Preparation method of composite fiber, fabric and mattress

By modifying soybean dregs, high-strength and elastic composite fibers were prepared, which solved the problem of insufficient strength of plant fiber fabrics, and achieved glue-free bonding in the mattress, improving the durability of textiles and human body Security.

CN118910888AInactive Publication Date: 2024-11-08FOSHAN HAOWEI NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410923181.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The strength and elasticity of existing plant fiber fabrics are insufficient, resulting in easy damage to textiles, and the use of a lot of glue on the mattress causes a large odor that is harmful to the human body.

Method used

Soybean slag is used as raw material, and the soybean fiber is modified by combining spandex and second modification aid to improve its compatibility and mechanical properties with spandex, through the treatment and cooking process of the first modification aid and specific pH conditions. Prepare composite fibers with high top breaking strength and elasticity for fabric and mattress production, avoiding glue.

Benefits of technology

It improves the service life of textiles and the mechanical properties of fabrics, reduces potential harm to the human body, and realizes glue-free mattress production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910888A_ABST
    Figure CN118910888A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of textiles, and discloses a preparation method of composite fibers, a fabric and a mattress. The preparation method of the composite fiber comprises the following steps: mixing soybean dregs, water and a first modification additive, adjusting the pH value to 10.5-11.5 for the first time, cooking, cooling after cooking, adding spandex and a second modification additive, stirring, centrifuging to obtain a precipitate, dissolving the precipitate in water, adjusting the pH value to be neutral for the second time, centrifuging, and drying the obtained precipitate to obtain the composite fiber, the first modification additive comprises sodium alginate, potassium carbonate and a silane coupling agent; the second performance additive comprises sodium alginate, sodium dodecyl sulfate, potassium acetate and polyoxyethylene. The prepared composite fiber has high bursting strength and good elasticity, and the composite fiber is applied to the textile field, such as fabrics and mattresses, and the service life of the mattresses can be prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textiles, and in particular relates to a preparation method of composite fibers, fabrics and mattresses. Background Art

[0002] Plant fiber fabrics have good skin-friendliness and are widely used in the textile field.

[0003] However, the existing plant fiber fabrics used for clothing or bedding have good skin affinity, but have poor strength. The existing soybean fiber has low bursting strength, which makes soybean fiber textiles prone to damage and other problems.

[0004] The fabrics used in existing mattresses have problems with poor elasticity and strength. In particular, existing mattresses require a large amount of glue to bond the layers of fabrics. The large amount of glue used results in a strong odor and is very harmful to the human body.

[0005] Therefore, there is an urgent need to provide a new plant fiber with high bursting strength and elasticity, and further, a mattress that does not require the use of glue. Summary of the invention

[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a preparation method of composite fiber, fabric, and mattress. The composite fiber prepared by the preparation method of the present invention has high bursting strength and good elasticity. The composite fiber is applied to the textile field, such as fabric and mattress, which is conducive to improving the service life of the mattress.

[0007] The present invention uses soybean residue as raw material, and is subjected to a first modifying agent, a specific pH condition treatment and a cooking treatment, so that the soybean residue of the present invention is treated to obtain soybean fiber. Then, through the treatment of spandex and a second modifying agent, the compatibility of soybean fiber and spandex can be significantly improved to obtain a composite fiber. When the first modifying agent is added, the soybean residue is cooked, so that the protein in the soybean residue is separated from the fiber, and the fiber strength after separation is strengthened and the fiber surface groups are activated. When the second modifying agent (sodium alginate, sodium dodecyl sulfate, potassium acetate, polyoxyethylene can increase the compatibility of soybean fiber and spandex, and the surface of soybean fiber and spandex fiber is modified to improve the interaction between soybean fiber and spandex) and spandex are added, the performance of spandex is better integrated, so that the composite fiber finally obtained has good mechanical properties.

[0008] A first aspect of the present invention provides a method for preparing a composite fiber.

