High-performance silicon wafer material and preparation process thereof
The problem of low cutting and grinding efficiency of silicon columns in silicon wafer preparation is solved by growing silicon crystal rods through regional melting method and combining pressure sensors and wipe roller technology, and the problem of low-quality silicon wafer preparation is achieved, which improves silicon crystals purity and resistivity of the circle.
Patent Information
- Application Number
- CN202410890100.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-08
AI Technical Summary
During the preparation of existing silicon wafers, the order of cutting and grinding of silicon columns leads to the inability to improve processing efficiency, and it is easy to produce debris and unsmooth edges, affecting subsequent processing.
The silicon crystal rod is grown by regional melting method, combining thermal energy generation method and surface tension support to avoid crucible contamination; during the grinding process, the pressure sensor and wipe roller are used to achieve real-time monitoring and cleaning, and through the coordination of silicon column rotation and cutting steel wire, it is achieved Combined grinding of silicon wafer edges reduces equipment occupancy and cost.
The purity and resistivity of the silicon wafer are improved, synchronous operation of grinding and detection is achieved, preparation efficiency is improved, and equipment cost and space occupation are reduced.
Smart Images

Figure CN118910723A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of silicon wafers, and in particular to a high-performance silicon wafer material and a preparation process thereof. Background Art
[0002] Silicon wafer: A wafer is purified silicon, which is then made into long silicon rods, which become the material for quartz semiconductors used to manufacture integrated circuits. After photoengraving, grinding, polishing, slicing and other processes, the polycrystalline silicon is melted and pulled out into single crystal silicon rods, which are then cut into thin wafers.
[0003] In the existing silicon wafer preparation process, the two processes of cutting silicon pillars to produce silicon slices and grinding the edges of the silicon slices to make them smooth are often separated and have a sequence, resulting in the inability to further improve the processing efficiency.
[0004] Therefore, in view of this, the existing structure and defects are studied and improved, and a high-performance silicon wafer material and its preparation process are proposed. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a high-performance silicon wafer material and a preparation process thereof, which solves the problems raised in the above-mentioned background technology.
[0006] To achieve the above objectives, the present invention is implemented through the following technical scheme: a high-performance silicon wafer material, the raw material of the high-performance silicon wafer material includes a zone melting method silicon crystal rod, and the zone melting method silicon crystal rod is a silicon crystal rod that is grown and purified by using a zone melting method to grow semiconductor rod material.
[0007] A preparation process for high-performance silicon wafer material, the preparation process comprising the following steps:
[0008] S1. Silicon crystal rod preparation:
[0009] First, the semiconductor rod is fixed vertically with a clamp from the upper and lower axes, and the heat energy is used to generate a molten zone at one end of the semiconductor rod, and then the single crystal seed crystal is melted, and then the molten zone is slowly moved to the other end of the rod until it passes through the entire rod to grow into a single crystal, i.e., a silicon crystal rod;
[0010] S2, outer diameter grinding:
[0011] The silicon crystal rod is taken out, and the cylindrical silicon crystal rod is clamped horizontally and its two ends are cut into segments to obtain silicon columns. The two ends of the silicon column are clamped and placed horizontally, and the surface of the silicon column is ground by a grinding device to obtain a silicon column with a precise diameter;
[0012] S3, cutting silicon wafer:
[0013] The silicon column is cut at equal intervals to obtain silicon wafers of preset thickness. When cutting, the grinding fixture is installed at equal intervals. The silicon column is placed horizontally on the top surface of the grinding fixture and clamped at both ends. The cutting steel wire moves vertically from top to bottom, and the silicon column rotates slowly at the same time, so that the steel wire first cuts a wire groove on the surface of the silicon column. As the wire groove deepens, the unseparated silicon wafer sinks so that its edge is stuck in the groove of the grinding fixture, and the self-rotation of the silicon column achieves the effect of grinding the edge of the unseparated silicon wafer. As the steel wire descends, the silicon wafers are completely separated, and then each silicon wafer is taken out and ground on both sides;
[0014] S4, structural etching:
[0015] After the silicon wafers are ground and cleaned, photosensitive resin is coated on the surface of each silicon wafer, and the photosensitive resin is exposed and developed using a photolithography machine to form the required pattern. The silicon wafers are then placed in an etching solution and etched according to the photolithography pattern to form the required structure by etching away the unnecessary silicon layer.
