Selenium antimony sulfide-lead sulfide composite film and preparation method and application thereof
By electrodeposition and annealing on the selenium antimony sulfide film, the high cost and toxicity of Spiro-OMeTAD are solved, and the efficiency of solar cells is improved and the efficiency of solar cells is improved. Stability has driven its commercialization process.
Patent Information
- Application Number
- CN202410993481.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, Spiro-OMeTAD, as the hole layer of a solar cell device, has problems such as high cost, high toxicity and unstable, which affects the efficiency and safety of selenium antimony sulfide thin film solar cells.
Electrochemical method is used to electrodeposit the selenium antimony sulfide film in the lead-containing electrolyte in the three-electrode system to form an antimony sulfide-lead sulfide composite film, and improve its crystallinity and stability through annealing treatment, as an inorganic space The acupoint layer replaces the traditional Spiro-OMeTAD.
It improves the photoelectric conversion efficiency of solar cells, reduces production costs, simplifies processes, extends the service life of the device, and provides a more stable inorganic hole layer, which promotes the commercialization of solar cell devices.
Smart Images

Figure CN118910689A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cell devices, and in particular to an antimony selenide sulfide-lead sulfide composite film and a preparation method and application thereof. Background Art
[0002] Antimony-based chalcogenide semiconductor materials have the advantages of abundant element reserves, non-toxicity and harmlessness. Among them, antimony selenide sulfide (Sb2(S,Se)3) has an adjustable band gap width (1.1-1.7eV) and a high absorption coefficient in the visible light range (>10 5 cm -1 ), has attracted widespread attention from researchers in recent years. Lead sulfide quantum dots also exhibit excellent photoelectric properties. However, due to the enrichment of lead by cadmium sulfide, improving the efficiency of antimony selenide sulfide thin-film solar cells remains to be studied.
[0003] Existing methods for preparing antimony selenide sulfide thin films include physical and chemical methods. Physical methods mainly include thermal evaporation, magnetron sputtering, near-space sublimation, molecular beam epitaxy, etc., but the equipment required for physical methods is generally expensive and has high costs. Chemical methods include solution methods, chemical water bath deposition methods, hydrothermal methods, electrochemical deposition, etc. These methods are low-cost and simple to operate, and are widely used preparation methods. At present, the photoelectric conversion efficiency of antimony selenide sulfide thin-film solar cells prepared by the hydrothermal method has reached 10.7%, but Spiro-OMeTAD is currently mainly used as the vacancy layer. The raw materials and preparation costs of this vacancy layer are relatively high, and it has great toxicity and instability. In addition, Spiro-OMeTAD needs to be dissolved in chlorobenzene and coated on the surface of the antimony selenide sulfide film. However, due to its acute toxicity, chlorobenzene can enter the human body through inhalation, ingestion, and skin contact, and has an inhibitory and anesthetic effect on the central nervous system. Long-term exposure can cause liver and kidney diseases. Summary of the Invention
[0004] The purpose of the present invention is to provide an antimony selenide sulfide-lead sulfide composite film and its preparation method and application, so as to solve the problems of high cost, high toxicity and instability when Spiro-OMeTAD is used as a cavitation layer.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing an antimony selenide sulfide-lead sulfide composite film, comprising the following steps:
[0007] (1) In a three-electrode system, an antimony selenide sulfide film is electrodeposited in a lead-containing electrolyte; the lead-containing electrolyte does not contain sulfur;
[0008] (2) annealing the antimony selenide sulfide film after electrodeposition obtained in step (1) to obtain an antimony selenide sulfide-lead sulfide composite film.
[0009] Preferably, in the preparation method, the three-electrode system in step (1) is: antimony selenide sulfide film is the working electrode, Pt is the counter electrode, and Ag / AgCl is the reference electrode.
[0010] Preferably, in the preparation method, the lead salt in the lead salt-containing electrolyte in step (1) includes one or more of lead nitrate, lead acetate and lead chloride.
[0011] Preferably, in the preparation method, the concentration of the lead salt in the lead salt-containing electrolyte in step (1) is 0.01 to 1 mol / L.
