Preparation method of medical Ti-Sn-Mo alloy coating on pure titanium surface
By using laser cladding technology to prepare Ti-Sn-Mo alloy coating on pure titanium surface, the stress shielding problem caused by the difference in elastic modulus of titanium alloy and human bones is solved, the existence of toxic elements is reduced, and biocompatibility is improved and wear resistance, achieving better metallurgical integration and microstructure meticulousness.
Patent Information
- Application Number
- CN202410999500.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The "stress shielding" phenomenon caused by the large difference between the elastic modulus and the human bones during human implantation has caused bone degeneration and loss of function. The Al and V elements in the common medical titanium alloy TC4 are toxic to cells.
Ti-10Sn-xMo(x=5, 10, 15, 20, wt%) alloy coating was prepared on pure titanium surface by laser cladding technology, and the mixture of spherical Ti powder, spherical Sn powder and spherical Mo powder. Cladding, forming a Ti-Sn-Mo alloy coating with low elastic modulus and non-toxicity, improving biocompatibility and wear resistance.
Reduces material wear and host reaction, reduces stress shielding, improves the wear resistance and hardness of the coating, avoids elements that are toxic to cells, enhances biocompatibility, and reduces porosity and inclusions through metallurgical combination Things.
Smart Images

Figure CN118910609A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium alloy industry, in particular to a method for preparing a medical Ti-Sn-Mo alloy coating on the surface of pure titanium. Background Art
[0002] The application of titanium alloys in human implant materials is mainly concentrated in relatively active or frequently rubbed areas; however, prolonged friction can cause material wear, thereby triggering a series of host reactions such as inflammation, allergies, and even cancer; in addition, due to the large difference in elastic modulus between titanium alloys and human bones, "stress shielding" may occur, leading to bone degeneration and loss of function; therefore, in the medical field, it is of great significance to find medical titanium alloys with good mechanical properties and low elastic modulus, which can improve the current medical level.
[0003] For example, the patent with publication number CN111172532A discloses a method for preparing a medium-entropy alloy coating on the surface of a pure titanium plate, including workpiece pretreatment; coating pretreatment: using an organic solvent to mix metal powders of components Fe, Ni or Cr, Ni in an equimolar ratio into a paste, coating the metal powder powders on the surface of the pretreated workpiece, and then drying the workpiece coated with the metal powder coating; performing pulsed laser surface cladding treatment on the workpiece after the coating pretreatment; obtaining a workpiece having a FeNiTix or CrNiTix medium-entropy alloy coating on the surface, wherein x=1-2; the method for preparing a medium-entropy alloy coating on the surface of a pure titanium plate provided by the invention conforms to the performance change law of the pure titanium plate, can effectively improve the mechanical properties of the pure titanium plate such as microhardness and strength, so that the hardened layer depth reaches 400-500μm, and the structure is finer and more uniform, and the method process is easy to operate, the equipment is simple, economical and practical, the technology is reliable, the efficiency is high, the quality is stable, and better economic benefits can be achieved.
[0004] However, traditional titanium alloys will face some problems in long-term use, such as inflammation, allergies, and even cancer caused by wear; the "stress shielding" phenomenon caused by the large difference in elastic modulus from human bones, which leads to bone degeneration and loss of function; the most common medical titanium alloy on the market is TC4, but its elastic modulus exceeds 100GPa, which is much higher than human bones, and the Al and V elements therein are toxic to cells; therefore, the development of non-toxic and low elastic modulus medical titanium alloys has always been a research focus. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides a method for preparing a medical Ti-Sn-Mo alloy coating on a pure titanium surface, which solves the "stress shielding" phenomenon caused by the large difference in elastic modulus between the prior art and human bones, thereby causing bone degeneration and loss of function; the most common medical titanium alloy on the market is TC4, but its elastic modulus exceeds 100GPa, which is much higher than that of human bones, and the Al and V elements therein are toxic to cells.
[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0007] The present invention provides a method for preparing a medical Ti-Sn-Mo alloy coating on a pure titanium surface, wherein a Ti-10Sn-xMo (x=5, 10, 15, 20, wt%) alloy coating is clad on the pure titanium surface by laser cladding technology, and the specific steps include:
[0008] Step 1. Material preparation: spherical Ti powder, quasi-spherical Sn powder and quasi-spherical Mo powder are mixed in the proportion of Ti-10Sn-xMo (x=5, 10, 15, 20, wt%);
[0009] Step 2. Substrate treatment: Use medium-strength TA1 pure titanium sheet as the substrate, and perform grinding, polishing and preheating on the substrate;
[0010] Step 3. Laser cladding: a laser machine with a wavelength of 1080nm is used for cladding. The coaxial powder feeding method is used to control the powder flow rate and coating thickness in real time. High-purity argon is used as the protective gas.
