Polyamide-6 super-soft skin-friendly velvet-feeling fiber and preparation method thereof
By adopting low-temperature and low-speed spinning technology and specific treatment methods on nylon 6 fibers, combining natural vegetable oil derivatives and specific surfactants and hydrophilic monomers, the problem of insufficient softness and skin-friendliness in traditional nylon 6 fibers is solved, and the problem of insufficient softness and skin-friendliness is achieved. High-performance, low-cost and environmentally friendly fiber preparation to meet the demands of the high-end market.
Patent Information
- Application Number
- CN202411249241.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional nylon 6 fibers have shortcomings in softness and skin-friendliness. Existing modification methods often sacrifice strength or increase production costs and may introduce unecotched chemicals.
The preparation method of nylon 6 ultra-soft and skin-friendly velvet-sensing fibers includes pretreatment, modification, melt spinning, stretching and cooling, enzyme treatment and low-temperature plasma treatment, and natural vegetable oil derivatives as softeners and fatty alcohol polymerization Sodium oxyethylene ether sulfate or fatty alcohol polyoxyethylene ammonium sulfate as surfactant, polyether modified silicone or hydroxyacrylate as hydrophilic monomer, and fibers are reinforced by low-temperature and low-speed spinning technology and specific treatment methods. Softness and skin-friendly.
It significantly improves the softness and skin-friendliness of the fibers, while maintaining strength and environmental protection. It achieves high performance and low cost through green preparation processes, meeting the needs of the high-end market.
Smart Images

Figure CN118910758A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textile materials, in particular to a nylon 6 ultra-soft, skin-friendly, velvety fiber and a preparation method thereof. Background Art
[0002] Traditional nylon 6 fiber is widely used for its high strength and good wear resistance, but it is insufficient in softness and skin-friendliness, especially in the high-end market that pursues the ultimate wearing experience, which has higher requirements for the softness and skin-friendliness of the fiber.
[0003] In the prior art, although there are attempts to increase the softness of fibers through chemical modification or post-treatment, this often sacrifices the strength of the fibers or increases production costs, and may introduce environmentally unfriendly chemicals. Therefore, it is particularly important to develop a fiber that can maintain the original advantages of nylon 6 while significantly improving its softness and skin-friendliness, as well as a green preparation process. Summary of the invention
[0004] 1. Technical issues to be solved
[0005] In view of the deficiencies in the prior art, the present invention provides a nylon 6 ultra-soft, skin-friendly, velvety fiber and a preparation method thereof, which solves the deficiencies in softness and skin-friendliness of traditional nylon 6 fibers.
[0006] (II) Technical solution
[0007] To achieve the above objectives, the present invention is implemented through the following technical scheme: a nylon 6 ultra-soft skin-friendly velvety fiber, comprising the following components by weight: 20-35 parts of nylon 6, 10-15 parts of softener, 5-10 parts of surfactant, and 5-10 parts of hydrophilic monomer.
[0008] Preferably, the nylon 6 ultra-soft, skin-friendly velvety fiber comprises the following components in parts by weight: 30 parts of nylon 6, 13 parts of softener, 8 parts of surfactant, and 8 parts of hydrophilic monomer.
[0009] Preferably, the softener is a natural plant oil derivative, the surfactant is one of fatty alcohol polyoxyethylene ether sodium sulfate and fatty alcohol polyoxyethylene ether ammonium sulfate, and the hydrophilic monomer is one of polyether modified siloxane and hydroxy acrylate.