[0012] Preferably, in the preparation method, the potential of the electrodeposition in step (1) is -1 to -0.25 V, and the time is 30 s to 3 min.
[0013] Preferably, in the preparation method, the temperature of the annealing treatment in step (2) is 350-380° C., and the time is 5-20 minutes.
[0014] Preferably, in the preparation method, the antimony selenide sulfide film in step (1) is prepared by a hydrothermal method.
[0015] The present invention also provides an antimony selenide sulfide-lead sulfide composite film prepared by the preparation method, wherein the antimony selenide sulfide-lead sulfide composite film comprises an antimony selenide sulfide layer and a lead sulfide layer grown on the antimony selenide sulfide layer.
[0016] The present invention also provides an application of the antimony selenide sulfide-lead sulfide composite film in a solar cell device.
[0017] Preferably, in the application, the solar cell device includes a cathode, an electron transport layer, an antimony selenide sulfide-lead sulfide composite film and an anode; the antimony selenide sulfide layer in the antimony selenide sulfide-lead sulfide composite film serves as a light absorption layer, and the lead sulfide layer serves as a hole layer.
[0018] It can be seen from the above technical solutions that compared with the prior art, the present invention has the following beneficial effects:
[0019] (1) The present invention adopts an electrochemical treatment method for the antimony selenide sulfide film, using the lead ions in the sulfur-free electrolyte to combine with the sulfur atoms of the antimony selenide sulfide film itself under electrochemical and concentration driving forces to form an ultra-thin lead sulfide layer with a thickness of about 10nm. The ultra-thin lead sulfide layer can be modified on its surface. At the same time, the ultra-thin lead sulfide layer can be used as an inorganic hole layer (or called an intermediate interface buffer layer), providing a new method for subsequent antimony selenide sulfide film to be made into devices to improve the photoelectric conversion efficiency. In addition, when the lead sulfide in the antimony selenide sulfide-lead sulfide composite film prepared by the present invention is used as an inorganic hole layer, the device efficiency does not change significantly within one month, while when Spiro-OMeTAD is used as the hole layer of antimony selenide under the same conditions, the device efficiency will decay to 70% of the original after one month, indicating that the antimony selenide sulfide-lead sulfide composite film prepared by the present invention has excellent stability.
[0020] (2) The electro-deposition process used in the present invention was tested by XRD and found that: as the deposition potential decreases, the peak intensity of the crystal plane (hk1) of the film gradually increases, which is conducive to the transport of carriers, thereby improving the efficiency of the device. In addition, the electrochemical treatment will give the antimony selenide sulfide film an electrochemical driving force, driving the amorphous amorphous film to form a more stable state, improving the crystallinity of the antimony selenide sulfide film and optimizing the film orientation of the antimony selenide sulfide, thereby improving the photoelectric performance of the antimony selenide sulfide film. The photoelectric conversion efficiency of the FTO / CdS / Sb2(S,Se)3-PbS / Au device prepared by the present invention can reach 6.19%, which can increase the basic photoelectric conversion efficiency value by 1% compared with the device with the FTO / CdS / Sb2(S,Se)3 / Au structure.
[0021] (3) The advantages of the annealing treatment used in the present invention are: assisting in the completion of ion diffusion and secondary crystal growth of the film, thereby increasing the grain size and improving the crystallinity of the film.
[0022] (4) The present invention prepares a solar cell device that relies solely on an antimony selenide sulfide-lead sulfide composite film as a key functional layer, discarding the Spiro-OMeTAD organic hole layer that is indispensable in traditional solar cells, directly reducing production costs and simplifying the preparation process of solar cells. In addition, the antimony selenide sulfide-lead sulfide composite film has better stability, which extends the battery life and is conducive to promoting the commercialization process of solar cell devices.
[0023] (5) The electrodeposition process provided by the present invention is simple and fast, with low raw material cost and mild reaction conditions. In addition, the reaction phenomenon and the curve of current change over time can be observed in real time, which facilitates deeper research on the reaction mechanism. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for describing the embodiments or the prior art.