[0011] Step 4. Cooling and testing: Place the alloy coating on the heating furnace and cool it down with the furnace to avoid the coating cracking caused by too large a difference in cooling speed between the substrate and the coating;
[0012] Step 5. Adjust the powder ratio according to the ratio of Ti-10Sn-xMo (x=5, 10, 15, 20, wt%) and repeat steps 1-4.
[0013] The present invention is further configured that in step 1, after the powders are configured in proportion, they are mixed in a vertical planetary ball mill at a rotation speed of 200-300 r / min and a ball milling time of 2-3 h to mix the powders uniformly;
[0014] The present invention is further configured that the cladding layer powders used in the process of cladding the Ti-10Sn-xMo alloy coating on the surface of pure titanium are all single-substance powders, including: spherical Ti powder (purity>99.4%, powder particle size of 70μm to 120μm), quasi-spherical Sn powder (purity>99.6%, powder particle size of 60μm to 90μm) and quasi-spherical molybdenum powder (99.99%, powder particle size of 60μm to 80μm), and the powder also contains other impurities. Through EDS energy spectrum scanning, it is found that the impurities are mainly C, O and Si;
[0015] The present invention is further configured to grind the pure titanium surface with a 4-inch silicon carbide louver blade in the grinding and polishing stage, and wipe off excess grinding chips with ethanol until the metallic luster is revealed, so as to avoid impurities affecting the properties of the cladding layer;
[0016] The present invention is further configured that the preheating temperature in step 2 is 400° C.;
[0017] The present invention is further configured that the laser cladding step of step 3 comprises:
[0018] First, take the preheated substrate out of the heating furnace and place it on the workbench;
[0019] The powder was loaded into the powder feeder, and the laser power was adjusted to 2000w and the speed to 6mm / s;
[0020] At the beginning, the protective Ar gas is turned on, and then the laser is turned on after the powder flows out. The laser beam causes the powder to quickly heat up to a temperature higher than the melting point on the substrate surface;
[0021] The melt forms a liquid pool, which expands on the material surface through surface tension and capillary phenomena, and gradually solidifies to form a uniform and dense cladding layer;
[0022] During this period, you can use goggles to observe the state of the laser molten pool. There are bubbles coming out of it. This is the gas discharged after the powder is melted. A good molten pool state can avoid alloy porosity.
[0023] The present invention is further configured that, in the laser cladding process, the laser power is 2000W and the scanning speed is 6mm / s;
[0024] The present invention is further configured that, in the laser cladding process, Ar is used as the protective gas, the gas flow rate is 10 (L / min), the delivery rate is 1.3 (r / min), the defocus amount is 40 mm, and the overlap rate is 50%.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention adopts a Ti-Sn-Mo alloy coating prepared by laser cladding technology, thereby improving the wear resistance of the coating, reducing material wear and host reaction, and reducing the elastic modulus of the Ti-Sn-Mo alloy coating by introducing the Mo element, making it closer to human bones and reducing stress shielding phenomenon;
[0027] The present invention is different from the traditional TC4 alloy, which contains Al and V elements that are toxic to cells; the present application adopts Ti-Sn-Mo alloy coating, which does not contain toxic elements and improves biocompatibility; and uses laser cladding technology to achieve better metallurgical bonding, reduce porosity and inclusions, and prepare a delicate microstructure through rapid heating and cooling, thereby improving the wear resistance and hardness of the coating;
[0028] The present invention adopts a pure titanium substrate having a thermal expansion coefficient and a melting point close to those of the coating, and performs a preheating treatment, thereby reducing the risk of cracking and having a low cost;
[0029] It solves the "stress shielding" phenomenon caused by the large difference in elastic modulus between the existing technology and human bones, which leads to bone degeneration and loss of function; the most common medical titanium alloy on the market is TC4, but its elastic modulus exceeds 100GPa, which is much higher than human bones, and the Al and V elements therein are toxic to cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The present invention is a flow chart of the preparation method of the medical Ti-Sn-Mo alloy coating on the surface of pure titanium;
[0031] Figure 2 The X-ray diffraction (XRD) diagram of the Ti-10Sn-xMo alloy coating in the preparation process of the medical Ti-Sn-Mo alloy coating on the pure titanium surface of the present invention;
[0032] Figure 3 The wear surface morphology of the Ti-10Sn-xMo alloy coating in the preparation process of the medical Ti-Sn-Mo alloy coating on the pure titanium surface of the present invention;