[0009] Specifically, a method for preparing a composite fiber comprises the following steps:

[0010] Mixing soybean residue, water and a first modifying agent, adjusting the pH to 10.5-11.5 for the first time, steaming, cooling after steaming, adding spandex and a second modifying agent, stirring, centrifuging to obtain a precipitate, dissolving the precipitate in water, adjusting the pH to neutral for the second time, centrifuging, and drying the obtained precipitate to obtain the composite fiber;

[0011] The first modification aid includes sodium alginate, potassium carbonate, and a silane coupling agent;

[0012] The second modification aid includes sodium alginate, sodium dodecyl sulfate, potassium acetate and polyoxyethylene.

[0013] Preferably, the mesh size of the soybean residue is 120-250 mesh, and more preferably 160-200 mesh.

[0014] Preferably, the first modifying aid, by weight, comprises 5-22 parts of sodium alginate, 1-3.2 parts of potassium carbonate, and 3.2-10 parts of silane coupling agent; further preferably, the first modifying aid, by weight, comprises 6-15.2 parts of sodium alginate, 1-2.5 parts of potassium carbonate, and 3-8.5 parts of silane coupling agent.

[0015] Preferably, the second modifying aid, by weight, comprises 4-15.5 parts of sodium alginate, 2-10.5 parts of sodium dodecyl sulfate, 1-8 parts of potassium acetate, and 3-10 parts of polyoxyethylene; further preferably, the second modifying aid, by weight, comprises 4-12 parts of sodium alginate, 2-8 parts of sodium dodecyl sulfate, 1-5 parts of potassium acetate, and 3-9 parts of polyoxyethylene.

[0016] Preferably, the silane coupling agent includes silane coupling agent KH560 or silane coupling agent KH570.

[0017] Preferably, the cooking temperature is 100-115°C, more preferably 110-115°C.

[0018] Preferably, the cooking time is 30-55 minutes, more preferably 45-50 minutes.

[0019] Preferably, the cooling refers to cooling to 40-60°C, more preferably 50-55°C.

[0020] Preferably, the rotation speed during centrifugation is 4000-8000 rpm, more preferably 5000-8000 rpm.

[0021] Preferably, the centrifugation time is 10-20 minutes, more preferably 15-20 minutes.

[0022] Preferably, the drying is spray drying.

[0023] Preferably, the pH is adjusted using sodium hydroxide solution or hydrochloric acid, for example, a sodium hydroxide solution or hydrochloric acid with a concentration of 0.5-1.5 mol / L is used to adjust the pH.

[0024] Preferably, the weight ratio of the soybean residue, water and the first modification aid is 100:(5-50):(0.5-5.5); further preferably, the weight ratio of the soybean residue, water and the first modification aid is 100:(5-40):(0.5-3.5).

[0025] Preferably, the weight ratio of the soybean residue to spandex and the second modifying agent is 100:(1-5.5):(0.5-2.5); further preferably, the weight ratio of the soybean residue to spandex and the second modifying agent is 100:(1-3.5):(0.5-2).

[0026] A second aspect of the present invention provides a composite fiber.

[0027] A composite fiber is prepared by the above preparation method.

[0028] A third aspect of the present invention provides an application of a composite fiber.

[0029] A fabric is obtained by spinning the composite fiber to obtain warp yarns and weft yarns, and the fabric is obtained by weaving the warp yarns and weft yarns.

[0030] A mattress comprises, from bottom to top, a first fabric layer, a first meltblown fabric layer, a bamboo fiber layer, a second meltblown fabric layer, and a second fabric layer;

[0031] The first fabric layer and the second fabric layer are both made of the above-mentioned fabric.

[0032] Preferably, the first meltblown cloth layer and the second meltblown cloth layer are both polypropylene meltblown cloth.