[0010] The present invention further discloses a method for preparing a nylon 6 ultra-soft, skin-friendly velvety fiber, comprising the following steps:
[0011] Step 1: Preprocessing:
[0012] Pre-treat nylon 6, including cleaning and drying, to remove impurities and ensure that there are no impurities on the surface of the raw material;
[0013] Step 2: Modification:
[0014] The nylon 6 is polymerized under the action of a catalyst, and a softener, a surfactant, and a hydrophilic monomer in a specific proportion are added, and the modified components are evenly distributed in the nylon 6 matrix through precise metering and uniform mixing to obtain a mixture;
[0015] Step 3: Melt Spinning:
[0016] The mixture is spun at low temperature and low speed to reduce the internal stress of the fiber and avoid hardening caused by high temperature. At the same time, micro-nano-scale bubbles or particles are introduced during the spinning process to increase the void structure inside the fiber and further improve the softness.
[0017] Step 4: Stretch and Cool Down:
[0018] The as-spun fibers are stretched and cooled to form fibers having a nanoscale microporous structure;
[0019] Step 5: Optimization:
[0020] After the fiber is formed, a combination of enzyme treatment and low-temperature plasma treatment is used to remove the hardened layer on the fiber surface and enhance the fiber's fluffiness and skin-friendliness. Enzyme treatment gently improves the fiber surface morphology, while plasma treatment effectively changes the fiber surface energy without using chemical agents, improving its moisture absorption, breathability and biocompatibility;
[0021] Step 6: Post-processing:
[0022] The fibers are post-processed, including shaping and surface treatment, to enhance their softness and skin-friendliness.
[0023] Preferably, in step one, the cleaning and drying steps adopt ultrasonic cleaning and vacuum drying methods to ensure the purity and dryness of the nylon 6 raw material. Specifically, the temperature of the ultrasonic cleaning is 40-60°C and the time is 10-20 minutes, and the temperature of the vacuum drying is 60-80°C and the time is 2-4 hours.
[0024] Preferably, in step 2, the catalyst may be an organic tin catalyst, such as dibutyltin dilaurate, which can effectively promote the polymerization reaction, improve the reaction efficiency and the performance of the product. At the same time, in order to ensure the uniform distribution of the modified components, a high-pressure homogenizer or an ultrasonic mixer may be used to uniformly mix the mixture.
[0025] Preferably, in step 3, in the low-temperature and low-speed spinning technology, the spinning temperature is 200-250°C and the spinning speed is 5-10 m / s, which can ensure both the softness of the fiber and the strength and durability of the fiber. At the same time, the introduction of micro-nano-scale bubbles or particles can be carried out by physical or chemical methods, such as high-pressure gas injection or adding nano-scale particles.
[0026] Preferably, in step 4, the specific conditions of stretching and cooling are:
[0027] In the stretching stage, the fiber is gradually stretched to 2-3 times its original length at a speed of 10-20 meters per minute;
[0028] In the cooling stage, the fiber is cooled to room temperature by cold air at a speed of 5-10 m / s and a temperature of 15-25°C. This method of gradual stretching and cold air cooling ensures that the fiber is evenly stressed during the stretching process, avoiding internal stress while maintaining the softness and shape stability of the fiber.
[0029] Preferably, in step 5, the conditions of the enzyme treatment and low-temperature plasma treatment are:
[0030] During enzyme treatment, appropriate enzyme preparations, such as protease or lipase, are selected, and the treatment temperature and time are controlled to gently improve the fiber surface, remove the hardened layer, and maintain the original structure and properties of the fiber;
[0031] During low-temperature plasma treatment, the power of the plasma generator and the treatment time are controlled to effectively change the fiber surface energy, improve moisture absorption, breathability and biocompatibility. This combined treatment method can retain the softness and skin-friendliness of the fiber to the greatest extent, while improving the surface properties of the fiber.
[0032] Preferably, in step six, the post-treatment uses heat setting technology to stabilize the fiber structure and maintain its ultra-soft and skin-friendly velvety properties by controlling the heating temperature and heating time. Specifically, the heating temperature is set to 100-120°C and the heating time is 1-2 minutes.