[0025] Figure 1 It is the it curve diagram of Examples 1 to 3;
[0026] Figure 2 SEM images of Examples 1 to 3 and Comparative Example 1, wherein (a) is Comparative Example 1, (b) is Example 1, (c) is Example 3, and (d) is Example 2;
[0027] Figure 3 1 are XPS graphs of Example 1 and Comparative Example 1, a is the Sb 3d graph of Comparative Example 1, b is the Pb 4f graph of Comparative Example 1, c is the Sb 3d graph of Example 1, and d is the Pb 4f graph of Example 1;
[0028] Figure 4 XRD patterns of Examples 1 to 3 and Comparative Example 1;
[0029] Figure 5 are SEM images of Examples 1, 4 to 6;
[0030] Figure 6 The XRD patterns of Examples 1, 4 to 6 and Comparative Example 1 are shown;
[0031] Figure 7 is a texture coefficient diagram of Examples 1, 4 to 6 and Comparative Example 1;
[0032] Figure 8 JV curves of solar cell devices obtained in Application Examples 1 to 3 and Comparative Application Example 1;
[0033] Figure 9 JV curves of the solar cell devices obtained in Application Example 4 and Comparative Application Example 2; DETAILED DESCRIPTION
[0034] The present invention provides a method for preparing an antimony selenide sulfide-lead sulfide composite film, comprising the following steps:
[0035] (1) In a three-electrode system, an antimony selenide sulfide film is electrodeposited in a lead-containing electrolyte; the lead-containing electrolyte does not contain sulfur;
[0036] (2) annealing the antimony selenide sulfide film after electrodeposition obtained in step (1) to obtain an antimony selenide sulfide-lead sulfide composite film.
[0037] In the present invention, the antimony selenide sulfide film in step (1) is prepared by a hydrothermal method.
[0038] In the present invention, the method for preparing the antimony selenide sulfide film in step (1) preferably includes the following steps: mixing potassium antimony tartrate, sodium thiosulfate and selenourea, performing a hydrothermal reaction in a closed environment, and drying to obtain an antimony selenide sulfide precursor film; and annealing the antimony selenide sulfide precursor film to obtain an antimony selenide sulfide film.
[0039] In the present invention, the condition parameters in the method for preparing the antimony selenide sulfide film are not limited, and schemes well known to those skilled in the art can be adopted.
[0040] In the present invention, the three-electrode system in step (1) is preferably: antimony selenide sulfide film is the working electrode, Pt is the counter electrode, and Ag / AgCl is the reference electrode.
[0041] In the present invention, the lead salt in the lead salt-containing electrolyte in step (1) preferably includes one or more of lead nitrate, lead acetate and lead chloride, further preferably includes one of lead nitrate, lead acetate and lead chloride, and more preferably is lead nitrate.
[0042] In the present invention, the lead salt electrolyte in step (1) is preferably an aqueous solution of lead salt.
[0043] In the present invention, the concentration of the lead salt in the lead salt-containing electrolyte in step (1) is preferably 0.01 to 1 mol / L, more preferably 0.01 to 0.1 mol / L, and more preferably 0.1 mol / L.
[0044] In the present invention, the potential of the electrodeposition in step (1) is preferably -1 to -0.25 V, more preferably -0.75 to -0.25 V, and more preferably -0.5 V; the time is preferably 30 s to 3 min, more preferably 40 s to 2 min, and more preferably 1 min.
[0045] In the present invention, after the electrodeposition in step (1), the following steps are preferably further performed: ultrapure water cleaning, ethanol cleaning, and nitrogen drying in sequence.
[0046] In the present invention, there is no limitation on the parameters of the ultrapure water cleaning, the ethanol cleaning and the nitrogen drying, and any scheme well known to those skilled in the art may be used.
[0047] In the present invention, the conditions for the annealing treatment in step (2) are: the temperature is preferably 350-380°C, more preferably 360-370°C, and more preferably 370°C; the time is preferably 5-20 minutes, more preferably 10-15 minutes, and more preferably 10 minutes; and the atmosphere is preferably nitrogen.