[0016] S5. Polishing and cleaning:
[0017] The etched and double-sided polished silicon wafer is also called a silicon wafer. The surface of the silicon wafer is polished with a polishing cloth and polishing slurry, and then the residual particle impurities on the surface of the silicon wafer are removed by cleaning.
[0018] S6. Quality inspection:
[0019] The thickness, flatness and resistivity of the polished silicon wafer are tested, and the silicon wafer is packaged after the test results pass.
[0020] Furthermore, in the step S1, the heat energy is generated by electron bombardment, high-frequency induction or optical focusing, and the material in the molten zone melts and is supported by surface tension without falling, and the crystal orientation of the single crystal is the same as that of the seed crystal.
[0021] Furthermore, in the step S2, the silicon column rotates when it is ground, and the grinding structure grinds it on the top surface of the silicon column, and a pressure sensor group distributed linearly is arranged at the bottom of the silicon column, and a wiping roller structure is arranged on one side of the silicon column. During grinding, the wiping roller is attached to the side of the silicon column to clean the residue produced by grinding, and the surface of the silicon column after wiping rotates to the bottom. At this time, the pressure sensor group detects the pressure value in real time. When the pressure sensed by the sensor at each part is within the threshold, it indicates that the diameter of each part of the silicon column has reached the preset size.
[0022] Furthermore, in the step S3, a groove is provided on the top surface of the grinding fixture, and the groove is arc-shaped to match the curvature of the edge of the silicon wafer.
[0023] Furthermore, the inner surface of the groove is a grinding surface, and the inner diameter of the groove on the top surface of the grinding fixture is adapted to the preset thickness of the silicon wafer.
[0024] Furthermore, in the step S4, the silicon wafer needs to be double-sided ground again after etching to remove surface protrusions and make the surface of the silicon wafer flat.
[0025] Furthermore, in the step S5, the particulate impurities include organic particulate impurities and inorganic particulate impurities.
[0026] Furthermore, in the step S6, laser scattering is used to determine the defects and quantity on the surface of the silicon wafer during the inspection, and the silicon wafer passes the inspection only when the inspection results meet the preset requirements.
[0027] Furthermore, the process for preparing the high-performance silicon wafer material is applied to the technical field of preparing silicon wafers.
[0028] The present invention provides a high-performance silicon wafer material and a preparation process thereof, which has the following beneficial effects:
[0029] 1. The high-performance silicon wafer material and its preparation process use the zone melting method to prepare silicon crystal rods without the need for a crucible during the preparation process, thereby avoiding crucible contamination and greatly improving the purity of the silicon crystal rods. Due to the impurity segregation and evaporation effects, high-resistivity silicon crystal rods can be grown, so that the silicon wafer prepared from the silicon crystal rods has high resistivity. In the process of grinding the outer diameter of the silicon column, the pressure sensor is used to linearly sense the pressure of each rotating part to monitor the grinding effect in real time, and based on the numerical feedback of the pressure sensing, the specific grinding part can be controlled to be precisely ground, so that the diameter of each part of the silicon column meets the standard.
[0030] 2. In order to prevent the debris generated by grinding from interfering with pressure sensing, the high-performance silicon wafer material and its preparation process utilize the self-rotation of the silicon column and the rotation of the wiping roller so that the surface of the silicon column is wiped to remove debris before receiving pressure sensing, so as to avoid the debris from interfering with the pressure sensing value. In this way, real-time detection is achieved while grinding, without the need to constantly switch between the grinding and detection processes, so as to improve work efficiency.