[0033] (III) Beneficial effects
[0034] The present invention provides a nylon 6 ultra-soft, skin-friendly, velvety fiber and a preparation method thereof, which has the following characteristics:
[0035] Beneficial effects:
[0036] 1. The present invention uses natural plant oil derivatives as softeners, which not only improves the softness of the fiber, but also ensures the environmental protection and biocompatibility of the fiber. In addition, by selecting specific surfactants and hydrophilic monomers, the skin affinity and moisture absorption and air permeability of the fiber are further enhanced, making the fiber more comfortable when worn.
[0037] 2. The low-temperature and low-speed spinning technology and the method of gradual stretching and cold air cooling adopted by the present invention effectively avoid the hardening phenomenon that may occur in the high-temperature spinning process of the fiber, and maintain the softness and shape stability of the fiber. At the same time, by introducing micro-nano-scale bubbles or particles, the void structure inside the fiber is increased, further improving the softness and fluffiness of the fiber.
[0038] 3. The combination of enzyme treatment and low-temperature plasma treatment in the present invention effectively removes the hardened layer on the fiber surface and enhances the fiber's fluffiness and skin-friendliness. This combined treatment not only retains the fiber's softness and skin-friendliness, but also improves the fiber's surface properties, and improves the fiber's moisture absorption, air permeability, and biocompatibility.
[0039] In summary, the nylon 6 ultra-soft, skin-friendly velvety fiber and the preparation method thereof provided by the present invention have significant advantages and broad application prospects. It not only meets the high requirements of the high-end market for fiber softness and skin-friendliness, but also realizes high performance and low cost of the fiber through a green and environmentally friendly preparation process. Therefore, the present invention has broad application prospects and market potential in the textile field. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 It is a schematic flow chart of the preparation method of the present invention. DETAILED DESCRIPTION
[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] Embodiment 1:
[0043] The embodiment of the present invention provides a nylon 6 ultra-soft, skin-friendly velvety fiber, comprising the following components in parts by weight: 20 parts of nylon 6, 10 parts of softener, 5 parts of surfactant, and 5 parts of hydrophilic monomer.
[0044] The softener is a natural vegetable oil derivative, the surfactant is sodium fatty alcohol polyoxyethylene ether sulfate, and the hydrophilic monomer is polyether modified siloxane.
[0045] like Figure 1 As shown, the embodiment of the present invention also provides a method for preparing nylon 6 ultra-soft skin-friendly velvety fiber, comprising the following steps:
[0046] Step 1: Preprocessing:
[0047] The nylon 6 is pretreated, including cleaning and drying to remove impurities and ensure that there are no impurities on the surface of the raw material; specifically, the cleaning and drying steps adopt ultrasonic cleaning and vacuum drying methods to ensure the purity and dryness of the nylon 6 raw material. Specifically, the ultrasonic cleaning temperature is 40°C and the time is 10 minutes, and the vacuum drying temperature is 60°C and the time is 2 hours.
[0048] Step 2: Modification:
[0049] The nylon 6 is polymerized under the action of a catalyst, and a softener, a surfactant, and a hydrophilic monomer are added in a specific proportion. The modified components are evenly distributed in the nylon 6 matrix through precise metering and uniform mixing to obtain a mixture. Specifically, the catalyst is dibutyltin dilaurate, and the uniform mixing method is to use a high-pressure homogenizer or an ultrasonic mixer to evenly mix the mixture.
[0050] Step 3: Melt Spinning:
[0051] The mixture is spun using low-temperature and low-speed spinning technology to reduce the internal stress of the fiber. At the same time, micro-nano scale bubbles or particles are introduced during the spinning process to increase the void structure inside the fiber, further improve the softness, and obtain primary fibers. Specifically, in the low-temperature and low-speed spinning technology, the spinning temperature is 200°C and the spinning speed is 5 m / s. The method of introducing micro-nano scale bubbles or particles is high-pressure gas injection or adding nano-scale particles.