[0048] The present invention also provides an antimony selenide sulfide-lead sulfide composite film, which comprises an antimony selenide sulfide layer and a lead sulfide layer grown on the antimony selenide sulfide layer.
[0049] The present invention also provides an application of the antimony selenide sulfide-lead sulfide composite film in a solar cell device.
[0050] In the present invention, the solar cell device includes a cathode, an electron transport layer, an antimony selenide sulfide-lead sulfide composite film and an anode; the antimony selenide sulfide layer in the antimony selenide sulfide-lead sulfide composite film serves as a light absorption layer, and the lead sulfide layer serves as a hole layer.
[0051] In the present invention, the cathode, the electron transport layer, and the anode are not limited and can be implemented using methods known to those skilled in the art. Specifically, in an embodiment of the present invention, the cathode is fluorine-doped tin dioxide transparent conductive glass (FTO), the electron transport layer is cadmium sulfide (CdS), and the anode is a gold electrode.
[0052] In the present invention, the FTO is preferably pre-treated before use, and the pre-treatment preferably includes the following steps:
[0053] The FTO was ultrasonically cleaned with glass cleaner, ultrapure water, isopropyl alcohol, acetone, and anhydrous ethanol for 10 to 60 minutes respectively, dried with nitrogen, and then cleaned with an oxygen ion cleaner for 15 to 20 minutes.
[0054] In the present invention, the method for preparing CdS preferably comprises the following steps: depositing a CdS film with a thickness of 50 to 70 nm on FTO using a chemical water bath method.
[0055] In the present invention, the parameter conditions in the chemical water bath method are not limited, and schemes well known to those skilled in the art can be adopted.
[0056] In the present invention, the method for preparing the gold electrode comprises the following steps: using a thermal evaporation process to deposit a gold electrode with a thickness of 60 to 80 nm.
[0057] In the present invention, the parameter conditions in the thermal evaporation process are not limited, and solutions well known to those skilled in the art can be adopted.
[0058] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.
[0059] Example 1
[0060] This embodiment provides a method for preparing an antimony selenide sulfide-lead sulfide composite film, comprising the following steps:
[0061] (1) 0.2003 g of potassium antimony tartrate, 0.7942 g of sodium thiosulfate, and 30 mg of selenourea were mixed with 40 mL of aqueous solution, and the mixture was hydrothermally reacted at 135° C. for 120 min in a closed environment, and then dried to obtain an antimony selenide sulfide precursor film; the antimony selenide sulfide precursor film was annealed at 370° C. for 5 min in a nitrogen atmosphere to obtain an antimony selenide sulfide film;
[0062] (2) 0.01 mol of lead nitrate (Pb(NO3)2) was dissolved in 100 mL of aqueous solution and stirred to obtain a 0.1 mol / L aqueous solution of lead nitrate; in a three-electrode system, the antimony selenide sulfide film was used as the working electrode, Pt was used as the counter electrode, and Ag / AgCl was used as the reference electrode. The antimony selenide sulfide film was electroplated in the electrolyte of the lead nitrate aqueous solution at a potential of -0.5 V for 1 min. During the reaction, a yellow-red acid-soluble substance was observed on the counter electrode, which was further speculated to be lead oxide. The film on the working electrode at a negative potential would undergo a reduction reaction; then, ultrapure water washing, ethanol washing, and nitrogen drying were performed in sequence;
[0063] (3) The antimony selenide sulfide film after electrodeposition obtained in step (2) is annealed in a nitrogen atmosphere at 370° C. for 5 min to obtain an antimony selenide sulfide-lead sulfide composite film.
[0064] Example 2
[0065] The difference between Example 2 and Example 1 is that the lead nitrate in step (2) is replaced by lead acetate ((CH3COO)2Pb), and the other parameter conditions are the same as those in Example 1.
[0066] Example 3
[0067] The difference between Example 3 and Example 1 is that the lead nitrate in step (2) is replaced by lead chloride (PbCl2), and the other parameter conditions are the same as those in Example 1.
[0068] Comparative Example 1
[0069] This comparative example provides a method for preparing an antimony selenide sulfide film, which differs from Example 1 in that steps (2) to (3) are deleted, and other parameter conditions are the same as those in Example 1.