[0031] 3. The high-performance silicon wafer material and its preparation process, the steel wire cuts the silicon column to produce wire grooves on its surface, and cooperates with the sinking of the clamping structure to make the silicon column through the wire grooves on its surface so that each unseparated silicon wafer is just stuck in the groove on the top surface of the grinding fixture, and the self-rotation of the silicon column makes its edge rub between the inner surfaces of the groove to achieve grinding of the silicon wafer edge and smooth its edge to reduce the possibility of fragments in subsequent processing, thereby realizing the combination of silicon wafer segmentation and silicon wafer edge grinding operations, thereby greatly reducing the space occupancy rate and equipment cost of the equipment, and greatly improving the preparation efficiency of silicon wafers. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The present invention is a schematic diagram of the preparation process of a high-performance silicon wafer material and its preparation process. DETAILED DESCRIPTION
[0033] The following embodiments of the present invention are described in further detail in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0034] like Figure 1 As shown, the present invention provides a technical solution: a high-performance silicon wafer material, the raw material of the high-performance silicon wafer material includes a zone melting method silicon crystal rod, and the zone melting method silicon crystal rod is a silicon crystal rod that adopts a regional melting method to grow and purify semiconductor rod materials.
[0035] A preparation process for high-performance silicon wafer material, the preparation process comprising the following steps:
[0036] S1. Silicon crystal rod preparation:
[0037] First, the semiconductor rod is fixed vertically with a clamp from the upper and lower axes, and the heat energy is used to generate a molten zone at one end of the semiconductor rod, and then the single crystal seed crystal is melted, and then the molten zone is slowly moved to the other end of the rod until it passes through the entire rod to grow into a single crystal, i.e., a silicon crystal rod;
[0038] The heat energy is generated by electron bombardment, high-frequency induction or optical focusing, and the material in the molten zone is melted and supported by surface tension without falling, and the crystal orientation of the single crystal is the same as that of the seed crystal;
[0039] The silicon crystal rod prepared by the zone melting method does not need to use a crucible during the preparation process, thereby avoiding crucible contamination, thereby greatly improving the purity of the silicon crystal rod, and due to the impurity segregation and evaporation effect, a high-resistivity silicon crystal rod can be grown, so that the silicon wafer prepared from the silicon crystal rod has a high resistivity;
[0040] S2, outer diameter grinding:
[0041] The silicon crystal rod is taken out, and the cylindrical silicon crystal rod is clamped horizontally and its two ends are cut into segments to obtain silicon columns. The two ends of the silicon column are clamped and placed horizontally, and the surface of the silicon column is ground by a grinding device to obtain a silicon column with a precise diameter;
[0042] When grinding the silicon column, the silicon column rotates, and the grinding structure grinds it on the top surface of the silicon column, and a pressure sensor group distributed in a linear shape is arranged at the bottom of the silicon column, and a wiping roller structure is arranged on one side of the silicon column. During grinding, the wiping roller is attached to the side of the silicon column to clean the residue generated by grinding. The wiped silicon column surface rotates to the bottom, and the pressure sensor group detects the pressure value in real time. When the pressure sensed by the sensor at each part is within the threshold, it means that the diameter of each part of the silicon column has reached the preset size.