[0033] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0034] The present invention uses soybean residue as raw material, and is subjected to a first modifying agent, a specific pH condition treatment and a cooking treatment, so that the soybean residue of the present invention is treated to obtain soybean fiber. Then, through the treatment of spandex and a second modifying agent, the compatibility of soybean fiber and spandex can be significantly improved to obtain a composite fiber. When the first modifying agent is added, the soybean residue is cooked, so that the protein in the soybean residue is separated from the fiber, and the fiber strength after separation is strengthened and the fiber surface groups are activated. When the second modifying agent (sodium alginate, sodium dodecyl sulfate, potassium acetate, polyoxyethylene can increase the compatibility of soybean fiber and spandex, and the surface of soybean fiber and spandex fiber is modified to improve the interaction between soybean fiber and spandex) and spandex are added, the performance of spandex is better integrated, so that the composite fiber finally obtained has good mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a schematic structural diagram of a mattress of the present invention. DETAILED DESCRIPTION

[0036] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be noted that the following embodiments do not limit the protection scope of the present invention.

[0037] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0038] Example 1

[0039] A method for preparing a composite fiber comprises the following steps:

[0040] The soybean residue, water and the first modifying agent are mixed, the pH value is adjusted to 10.5 for the first time with 1 mol / L sodium hydroxide solution, and the mixture is steamed (autoclaved) at 110°C for 45 minutes. After the steaming, the mixture is cooled to 50°C, and spandex (the fineness of the spandex is 20D and the number of single fibers is 24F) and the second modifying agent are added, and the mixture is stirred for 30 minutes, and then centrifuged (the speed during the centrifugation is 5500 rpm and the centrifugation time is 15 minutes) to obtain a precipitate, which is dissolved in water, and the pH value is adjusted to 7 for the second time with 0.5 mol / L hydrochloric acid, and the mixture is centrifuged (the speed during the centrifugation is 4500 rpm and the centrifugation time is 15 minutes). The obtained precipitate is spray-dried to obtain a composite fiber;

[0041] The first modification aid is composed of the following components by weight: 6 parts of sodium alginate, 2.8 parts of potassium carbonate, and 6 parts of silane coupling agent KH560;

[0042] The second modification aid is composed of the following components by weight: 8 parts of sodium alginate, 4.8 parts of sodium dodecyl sulfate, 1.7 parts of potassium acetate, and 5 parts of polyoxyethylene;

[0043] The weight ratio of soybean residue, water and the first modifying aid is 100:50:1.9.

[0044] The weight ratio of soybean residue to spandex and the second modifying agent is 100:1.1:1.2.

[0045] Example 2

[0046] A method for preparing a composite fiber comprises the following steps:

[0047] The soybean residue, water and the first modifying agent are mixed, the pH value is adjusted to 11 for the first time with 1 mol / L sodium hydroxide solution, and the mixture is steamed (autoclaved) at 105°C for 55 minutes. After the steaming, the mixture is cooled to 50°C, and spandex (the fineness of the spandex is 10D and the number of single fibers is 12F) and the second modifying agent are added, and the mixture is stirred for 30 minutes, and then centrifuged (the speed during the centrifugation is 5500 rpm and the time of the centrifugation is 15 minutes) to obtain a precipitate, which is dissolved in water, the pH value is adjusted to 7 for the second time with 0.5 mol / L hydrochloric acid, and the mixture is centrifuged (the speed during the centrifugation is 4500 rpm and the time of the centrifugation is 15 minutes). The obtained precipitate is spray-dried to obtain a composite fiber;

[0048] The first modification aid is composed of the following components by weight: 6.5 parts of sodium alginate, 2.9 parts of potassium carbonate, and 5.5 parts of silane coupling agent KH570;

[0049] The second modification aid is composed of the following components by weight: 8.5 parts of sodium alginate, 4.9 parts of sodium dodecyl sulfate, 1.6 parts of potassium acetate, and 5.3 parts of polyoxyethylene;

[0050] The weight ratio of soybean residue, water and the first modifying agent is 100:45:1.8.

[0051] The weight ratio of soybean residue to spandex and the second modifying agent is 100:1.2:1.5.