[0070] The corresponding it curves are drawn for the electrodeposition process of steps (2) of Examples 1 to 3, as shown in FIG. Figure 1 As shown. Figure 1It can be seen that the electrolyte activity of the lead nitrate aqueous solution is the highest, the reaction of lead ions in the lead nitrate aqueous solution is more active, and the current gradually decreases with time. It can be understood that the electrolyte system has reached dynamic equilibrium at this time.
[0071] The antimony selenide sulfide films prepared in Examples 1 to 3 and Comparative Example 1 were subjected to SEM examination. The results are as follows: Figure 2 As shown. Figure 2 It can be seen that after electrochemical treatment, the three lead salts can produce an adsorbable substance, namely lead sulfide, on the surface of the antimony selenide sulfide film, which will make the grain boundaries of the antimony selenide sulfide film blurred.
[0072] The antimony selenide sulfide films prepared in Example 1 and Comparative Example 1 were subjected to XPS testing. The results are as follows: Figure 3 As shown. Figure 3 As can be seen, compared with Comparative Example 1, Example 1 exhibits lead sulfide peaks at 137.7 eV and 138.74 eV, demonstrating the formation of lead sulfide on the surface. Among the Sb 3d peaks, the O1s peaks (at 530 eV and 532 eV) in Example 1 are significantly weakened compared to those in Comparative Example 1, indicating that the electrochemical treatment inhibits oxidation of the antimony selenide sulfide film.
[0073] The antimony selenide sulfide films prepared in Examples 1 to 3 and Comparative Example 1 were subjected to XRD testing. The results are as follows: Figure 4 As shown. Figure 4 It can be seen that after electrochemical treatment, the crystallinity of antimony selenide sulfide film is significantly improved compared with that of comparative example 1, and the (hk1) orientation is enhanced to a certain extent ((hk1) orientation is in Figure 4 The corresponding values are: 29.296° corresponds to (211), 32.399° corresponds to (221), 33.445° corresponds to (301), and 46.711° corresponds to (431).
[0074] Example 4
[0075] The difference between Example 4 and Example 1 is that the potential of the electrodeposition in step (2) is modified to -0.25 V, and the other parameter conditions are the same as those in Example 1.
[0076] Example 5
[0077] The difference between Example 5 and Example 1 is that the potential of the electrodeposition in step (2) is modified to -0.75 V, and the other parameter conditions are the same as those in Example 1.
[0078] Example 6
[0079] The difference between Example 6 and Example 1 is that the potential of the electrodeposition in step (2) is changed to -1V, and the other parameter conditions are the same as those in Example 1.
[0080] The antimony selenide sulfide films prepared in Examples 1, 4 to 6 were subjected to SEM examination. The results are as follows: Figure 5 As shown. Figure 5 It can be seen that as the electrodeposition potential decreases, the surface of the antimony selenide sulfide film becomes more mottled. This can be attributed to the partial reduction of antimony selenide sulfide to produce impurities that destroy the film. Too low a potential will lead to a series of side reactions, so it is crucial to determine the appropriate working potential.
[0081] The antimony selenide sulfide films prepared in Examples 1, 4 to 6 and Comparative Example 1 were subjected to XRD testing. The results are as follows: Figure 6 As shown. Figure 6 It can be seen that Figure 6 It can be seen that the (hk1) crystal plane peak intensity of the antimony selenide sulfide films prepared in Examples 1 and 4 to 6 is enhanced after electrochemical treatment, and the enhancement becomes more obvious as the potential decreases. When the potential is -1 V, some miscellaneous peaks appear, indicating that by-products are generated.
[0082] according to Figure 6 The XRD pattern of the antimony selenide sulfide film is further used to calculate the texture coefficient. The calculation formula is shown in Formula 1. The results are shown in Figure 7 As shown ( Figure 7 The "C" in the table refers to Comparative Example 1). Figure 7 It can be seen that the antimony selenide sulfide film treated with a potential ranging from -0.25V to -0.75V has enhanced (211) and (211) crystallinity, which will be more conducive to carrier transport; when the potential is more negative, the antimony selenide sulfide film will be destroyed.