[0033] Figure 4 The microstructure of the Ti-10Sn-xMo alloy coating of the preparation method of the medical Ti-Sn-Mo alloy coating on the pure titanium surface of the present invention;
[0034] Figure 5 The effect of the Mo content on the friction coefficient and hardness of the Ti-10Sn-xMo alloy coating in the preparation method of the pure titanium surface medical Ti-Sn-Mo alloy coating of the present invention;
[0035] Figure 6The potentiodynamic polarization curve of the Ti-10Sn-xMo alloy coating of the preparation method of the medical Ti-Sn-Mo alloy coating on the pure titanium surface of the present invention;
[0036] Figure 7 The corrosion potential of the Ti-10Sn-xMo alloy coating of the preparation method of the medical Ti-Sn-Mo alloy coating on the pure titanium surface of the present invention changes with time;
[0037] Figure 8 Electrochemical impedance spectroscopy (EIS) of the Ti-10Sn-xMo alloy coating of the preparation method of the medical Ti-Sn-Mo alloy coating on the pure titanium surface of the present invention;
[0038] Fig. 9 The effect of the Mo content on the hardness of the Ti-10Sn-xMo alloy coating in the preparation method of the pure titanium surface medical Ti-Sn-Mo alloy coating of the present invention;
[0039] Fig.10 The invention discloses a method for preparing a medical Ti-Sn-Mo alloy coating on a pure titanium surface and shows changes in the friction coefficient of the Ti-10Sn-xMo alloy coating over time. DETAILED DESCRIPTION
[0040] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0041] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0042] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0043] Example 1
[0044] The present invention provides a method for preparing a medical Ti-Sn-Mo alloy coating on a pure titanium surface, comprising: powder mixing and alloy preparation;
[0045] Powder Mixing:
[0046] The cladding powders used in the present invention are all single-substance powders, including: spherical Ti powder (purity>99.4%, powder particle size of 70μm-120μm), quasi-spherical Sn powder (purity>99.6%, powder particle size of 60μm-90μm) and quasi-spherical molybdenum powder (99.99%, powder particle size of 60μm-80μm), and the powders also contain some impurities. EDS energy spectrum scanning shows that the impurities are mainly C, O and Si, as shown in Table 1;
[0047] When preparing alloys by laser cladding, uneven powder mixing will lead to large differences in the composition of different positions in the prepared alloys. After the single powders are configured in proportion, they are mixed in a vertical planetary ball mill (Changsha Tianchuang XQM-44) at a speed of 200r / min and a ball milling time of 3h to ensure uniform powder mixing.
[0048] Table 1 Chemical composition of impurities in single substance powder and mixed powder (mass fraction, %)
[0049]
[0050] Laser cladding technology is gradually maturing, and cracking of the cladding layer is one of the common problems in the laser cladding process. The main factors affecting it are the thermal expansion coefficient and the bonding strength between the coating and the substrate. In order to prevent the cladding layer from being poorly bonded to the substrate material and easy to crack, the thermal expansion coefficient and melting point of the substrate and the alloy are required to be as close as possible.
[0051] In this application, the base material is a medium-strength TA1 pure titanium plate purchased by Changan Yulian Metal Products Co., Ltd. in Dongguan City, and its size is 100mm×100mm×8mm; although the strength of pure titanium is not enough to meet the requirements of bone implants, it has good biocompatibility and plasticity, and is still widely used in the field of bone plates and fixation screws, and its melting point is similar to that of the titanium alloy cladding layer, avoiding the cracking problem caused by the large difference in melting points; at the same time, pure titanium is cheap, so it is an excellent material for laser cladding to prepare medical titanium alloy substrates; its chemical composition is shown in Table 2, and the elements contained, in addition to Ti, also contain some impurities such as C, N, and O;
[0052] Table 2 Chemical composition of pure titanium (TA1) (mass fraction, %)
[0053]
[0054] Alloy preparation:
[0055] The present invention adopts laser cladding technology to clad Ti-10Sn-5Mo alloy coating on the surface of pure titanium; a commercial laser machine (IPGYLS-10000, IPG Company, USA) with a wavelength of 1080nm and a spot diameter of 4.0mm is used as a laser source to perform laser cladding on a pure Ti plate; a far-infrared microcrystalline electric heating plate (DB-XWJ) is used to preheat the substrate before laser cladding; during the laser cladding experiment, a double-barrel double-control powder feeder (PF2-2LC) is used to feed powder, and the protective gas is high-purity argon (Ar) gas, and the steps include:
[0056] (1) Before cladding, the substrate (pure titanium) was polished and ground with a 4-inch silicon carbide louver blade to make the surface of the pure titanium smooth. Excess grinding debris was wiped off with ethanol to reveal the metallic luster and avoid impurities affecting the properties of the cladding layer.