[0052] Example 3

[0053] A method for preparing a composite fiber comprises the following steps:

[0054] The soybean residue, water and the first modifying agent are mixed, the pH value is adjusted to 11 for the first time with 1 mol / L sodium hydroxide solution, and the mixture is steamed (autoclaved) at 110°C for 45 minutes. After the steaming, the mixture is cooled to 50°C, and spandex (the fineness of the spandex is 20D and the number of single fibers is 24F) and the second modifying agent are added, and the mixture is stirred for 30 minutes, and then centrifuged (the speed during the centrifugation is 5500 rpm and the time of the centrifugation is 15 minutes) to obtain a precipitate, which is dissolved in water, the pH value is adjusted to 7 for the second time with 0.5 mol / L hydrochloric acid, and the mixture is centrifuged (the speed during the centrifugation is 5500 rpm and the time of the centrifugation is 15 minutes). The obtained precipitate is spray-dried to obtain a composite fiber;

[0055] The first modification aid is composed of the following components by weight: 8 parts of sodium alginate, 3.2 parts of potassium carbonate, and 6.6 parts of silane coupling agent KH560;

[0056] The second modification aid is composed of the following components by weight: 8.2 parts of sodium alginate, 4.5 parts of sodium dodecyl sulfate, 2.1 parts of potassium acetate, and 5.9 parts of polyoxyethylene;

[0057] The weight ratio of soybean residue, water and the first modifying agent is 100:48:2.1.

[0058] The weight ratio of soybean residue to spandex and the second modifying agent is 100:1.3:1.6.

[0059] Comparative Example 1

[0060] Compared with Example 1, the difference of Comparative Example 1 is that the silane coupling agent KH560 is replaced by an equal amount of sodium alginate in Comparative Example 1, and the pH is adjusted to 9.0 for the first time. The rest of the process is the same as that of Example 1.

[0061] Comparative Example 2

[0062] Compared with Example 1, the difference of Comparative Example 2 is that an equal amount of sodium dodecyl sulfate is used instead of sodium dodecyl sulfonate, and an equal amount of potassium carbonate is used instead of potassium acetate, and the rest of the process is the same as that of Example 1.

[0063] Comparative Example 3

[0064] Compared with Example 1, the difference of Comparative Example 3 is that an equal amount of sodium alginate is used to replace polyethylene oxide, and the pH value is adjusted to 8 for the second time. The rest of the process is the same as that of Example 1.

[0065] Application Example 1

[0066] The composite fiber prepared in the above embodiment 1 is taken and spun to obtain warp yarn and weft yarn. The warp yarn and weft yarn are woven (this process is a conventional process in the field) to obtain a fabric, the imperial count of the warp yarn is 35s, and the imperial count of the weft yarn is 30s; the density of the fabric is 150 warp yarns and 105 weft yarns per square inch.

[0067] Application Example 2

[0068] The composite fiber prepared in Example 2 is taken and spun to obtain warp yarn and weft yarn. The warp yarn and weft yarn are woven (this process is a conventional process in the field) to obtain a fabric, the imperial count of the warp yarn is 35s, and the imperial count of the weft yarn is 30s; the density of the fabric is 150 warp yarns and 105 weft yarns per square inch.

[0069] Comparative Application Examples 1-3

[0070] Compared with Application Example 1, the comparative application examples respectively use the composite fibers of Comparative Examples 1-3 to replace the composite fibers of Example 1, and the remaining processes are the same as those of Application Example 1 to obtain the fabrics corresponding to Comparative Application Examples 1-3.

[0071] Product effect testing

[0072] The bursting strength of the fabrics corresponding to the above application examples 1-2 and comparative application examples 1-3 was tested. The bursting strength was tested with reference to the standard GB / T19976-2005. The results are shown in Table 1.

[0073] Table 1

[0074] Application Example 1 Application Example 2 Comparative application example 1 Comparative Application Example 2 Comparative Application Example 3 Bursting strength(N) 290 284 251 264 272

[0075] It can be seen from Table 1 that the bursting strength of the fabric corresponding to the composite fiber prepared in Examples 1-2 is significantly higher than that of Comparative Examples 1-3. The main reason is that the selection of the components in the first modifying agent and the second modifying agent, as well as the pH value, have a great influence on the modification of the composite fiber surface, thereby affecting the mechanical properties of the fabric.