[0043] During the process of grinding the outer diameter of the silicon column, the pressure sensor is used to linearly sense the pressure of each rotating part to monitor the grinding effect in real time, and based on the numerical feedback of the pressure sensing, the specific grinding part can be controlled to be precisely ground, so that the diameter of each part of the silicon column meets the standard. In order to prevent the debris generated by grinding from interfering with the pressure sensing, the self-rotation of the silicon column and the rotation of the wiping roller are used to wipe the surface of the silicon column before receiving the pressure sensing to remove debris, so as to avoid the debris from interfering with the pressure sensing value, thereby achieving real-time detection while grinding, without the need to constantly switch between the grinding and detection processes, so as to improve work efficiency;
[0044] S3, cutting silicon wafer:
[0045] The silicon column is cut at equal intervals to obtain silicon wafers of preset thickness. When cutting, the grinding fixture is installed at equal intervals. The silicon column is placed horizontally on the top surface of the grinding fixture and clamped at both ends. The cutting steel wire moves vertically from top to bottom, and the silicon column rotates slowly at the same time, so that the steel wire first cuts a wire groove on the surface of the silicon column. As the wire groove deepens, the unseparated silicon wafer sinks so that its edge is stuck in the groove of the grinding fixture, and the self-rotation of the silicon column achieves the effect of grinding the edge of the unseparated silicon wafer. As the steel wire descends, the silicon wafers are completely separated, and then each silicon wafer is taken out and ground on both sides;
[0046] The top surface of the grinding fixture is provided with a groove, the groove is arc-shaped and matches the curvature of the edge of the silicon wafer, the inner surface of the groove is a grinding surface, and the inner diameter of the groove on the top surface of the grinding fixture matches the preset thickness of the silicon wafer;
[0047] As the steel wire cuts the silicon column, grooves are generated on its surface. With the sinking of the clamping structure, the silicon column passes through the grooves on its surface so that each unseparated silicon wafer is just stuck in the groove on the top surface of the grinding fixture. The silicon column rotates so that its edge is in friction between the inner surfaces of the groove, so as to achieve grinding of the edge of the silicon wafer and smooth its edge, thereby reducing the possibility of fragments in subsequent processing. After grinding, the silicon column can stop rotating, and the steel wire further descends to separate the silicon wafers, thereby realizing the combination of silicon wafer segmentation and silicon wafer edge grinding operations, thereby greatly reducing the space occupancy rate and equipment cost of the equipment, and greatly improving the preparation efficiency of silicon wafers.
[0048] S4, structural etching:
[0049] After the silicon wafers are ground and cleaned, photosensitive resin is coated on the surface of each silicon wafer, and the photosensitive resin is exposed and developed using a photolithography machine to form the required pattern. The silicon wafer is then placed in an etching solution and etched according to the photolithography pattern to form the required structure by etching away the unnecessary silicon layer. After etching, the silicon wafer needs to be double-sided ground again to remove surface protrusions and make the surface of the silicon wafer flat.
[0050] S5. Polishing and cleaning:
[0051] The etched and double-sided polished silicon wafer is also called a silicon wafer. The surface of the silicon wafer is polished with a polishing cloth and a polishing slurry to eliminate the mechanical damage left by the previous process to obtain a silicon wafer with a smooth surface. The particle impurities remaining on the surface of the silicon wafer are then removed by cleaning. The particle impurities include organic particle impurities and inorganic particle impurities.
[0052] S6. Quality inspection:
[0053] The thickness, flatness and resistivity of the polished silicon wafer are tested, and the silicon wafer is packaged after the test results are passed. Laser scattering is used to determine the defects and quantity on the surface of the silicon wafer. The silicon wafer passes the test only when the test results meet the preset requirements.
[0054] The preparation process of the high-performance silicon wafer material is applied to the technical field of preparing silicon wafers.