[0057] (2) After grinding, the substrate is placed in a heating furnace for preheating. The preheating temperature is 400°C. Preheating can avoid most cracks.
[0058] (3) The powder feeding method for cladding is coaxial powder feeding, which can control the flow rate in real time and adjust the coating thickness;
[0059] (4) The laser scanning speed v is 6 mm / s, the protective gas (Ar gas) flow rate is 10 (L / min), the delivery rate is 1.3 (r / min), the defocusing amount is 40 mm, and the overlap rate is 50%; in the experimental stage, the present application changes the laser power (1000w, 1500w, 2000w, 2500w) to prepare the alloy coating. The result shows that the coating quality is the best and the hardness is the highest when the power is 2000w, so the laser power is 2000w and the scanning speed is 6mm / s;
[0060] (5) First, take the preheated substrate out of the heating furnace and place it on a flat workbench. Load the powder into the powder feeder, adjust the laser power (2000w) and speed (6mm / s), start the protective Ar gas at the beginning, and then turn on the laser after the powder flows out. The laser beam causes the powder to quickly heat up to a temperature higher than the melting point on the surface of the substrate, and melts to form a layer of liquid pool. Through surface tension and capillary phenomenon, the liquid pool expands on the surface of the material and gradually solidifies to form a uniform and dense cladding layer. During this period, goggles can be used to observe the state of the laser molten pool. Bubbles are constantly coming out of it. This is the gas discharge after the powder is melted. A good molten pool state can avoid alloy pores. Finally, a 25mm*40mm alloy block coating is prepared.
[0061] (6) Place the alloy coating on a heating furnace and cool it down with the furnace to avoid cracking of the coating due to a large difference in cooling speed between the substrate and the coating.
[0062] Example 2
[0063] The difference from Example 1 is the powder mixing ratio. Laser cladding technology is used to clad the Ti-10Sn-10Mo alloy coating on the surface of pure titanium.
[0064] Example 3
[0065] The difference from Example 1 is the powder mixing ratio. Laser cladding technology is used to clad the Ti-10Sn-15Mo alloy coating on the surface of pure titanium.
[0066] Example 4
[0067] The difference from Example 1 is the powder mixing ratio. Laser cladding technology is used to clad the Ti-10Sn-20Mo alloy coating on the surface of pure titanium.
[0068] Experimental example
[0069] The hardness and friction and wear tests were performed on the prepared alloy coatings. The coating test parameters of Examples 1 to 4 were divided into Experimental Group 1, Experimental Group 2, Experimental Group 3 and Experimental Group 4. The specific test results are shown in Tables 3 and 4.
[0070] Table 3 Average friction coefficient of Ti-Sn-Mo ternary alloy
[0071]
[0072] Table 4 Hardness test of Ti-Sn alloy under different process parameters
[0073]
[0074]
[0075] Combining Table 3 and Table 4 and Figure 2-Figure 10 It can be seen that the friction coefficient of Ti-Sn-Mo alloy shows a trend of decreasing and then increasing with the increase of Mo. The smaller the friction coefficient, the better the wear resistance of the alloy. Among them, the friction coefficients of Ti-10Sn-10Mo and Ti-10Sn-15Mo alloys are relatively small and the difference is not large. The friction coefficients are 0.637 and 0.641 respectively, indicating that they have good wear resistance.