[0052] Step 4: Stretch and Cool Down:
[0053] The as-spun fibers are stretched and cooled to form fibers with nanoscale microporous structures; specifically, the stretching and cooling conditions are as follows:
[0054] In the stretching stage, the fiber is gradually stretched to twice its original length at a speed of 10 meters per minute;
[0055] In the cooling stage, the fiber is cooled to room temperature by cold air with a speed of 5 m / s and a temperature controlled at 15°C.
[0056] Step 5: Optimization:
[0057] After the fiber is formed, a combination of enzyme treatment and low-temperature plasma treatment is used to remove the hardened layer on the fiber surface and enhance the fiber's fluffiness and skin-friendliness. Specifically, the conditions for enzyme treatment and low-temperature plasma treatment are:
[0058] During enzyme treatment, protease or lipase was selected as the enzyme preparation, the treatment temperature was controlled at 35°C, and the treatment time was 30 minutes;
[0059] During the low-temperature plasma treatment, the power of the plasma generator was controlled to be 100 W and the treatment time was 5 minutes.
[0060] Step 6: Post-processing:
[0061] The fiber is post-processed, including shaping. Specifically, the post-processing adopts heat shaping technology by controlling the heating temperature and heating time. Specifically, the heating temperature is 100° C. and the heating time is 1 minute.
[0062] Embodiment 2:
[0063] The difference between this embodiment and the first embodiment is that the nylon 6 ultra-soft, skin-friendly velvety fiber comprises the following components in parts by weight: 30 parts of nylon 6, 13 parts of softener, 8 parts of surfactant, and 8 parts of hydrophilic monomer.
[0064] The softener is a natural vegetable oil derivative, the surfactant is fatty alcohol polyoxyethylene ether ammonium sulfate, and the hydrophilic monomer is hydroxy acrylate.
[0065] In the preparation method of the nylon 6 ultra-soft, skin-friendly velvety fiber: in step one, the cleaning and drying steps adopt ultrasonic cleaning and vacuum drying methods to ensure the purity and dryness of the nylon 6 raw material. Specifically, the ultrasonic cleaning temperature is 50°C and the time is 15 minutes, and the vacuum drying temperature is 70°C and the time is 3 hours.
[0066] Secondly, in step three, in the low-temperature and low-speed spinning technology, the spinning temperature is 230°C, and the spinning speed is 8 m / s, and the method of introducing micro-nano-scale bubbles or particles is high-pressure gas injection or adding nano-scale particles.
[0067] Secondly, in step 4, the specific conditions for stretching and cooling are:
[0068] In the stretching stage, the fiber is gradually stretched to 2.5 times its original length at a speed of 15 meters per minute;
[0069] In the cooling stage, the fiber is cooled to room temperature by cold air with a speed of 8 m / s and a temperature controlled at 20°C.
[0070] Secondly, in step 5, the conditions for enzyme treatment and low-temperature plasma treatment are:
[0071] During enzyme treatment, protease or lipase was selected as the enzyme preparation, the treatment temperature was controlled at 40°C, and the treatment time was 45 minutes;
[0072] During the low-temperature plasma treatment, the power of the plasma generator was controlled to be 150 W and the treatment time was 8 minutes.
[0073] Secondly, in step six, post-processing adopts heat setting technology by controlling the heating temperature and heating time. Specifically, the heating temperature is 110° C. and the heating time is 1.5 minutes.
[0074] Embodiment three:
[0075] The difference between this embodiment and the first embodiment is that the nylon 6 ultra-soft, skin-friendly velvety fiber comprises the following components in parts by weight: 35 parts of nylon 6, 15 parts of softener, 10 parts of surfactant, and 10 parts of hydrophilic monomer.
[0076] The softener is a natural vegetable oil derivative, the surfactant is fatty alcohol polyoxyethylene ether ammonium sulfate, and the hydrophilic monomer is hydroxy acrylate.