[0055] In summary, if Figure 1As shown, the high-performance silicon wafer material and its preparation process, when used, firstly, the semiconductor rod is vertically fixed by clamps from the upper and lower axes, and a molten zone is generated at one end of the semiconductor rod by using heat energy, and then a single crystal seed crystal is melted, and then the molten zone is slowly moved to the other end of the rod until it passes through the entire rod to grow into a single crystal, i.e., a silicon crystal rod; wherein, the heat energy is generated by electron bombardment, high-frequency induction or optical focusing, and the material in the molten zone is melted and supported by surface tension without falling, and the crystal orientation of the single crystal is the same as that of the seed crystal;
[0056] The silicon crystal rod is taken out, and the cylindrical silicon crystal rod is clamped horizontally and then its two ends are cut and segmented to obtain silicon columns. The two ends of the silicon column are clamped and placed horizontally, and the surface of the silicon column is ground by a grinding device to obtain a silicon column with a precise diameter; wherein, when the silicon column is ground, the silicon column rotates, and the grinding structure grinds it on the top surface of the silicon column, and a pressure sensor group distributed linearly is arranged at the bottom of the silicon column, and a wiping roller structure is arranged on one side of the silicon column. During the grinding, the wiping roller is attached to the side of the silicon column to clean the residue generated by the grinding, and the surface of the silicon column after wiping rotates to the bottom, and the pressure sensor group detects the pressure value in real time. When the pressure sensed by the sensor at each part is within the threshold, it indicates that the diameter of each part of the silicon column has reached the preset size;
[0057] The silicon column is cut at equal intervals to obtain silicon wafers of preset thickness. When cutting, the grinding fixture is first installed at equal intervals. The silicon column is horizontally placed on the top surface of the grinding fixture and clamped at both ends. The cutting steel wire moves vertically from top to bottom, and the silicon column rotates slowly at the same time, so that the steel wire first cuts a wire groove on the surface of the silicon column. As the wire groove deepens, the unseparated silicon wafer sinks so that its edge is stuck in the groove of the grinding fixture, and the effect of grinding the edge of the unseparated silicon wafer is achieved through the rotation of the silicon column. As the steel wire descends, the silicon wafers are completely separated, and then each silicon wafer is taken out and ground on both sides; wherein, a groove is opened on the top surface of the grinding fixture, the groove is arc-shaped to match the curvature of the edge of the silicon wafer, the inner surface of the groove is a grinding surface, and the inner diameter size of the groove on the top surface of the grinding fixture is matched with the preset thickness of the silicon wafer;
[0058] After the silicon wafers are ground and cleaned, photosensitive resin is coated on the surface of each silicon wafer, and the photosensitive resin is exposed and developed using a photolithography machine to form the required pattern. The silicon wafer is then placed in an etching solution and etched according to the photolithography pattern to form the required structure by etching away the unnecessary silicon layer. After etching, the silicon wafer needs to be double-sided ground again to remove surface protrusions and make the surface of the silicon wafer flat.
[0059] The etched and double-sided polished silicon wafer is also called a silicon wafer. The surface of the silicon wafer is polished with a polishing cloth and a polishing slurry to eliminate the mechanical damage left by the previous process to obtain a silicon wafer with a smooth surface. The particle impurities remaining on the surface of the silicon wafer are then removed by cleaning. The particle impurities include organic particle impurities and inorganic particle impurities.
[0060] The thickness, flatness and resistivity of the polished silicon wafer are tested, and the silicon wafer is packaged after the test results are passed. Laser scattering is used to determine the defects and quantity on the surface of the silicon wafer. The silicon wafer passes the test only when the test results meet the preset requirements.
[0061] The embodiments of the present invention are given for the purpose of illustration and description, and are not intended to be exhaustive or to limit the invention to the disclosed forms. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described in order to better illustrate the principles and practical applications of the present invention and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for specific uses.
Claims
1. A high-performance silicon wafer material, characterized by: The raw material of the high-performance silicon wafer material includes a zone melting method silicon crystal rod, which is a silicon crystal rod grown and purified by using a zone melting method to grow semiconductor rod material.