[0076] With the change of Mo content, the microhardness of Ti-Sn-Mo alloy shows a pattern of first increasing and then decreasing; with the increase of Mo element content, the alloy hardness gradually increases, reaches the maximum value and then gradually decreases. When the Mo element content is 10% and 15%, the hardness of Ti-Sn-Mo alloy is almost the same, which is 661.38HV and 660.72HV respectively. The preparation method of medical Ti-Sn-Mo alloy coating on pure titanium surface improves the wear resistance, hardness and biocompatibility of the coating through laser cladding technology, and has broad application prospects.
[0077] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a medical Ti-Sn-Mo alloy coating on a pure titanium surface, characterized in that: Laser cladding technology is used to clad a Ti-10Sn-xMo (x=5, 10, 15, 20, wt%) alloy coating on the surface of pure titanium. The specific steps include: Step 1. Material preparation: spherical Ti powder, quasi-spherical Sn powder and quasi-spherical Mo powder are mixed in the proportion of Ti-10Sn-xMo (x=5, 10, 15, 20, wt%); Step 2. Substrate treatment: using TA1 pure titanium plate as the substrate, grinding, polishing and preheating the substrate; Step 3. Laser cladding: a laser machine with a wavelength of 1080nm is used for cladding. The coaxial powder feeding method is used to control the powder flow rate and coating thickness in real time. High-purity argon is used as the protective gas. Step 4. Cooling and testing: placing the alloy coating on a heating furnace and cooling it with the furnace; Step 5. Adjust the powder ratio according to the ratio of Ti-10Sn-xMo (x=5, 10, 15, 20, wt%), and repeat the operations of steps 1 to 4.
2. The method for preparing a medical Ti-Sn-Mo alloy coating on a pure titanium surface according to claim 1, characterized in that: In step 1, after the powders are prepared in proportion, they are mixed in a vertical planetary ball mill at a rotation speed of 200-300 r / min and a ball milling time of 2-3 h to mix the powders evenly.
3. The method for preparing a medical Ti-Sn-Mo alloy coating on a pure titanium surface according to claim 2, characterized in that: The cladding powders used in the process of cladding Ti-10Sn-xMo alloy coating on the surface of pure titanium are all single-element powders, including: spherical Ti powder (purity>99.4%, powder particle size of 70μm~120μm), quasi-spherical Sn powder (purity>99.6%, powder particle size of 60μm~90μm) and quasi-spherical molybdenum powder (99.99%, powder particle size of 60μm~80μm).
4. The method for preparing a medical Ti-Sn-Mo alloy coating on a pure titanium surface according to claim 3, characterized in that: During the grinding and polishing stage, a 4-inch silicon carbide louver is used to grind the pure titanium surface, and excess grinding chips are wiped off with ethanol until the metallic luster appears.
5. The method for preparing a medical Ti-Sn-Mo alloy coating on a pure titanium surface according to claim 4, characterized in that: The preheating temperature in step 2 is 400°C.
6. The method for preparing a medical Ti-Sn-Mo alloy coating on a pure titanium surface according to claim 5, characterized in that: The laser cladding steps of step 3 include: First, take the preheated substrate out of the heating furnace and place it on the workbench; The powder was loaded into the powder feeder, and the laser power was adjusted to 2000w and the speed to 6mm / s; At the beginning, the protective Ar gas is turned on, and then the laser is turned on after the powder flows out. The laser beam causes the powder to quickly heat up to a temperature higher than the melting point on the substrate surface; The melt forms a liquid pool, which expands on the material surface through surface tension and capillary phenomena, and gradually solidifies to form a uniform and dense cladding layer.
7. The method for preparing a medical Ti-Sn-Mo alloy coating on a pure titanium surface according to claim 6, characterized in that: In the laser cladding process, the laser power was 2000 W and the scanning speed was 6 mm / s.
8. The method for preparing a medical Ti-Sn-Mo alloy coating on a pure titanium surface according to claim 7, characterized in that: During the laser cladding process, Ar was used as the protective gas, the gas flow rate was 10 (L / min), the delivery rate was 1.3 (r / min), the defocusing amount was 40 mm, and the overlap rate was 50%.
Citation Information
Patent Citations
Preparation methods of biomedical Ti-Sn coating alloy and medical dental alloy
CN104651829A
Processing method of surface anti-bacterial biological coating of medical titanium alloy
CN109023343A
Titanium alloy, powder of the titanium alloy and method of manufacturing thereof
EP4349509A1
Process for producing a beta-alloy Titanium Niobium Zirconium (TNZ) with a very low modulus of elasticity for biomedical applications and its embodiment by additive manufacturing.
US20190111482A1