[0076] Take the fabric prepared in Application Example 1, stretch it in the warp direction of the fabric, and each stretching length is 1.5 times the original length of the fabric in the warp direction. After the fabric corresponding to Application Example 1 is stretched 3000 times, the change rate of the original length of the fabric in the warp direction only increases by 0.8%. When the fabric of Application Example 1 is stretched according to this method, after 3000 times, the change rate of the original length of the fabric in the warp direction increases by 5%.

[0077] It can be seen that the composite fiber prepared in the embodiment of the present invention has good elasticity.

[0078] A mattress comprises, from bottom to top, a first fabric layer, a first meltblown fabric layer, a bamboo fiber layer, a second meltblown fabric layer, and a second fabric layer;

[0079] The first fabric layer and the second fabric layer are both made of the fabric of Example 1.

[0080] The first meltblown cloth layer and the second meltblown cloth layer are both polypropylene meltblown cloth.

[0081] The structure of the above mattress is as follows Figure 1 As shown, 100 represents the first fabric layer, 200 represents the first meltblown fabric layer, 300 represents the bamboo fiber layer, 400 represents the second meltblown fabric layer, and 500 represents the second fabric layer.

[0082] Since the first modifying agent and the second modifying agent are used in the preparation process of the composite fiber of the present invention, as well as the use of spandex, the first fabric layer and the second fabric layer have good affinity with the polypropylene meltblown cloth, and therefore, no additional glue is needed for bonding.

Claims

1. A method for preparing a composite fiber, characterized in that: The following steps are involved: Mixing soybean residue, water and a first modifying agent, adjusting the pH to 10.5-11.5 for the first time, steaming, cooling after steaming, adding spandex and a second modifying agent, stirring, centrifuging to obtain a precipitate, dissolving the precipitate in water, adjusting the pH to neutral for the second time, centrifuging, and drying the obtained precipitate to obtain the composite fiber; The first modification aid includes sodium alginate, potassium carbonate, and a silane coupling agent; The second modification aid includes sodium alginate, sodium dodecyl sulfate, potassium acetate and polyoxyethylene.

2. The preparation method according to claim 1, characterized in that: The first modification aid comprises, by weight, 5-22 parts of sodium alginate, 1-3.2 parts of potassium carbonate, and 3.2-10 parts of a silane coupling agent.

3. The preparation method according to claim 1, characterized in that: The second modification aid comprises, by weight, 4-15.5 parts of sodium alginate, 2-10.5 parts of sodium dodecyl sulfate, 1-8 parts of potassium acetate, and 3-10 parts of polyoxyethylene.

4. The preparation method according to claim 1, characterized in that: The silane coupling agent includes silane coupling agent KH560 or silane coupling agent KH570.

5. The preparation method according to claim 1, characterized in that: The cooking temperature is 100-115°C.

6. The preparation method according to claim 1, characterized in that: The weight ratio of the soybean residue, water and the first modification aid is 100:(5-50):(0.5-5.5).

7. The preparation method according to claim 1, characterized in that: The weight ratio of the soybean residue to the spandex and the second modifying auxiliary agent is 100:(1-5.5):(0.5-2.5).

8. A composite fiber, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 7.

9. A fabric, characterized in that: The composite fiber according to claim 8 is spun into warp yarns and weft yarns, and the fabric is obtained by weaving the warp yarns and weft yarns.

10. A mattress, characterized in that: From bottom to top, it includes the first fabric layer, the first meltblown fabric layer, the bamboo fiber layer, the second meltblown fabric layer, and the second fabric layer; The first fabric layer and the second fabric layer are both made of the fabric described in claim 9.

Citation Information

Patent Citations

  • Method for preparing water-insoluble soy bean dregs dietary fiber using enzyme-alkaline method combined with degreasing

    CN101433292A

  • Fiber mix-using soybean protein fiber and polyamide fiber, and method for producing the same