2. The process for preparing a high-performance silicon wafer material according to claim 1, characterized in that: The preparation process comprises the following steps: S1. Silicon crystal rod preparation: First, the semiconductor rod is fixed vertically with a clamp from the upper and lower axes, and the heat energy is used to generate a molten zone at one end of the semiconductor rod, and then the single crystal seed crystal is melted, and then the molten zone is slowly moved to the other end of the rod until it passes through the entire rod to grow into a single crystal, i.e., a silicon crystal rod; S2, outer diameter grinding: The silicon crystal rod is taken out, and the cylindrical silicon crystal rod is clamped horizontally and its two ends are cut into segments to obtain silicon columns. The two ends of the silicon column are clamped and placed horizontally, and the surface of the silicon column is ground by a grinding device to obtain a silicon column with a precise diameter; S3, cutting silicon wafer: The silicon column is cut at equal intervals to obtain silicon wafers of preset thickness. When cutting, the grinding fixture is installed at equal intervals. The silicon column is placed horizontally on the top surface of the grinding fixture and clamped at both ends. The cutting steel wire moves vertically from top to bottom, and the silicon column rotates slowly at the same time, so that the steel wire first cuts a wire groove on the surface of the silicon column. As the wire groove deepens, the unseparated silicon wafer sinks so that its edge is stuck in the groove of the grinding fixture, and the self-rotation of the silicon column achieves the effect of grinding the edge of the unseparated silicon wafer. As the steel wire descends, the silicon wafers are completely separated, and then each silicon wafer is taken out and ground on both sides; S4, structural etching: After the silicon wafers are ground and cleaned, photosensitive resin is coated on the surface of each silicon wafer, and the photosensitive resin is exposed and developed using a photolithography machine to form the required pattern. The silicon wafers are then placed in an etching solution and etched according to the photolithography pattern to form the required structure by etching away the unnecessary silicon layer. S5. Polishing and cleaning: The etched and double-sided polished silicon wafer is also called a silicon wafer. The surface of the silicon wafer is polished with a polishing cloth and polishing slurry, and then the residual particle impurities on the surface of the silicon wafer are removed by cleaning. S6. Quality inspection: The thickness, flatness and resistivity of the polished silicon wafer are tested, and the silicon wafer is packaged after the test results pass.
3. The process for preparing a high-performance silicon wafer material according to claim 2, characterized in that: In the step S1, the heat energy is generated by electron bombardment, high-frequency induction or optical focusing, and the material in the molten zone is melted and supported by surface tension without falling, and the crystal orientation of the single crystal is the same as that of the seed crystal.
4. The process for preparing a high-performance silicon wafer material according to claim 2, characterized in that: In the step S2, the silicon column rotates when it is ground, and the grinding structure grinds it on the top surface of the silicon column. A pressure sensor group distributed linearly is provided at the bottom of the silicon column, and a wiping roller structure is provided on one side of the silicon column. During grinding, the wiping roller is attached to the side of the silicon column to clean the residue produced by grinding. The surface of the silicon column after wiping rotates to the bottom. At this time, the pressure sensor group detects the pressure value in real time. When the pressure sensed by the sensor at each part is within the threshold, it indicates that the diameter of each part of the silicon column has reached the preset size.
5. The process for preparing a high-performance silicon wafer material according to claim 2, characterized in that: In the step S3, a groove is formed on the top surface of the grinding fixture, and the groove is arc-shaped to match the curvature of the edge of the silicon wafer.
6. The process for preparing a high-performance silicon wafer material according to claim 5, characterized in that: The inner surface of the groove is a grinding surface, and the inner diameter of the groove on the top surface of the grinding fixture is adapted to the preset thickness of the silicon wafer.
7. The process for preparing a high-performance silicon wafer material according to claim 2, characterized in that: In the step S4, the silicon wafer needs to be double-sided ground again after etching to remove surface protrusions and make the surface of the silicon wafer flat.
8. The process for preparing a high-performance silicon wafer material according to claim 2, characterized in that: In the step S5, the particulate impurities include organic particulate impurities and inorganic particulate impurities.
9. The process for preparing a high-performance silicon wafer material according to claim 2, characterized in that: In the step S6, laser scattering is used to measure the defects and quantity on the surface of the silicon wafer during the inspection. Only when the inspection results meet the preset requirements can the silicon wafer pass the inspection.
10. A process for preparing a high-performance silicon wafer material according to any one of claims 2 to 9, characterized in that: The preparation process of the high-performance silicon wafer material is applied to the technical field of preparing silicon wafers.