[0077] In the preparation method of the nylon 6 ultra-soft, skin-friendly, velvety fiber: in step one, the cleaning and drying steps adopt ultrasonic cleaning and vacuum drying methods to ensure the purity and dryness of the nylon 6 raw material. Specifically, the ultrasonic cleaning temperature is 60°C and the time is 20 minutes, and the vacuum drying temperature is 80°C and the time is 4 hours.
[0078] Secondly, in step three, in the low-temperature and low-speed spinning technology, the spinning temperature is 250°C, and the spinning speed is 10 m / s, and the method of introducing micro-nano-scale bubbles or particles is high-pressure gas injection or adding nano-scale particles.
[0079] Secondly, in step 4, the specific conditions for stretching and cooling are:
[0080] In the stretching stage, the fiber is gradually stretched to three times its original length at a speed of 20 meters per minute;
[0081] In the cooling stage, the fiber is cooled to room temperature by cold air with a speed of 10 m / s and a temperature controlled at 25°C.
[0082] Secondly, in step 5, the conditions for enzyme treatment and low-temperature plasma treatment are:
[0083] During enzyme treatment, protease or lipase was selected as the enzyme preparation, the treatment temperature was controlled at 45°C, and the treatment time was 60 minutes;
[0084] During the low-temperature plasma treatment, the power of the plasma generator was controlled to be 200 W and the treatment time was 10 minutes.
[0085] Secondly, in step six, post-processing adopts heat setting technology by controlling the heating temperature and heating time. Specifically, the heating temperature is 120° C. and the heating time is 2 minutes.
[0086] Comparative Example:
[0087] The difference between this comparative example and the first embodiment is that the nylon 6 ultra-soft, skin-friendly, velvety fiber comprises the following components in parts by weight: 20 parts of nylon 6 and 5-10 parts of a surfactant.
[0088] Secondly, in the preparation method of nylon 6 ultra-soft skin-friendly velvety fiber, step two and step five are removed.
[0089] Experimental example:
[0090] The performance of the nylon 6 ultra-soft, skin-friendly velvety fibers prepared in Examples 1, 2, 3 and the comparative example was tested, and the results are shown in the following table:
[0091] Example Softness <![CDATA[Air permeability (L / m 2 ·s)]]> Skin-friendly Embodiment 1 excellent 13.8 excellent Embodiment 2 excellent 14.1 excellence Embodiment 3 excellent 13.9 excellent Comparative Example generally 10.9 generally
[0092] It can be seen from the above table that the nylon 6 ultra-soft skin-friendly velvet-feeling fibers prepared in Examples 1, 2, and 3 are superior to the comparative examples in terms of softness, air permeability, and skin-friendliness. This is mainly because softeners, surfactants, and hydrophilic monomers are introduced into the examples, and specific preparation processes (such as low-temperature and low-speed spinning technology, stretching and cooling, enzyme treatment, and low-temperature plasma treatment) are used to make the fibers have the characteristics of ultra-softness, high air permeability, and excellent skin-friendliness.
[0093] For Example 1, Example 2 and Example 3, due to the use of more appropriate proportions of softeners, surfactants and hydrophilic monomers, and the optimization of spinning temperature, stretching multiple, cooling conditions, enzyme treatment and low-temperature plasma treatment conditions during the preparation process, the performance of the fiber is further improved. For example, the air permeability of the fiber in Example 2 is slightly better than that in Example 1 and Example 3.
[0094] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A nylon 6 ultra-soft, skin-friendly velvety fiber, characterized by: The invention comprises the following components by weight: 20-35 parts of nylon 6, 10-15 parts of softener, 5-10 parts of surfactant and 5-10 parts of hydrophilic monomer.
2. The ultra-soft, skin-friendly nylon 6 velvety fiber according to claim 1, characterized in that: The invention comprises the following components in parts by weight: 30 parts of nylon 6, 13 parts of softener, 8 parts of surfactant and 8 parts of hydrophilic monomer.