[0083]
[0084] In formula 1, N is the total number of crystal planes used in the calculation, and h, k, and l are the diffraction crystal planes. Index: I (hkl) and I 0(hkl) are the diffraction peak intensities of the corresponding standard samples on the (hkl) crystal plane in actual measurement and in the database recognized by the Joint Committee on Powder Diffraction Standards, respectively.
[0085] Application Example 1
[0086] This application example provides a method for preparing a solar cell device, comprising the following steps:
[0087] (1) The FTO was ultrasonically cleaned with glass cleaner, ultrapure water, isopropyl alcohol, acetone, and anhydrous ethanol for 30 min, dried with nitrogen, and then cleaned with oxygen ion cleaner for 15 min;
[0088] (2) A CdS film was deposited on FTO using a chemical water bath method. The specific scheme of the chemical water bath method is as follows: first, 10 mL of a 15 mmol / L cadmium nitrate solution and 13 mL of an ammonia solution were measured and mixed in a beaker for 90 seconds, 6.4 mL of a 5 mol / L thiourea solution was added and stirred for 30 seconds, and finally 70 mL of ultrapure water was added and stirred evenly to obtain a precursor solution. The cleaned FTO was deposited in a water bath at 66°C for 9.5 minutes to obtain a CdS film with a thickness of 60 nm.
[0089] (3) is the same as steps (1) to (3) of Example 1;
[0090] (4) A layer of gold electrode was deposited on the antimony selenide sulfide-lead sulfide composite film using a thermal evaporation process. The thermal evaporation process was as follows: the prepared FTO / CdS / Sb2(S,Se)3-PbS film was fixed in a mask at 5.0×10 -4 A 65 nm thick Au electrode layer was deposited under a pressure of Pa.
[0091] Application Example 2
[0092] The difference between Application Example 2 and Application Example 1 is that Example 1 in step (3) is replaced by Example 2, and other parameter conditions are the same as those of Application Example 1.
[0093] Application Example 3
[0094] The difference between Application Example 3 and Application Example 1 is that Example 1 in step (3) is replaced by Example 3, and other parameter conditions are the same as those of Application Example 1.
[0095] Comparative Application Example 1
[0096] The difference between comparative application example 1 and application example 1 is that embodiment 1 in step (3) is replaced by comparative example 1, and other parameter conditions are the same as those of application example 1.
[0097] The solar cell devices obtained in Application Examples 1 to 3 and Comparative Application Example 1 were subjected to bright-state volt-ampere characteristic curve tests at 25°C. The light source used was a XES-70S1 solar simulator with a xenon lamp. The irradiance of the light source was calibrated to AM1.5 (1000W / m 2 ), and connect a Keithley 2400 digital source meter to provide voltage. Under this condition, the test was carried out to obtain the current density-voltage (JV) curve as shown in Figure 8 , as shown in Table 1. Figure 8 As shown in Table 1, the electrochemical treatment of lead salts improves the photoelectric conversion efficiency of the device, which is mainly reflected in the improvement of open circuit voltage and fill factor, but its short-circuit current decreases to a certain extent.
[0098] Table 1. Performance results of solar cell devices obtained in Application Examples 1 to 3 and Comparative Application Example 1
[0099] Application Cases <![CDATA[V oc (V)]]> <![CDATA[J sc (mA cm -2 )]]> FF(%) PCE (%) Application Example 1 0.53 17.64 54.95 5.09 Application Example 2 0.52 17.67 52.14 4.76 Application Example 3 0.53 17.39 52.84 4.86 Comparative Application Example 1 0.43 17.99 53.34 4.16
[0100] Application Example 4
[0101] This application example provides a method for preparing a solar cell device, comprising the following steps:
[0102] (1) The FTO was ultrasonically cleaned with glass cleaner, ultrapure water, isopropyl alcohol, acetone, and anhydrous ethanol for 60 min, dried with nitrogen, and then cleaned with oxygen ion cleaner for 20 min;
[0103] (2) A CdS thin film was deposited on FTO using a chemical water bath method. The specific scheme of the chemical water bath method is as follows: first, 10 mL of a 15 mmol / L cadmium nitrate solution and 13 mL of an ammonia solution were measured and mixed in a beaker for 90 seconds, 6.4 mL of a 5 mol / L thiourea solution was added and stirred for 30 seconds, and finally 70 mL of ultrapure water was added and stirred evenly to obtain a precursor solution. The cleaned FTO was deposited in a water bath at 66°C for 10 minutes to obtain a CdS thin film with a thickness of 70 nm.
