000° C. in step 3 is 2-10° C. / min.

7. The method for improving the interlaminar shear performance of carbon fiber reinforced aluminum matrix composite materials according to claim 1, characterized in that The aluminum alloy described in step 4 is a 5xxx series aluminum alloy, a 6xxx series aluminum alloy or a 7xxx series aluminum alloy.

8. The method for improving the interlaminar shear performance of carbon fiber reinforced aluminum matrix composite materials according to claim 1, characterized in that In step 4, the preheating temperature is controlled to be 500°C and the preheating time is 1h.

9. The method for improving the interlaminar shear performance of carbon fiber reinforced aluminum matrix composite materials according to claim 1, characterized in that In step 4, the impregnation pressure is controlled to be 25-50 MPa during pressure impregnation.

10. The method for improving the interlaminar shear performance of carbon fiber reinforced aluminum matrix composite materials according to claim 1, characterized in that The heating rate in step 5 is 2-10°C / min.

Citation Information

Patent Citations

  • Manufacturing method of carbon fiber reinforced aluminum composite material with high interlayer strength

    CN110484839A

  • Method for improving mechanical property of carbon fiber-reinforced aluminum matrix composite

    CN112981282A

  • Method for preparing Cf-SiCNWs / aluminum-based composite material with high interlaminar shear strength by combining tape casting and pressure infiltration methods

    CN117265434A

  • Preparation method of carbon fiber reinforced aluminum-based composite material with high strength and interlaminar shear strength

    CN118326210A

  • Metal-matrix carbon-fiber-reinforced composite material and its manufacturing method

    JP2002294359A