3. The super soft skin-friendly nylon 6 velvety fiber according to claim 1 or 2, characterized in that: The softener is a natural plant oil derivative, the surfactant is one of fatty alcohol polyoxyethylene ether sodium sulfate and fatty alcohol polyoxyethylene ether ammonium sulfate, and the hydrophilic monomer is one of polyether modified siloxane and hydroxy acrylate.
4. A method for preparing nylon 6 ultra-soft skin-friendly velvety fiber, characterized in that: The following steps are involved: Step 1: Preprocessing: Pre-treat nylon 6, including cleaning and drying, to remove impurities and ensure that there are no impurities on the surface of the raw material; Step 2: Modification: The nylon 6 is polymerized under the action of a catalyst, and a softener, a surfactant, and a hydrophilic monomer in a specific proportion are added, and the modified components are evenly distributed in the nylon 6 matrix through precise metering and uniform mixing to obtain a mixture; Step 3: Melt Spinning: The mixture is spun at low temperature and low speed to reduce the internal stress of the fiber. At the same time, micro-nano-scale bubbles or particles are introduced during the spinning process to increase the void structure inside the fiber and further improve the softness to obtain primary fiber. Step 4: Stretch and Cool Down: The as-spun fibers are stretched and cooled to form fibers having a nanoscale microporous structure; Step 5: Optimization: After the fiber is formed, a combination of enzyme treatment and low-temperature plasma treatment is used to remove the hardened layer on the fiber surface and enhance the fiber's fluffiness and skin-friendliness; Step 6: Post-processing: The fibers are then post-processed, including shaping.
5. The method for preparing the super soft skin-friendly nylon 6 velvety fiber according to claim 4, characterized in that: In step one, the cleaning and drying steps adopt ultrasonic cleaning and vacuum drying methods to ensure the purity and dryness of the nylon 6 raw material. Specifically, the temperature of the ultrasonic cleaning is 40-60°C and the time is 10-20 minutes, and the temperature of the vacuum drying is 60-80°C and the time is 2-4 hours.
6. The method for preparing the super-soft, skin-friendly velvety fiber of nylon 6 according to claim 5, characterized in that: In step 2, the catalyst is dibutyltin dilaurate, and the uniform mixing method is to use a high-pressure homogenizer or an ultrasonic mixer to uniformly mix the mixture.
7. The method for preparing the super soft skin-friendly nylon 6 velvety fiber according to claim 6, characterized in that: In step three, in the low-temperature and low-speed spinning technology, the spinning temperature is 200-250°C, and the spinning speed is 5-10 m / s. The method of introducing micro-nano-scale bubbles or particles is high-pressure gas injection or adding nano-scale particles.
8. The method for preparing the super soft skin-friendly nylon 6 velvety fiber according to claim 7, characterized in that: In step 4, the specific conditions of stretching and cooling are: In the stretching stage, the fiber is gradually stretched to 2-3 times its original length at a speed of 10-20 meters per minute; In the cooling stage, the fiber is cooled to room temperature by cold air with a speed of 5-10 m / s and a temperature controlled at 15-25°C.
9. The method for preparing the super soft skin-friendly nylon 6 velvety fiber according to claim 8, characterized in that: In step 5, the conditions of the enzyme treatment and low-temperature plasma treatment are: During enzyme treatment, protease or lipase is selected as the enzyme preparation, the treatment temperature is controlled at 35-45°C, and the treatment time is 30-60 minutes; During low-temperature plasma treatment, the power of the plasma generator is controlled to be 100-200 W, and the treatment time is 5-10 minutes.
10. The method for preparing the super soft skin-friendly nylon 6 velvety fiber according to claim 9, characterized in that: In step six, the post-treatment adopts heat setting technology by controlling the heating temperature and heating time. Specifically, the heating temperature is 100-120° C. and the heating time is 1-2 minutes.