[0104] (3) is the same as steps (1) to (3) of Example 1;
[0105] (4) A layer of gold electrode was deposited on the antimony selenide sulfide-lead sulfide composite film using a thermal evaporation process. The thermal evaporation process was as follows: the prepared FTO / CdS / Sb2(S,Se)3-PbS film was fixed in a mask at 5.0×10 -4 An 80 nm thick Au electrode layer was deposited under a pressure of 1 Pa.
[0106] Comparative Application Example 2
[0107] The difference between Comparative Application Example 2 and Application Example 4 is that Example 1 in step (3) is replaced by Comparative Example 1, and other parameter conditions are the same as those of Application Example 4.
[0108] Application Example 4 and Comparative Application Example 2 The prepared solar cell was subjected to bright-state volt-ampere characteristic curve test at 25°C. The light source used was a XES-70S1 solar simulator with a xenon lamp. The irradiance of the light source was calibrated to AM1.5 (1000W / m 2 ), and connect a Keithley 2400 digital source meter to provide voltage. The JV curve under this condition is as follows Figure 9 As shown. Figure 9It can be seen that the photoelectric conversion efficiency of Comparative Application Example 2 is 4.5%; and compared with Comparative Application Example 2, the photoelectric conversion efficiency of Application Example 4 is 6.19%, which is increased by 37%.
[0109] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A method for preparing an antimony selenide sulfide-lead sulfide composite film, characterized in that: The following steps are involved: (1) In a three-electrode system, an antimony selenide sulfide film is electrodeposited in a lead salt electrolyte; the lead salt electrolyte does not contain sulfur; (2) annealing the antimony selenide sulfide film after electrodeposition obtained in step (1) to obtain an antimony selenide sulfide-lead sulfide composite film.
2. The preparation method according to claim 1, characterized in that: The three-electrode system in step (1) is: antimony selenide sulfide film is the working electrode, Pt is the counter electrode, and Ag / AgCl is the reference electrode.
3. The preparation method according to claim 1, characterized in that: The lead salt in the lead salt-containing electrolyte in step (1) includes one or more of lead nitrate, lead acetate and lead chloride.
4. The preparation method according to claim 1 or 3, characterized in that: The concentration of lead salt in the lead salt-containing electrolyte in step (1) is 0.01 to 1 mol / L.
5. The preparation method according to any one of claims 1 to 3, characterized in that: The potential of the electrodeposition in step (1) is -1 to -0.25 V, and the time is 30 s to 3 min.
6. The preparation method according to claim 1, characterized in that: The annealing treatment in step (2) is carried out at a temperature of 350 to 380° C. and for a time of 5 to 20 minutes.
7. The preparation method according to claim 5, characterized in that: The antimony selenide sulfide film in step (1) is prepared by a hydrothermal method.
8. The antimony selenide sulfide-lead sulfide composite film obtained by the preparation method according to any one of claims 1 to 7, characterized in that: The antimony selenide sulfide-lead sulfide composite film comprises an antimony selenide sulfide layer and a lead sulfide layer grown on the antimony selenide sulfide layer.
9. Use of the antimony selenide sulfide-lead sulfide composite film according to claim 8 in a solar cell device.
10. The use according to claim 9, characterized in that: The solar cell device comprises a cathode, an electron transport layer, an antimony selenide sulfide-lead sulfide composite film and an anode; the antimony selenide sulfide layer in the antimony selenide sulfide-lead sulfide composite film serves as a light absorption layer, and the lead sulfide layer serves as a hole layer.