Preparation method of soft artificial leather

Through composite spinning method and two-step reduction treatment technology, combined with resin composite and surface treatment technology, the problems of poor rebound and low fracture strength of microfiber synthetic leather are solved, and high fracture strength, elasticity and softness are prepared. The microfiber synthetic leather achieves strength, softness and breathable moisture permeability.

CN118910897AActive Publication Date: 2024-11-08SHAOXING FURUITE NEW MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411173956.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-08
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The application of microfiber synthetic leather in boots, clothing and other fields is limited by the problems of poor rebound, low fracture strength and low softness.

Method used

The first and second island microfibers were prepared by composite spinning method, and the composite fiber lines were blended. After two-step reduction treatment and resin composite, combined with dry veneer, surface treatment and other processes, soft artificial leather was produced. .

Benefits of technology

It improves the breaking strength, elasticity and softness of artificial leather, taking into account strength, softness, elasticity and breathable moisture permeability, and obtains good comprehensive performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910897A_ABST
    Figure CN118910897A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of soft artificial leather. The preparation method comprises the following steps: preparing first sea-island superfine fibers and second sea-island superfine fibers by a composite spinning method, preparing base cloth, performing first decrement, performing resin compounding and curing, performing second decrement and performing after-treatment. Two-step reduction treatment is adopted, the first reduction aims to expose part of superfine fibers and increase the contact area of the fibers and resin slurry, so that the combination tightness degree of the fibers and resin is improved, and the breaking strength and rebound resilience of the artificial leather are improved; and the second reduction purpose is to improve the fluffy feeling, softness, air permeability, moisture permeability and other properties of the superfine fiber synthetic leather. Therefore, the artificial leather prepared by the invention has strength, softness, elasticity, air permeability and moisture permeability, and has good comprehensive performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of artificial leather manufacturing, and in particular relates to a method for preparing soft artificial leather. Background Art

[0002] Superfine fiber synthetic leather is a new type of high-end artificial leather made of extremely fine fibers. It is made by blending or composite spinning of sea component and island component polymers, then processed into cloth by non-woven fabric, and then impregnated with polyurethane for coagulation, and the sea component is removed by fiber opening to obtain a superfine fiber leather base cloth with a triple helix structure similar to that of genuine dermal collagen fibers. Finally, it is coated or veneered to obtain highly simulated leather products. Superfine fiber synthetic leather has become a high-end substitute for natural leather due to its high physical properties, durability and softness, and is widely used in various fields such as clothing, shoes, bags, furniture, and automotive interiors. The gaps left after the sea component of the sea island fiber is reduced produce a "release" effect between the island component and polyurethane, which can greatly improve the fluffiness, softness, breathability and moisture permeability of the superfine fiber synthetic leather. However, superfine fiber synthetic leather currently has problems such as poor rebound, low breaking strength, and low softness, which limits its application in boots, clothing and other fields.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] The invention provides a method for preparing soft artificial leather, aiming to provide soft artificial leather with good resilience and high breaking strength.

[0005] The present invention is achieved through the following technical solutions:

[0006] A method for preparing soft artificial leather comprises the following steps:

[0007] Step 1: using a composite spinning method to prepare a first island-in-sea type ultrafine fiber and a second island-in-sea type ultrafine fiber, wherein the first island-in-sea type ultrafine fiber comprises a first island component and a first sea component; and the second island-in-sea type ultrafine fiber comprises a second island component and a second sea component;

[0008] Step 2: blending the first sea-island type ultrafine fiber and the second sea-island type ultrafine fiber to obtain a composite fiber yarn, and then weaving the blended fiber yarn to form a base fabric;

[0009] Step 3: placing the base fabric in a treatment agent solution for a first reduction, the purpose of which is to remove the second sea component, thereby obtaining a partially reduced base fabric;

[0010] Step 4: compounding the partially reduced base fabric with resin by a doctor blade method, and obtaining a sea island microfiber leather precursor after heating and curing;

[0011] Step 5: placing the sea island microfiber leather precursor in a weight reduction treatment liquid for a second weight reduction, and then washing and drying to obtain a microfiber synthetic leather base fabric;

[0012] Step 6: The ultrafine fiber synthetic leather base fabric is processed by at least one post-finishing process including dry veneer, surface treatment, polishing, embossing, water kneading, and ironing to obtain soft artificial leather.

[0013] In some embodiments of the present invention, the second sea component is a water-soluble spinnable polymer or a composition containing a water-soluble spinnable polymer.

[0014] In some embodiments of the present invention, the first island component and the second island component are independently selected from one of the following: polyamide or its derivatives, polyester or its derivatives; wherein the polyamide or its derivatives include at least one of polyamide 6, polyamide 56, polyamide 510, polyamide 511, polyamide 512, polyamide 513, polyamide 514, polyamide 515, polyamide 516 or polyamide copolymers; preferably polyamide 6 and polyamide 56; the polyester or its derivatives include polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate or copolymers of the above polyesters; the polyethylene includes high-density polyethylene, etc.

[0015] In some embodiments of the present invention, the second sea component comprises at least one of polyvinyl pyrrolidone or a combination thereof, polyvinyl alcohol or a combination thereof.

[0016] In some embodiments of the present invention, the first sea component includes at least one of polyester or its derivatives, polyurethane or its derivatives; wherein the polyester or its derivatives include at least one of polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate or copolymers of the above polyesters, high shrinkage polyester (HSPET), and water-soluble copolyester (COPET); the polyurethane or its derivatives include at least one of water-based polyurethane and elastic polyurethane.

[0017] In some embodiments of the present invention, the mass ratio of the first sea component to the first island component is (20:80) to (80:20), preferably (40:60) to (60:40).

[0018] In some embodiments of the present invention, the mass ratio of the second sea component to the second island component is (20:80) to (80:20), preferably (40:60) to (60:40).

[0019] In some embodiments of the present invention, the number of islands of the first sea-island type ultrafine fiber and the second sea-island type ultrafine fiber is independently 16-500, preferably, the number of islands is 37-51.

[0020] In some embodiments of the present invention, in step 2, the mass ratio of the blend of the first island-in-sea type microfiber and the second island-in-sea type microfiber is (90:10) to (50:50), preferably 70:30.

[0021] In some embodiments of the present invention, the treatment agent solution in step three is an alcohol aqueous solution of the treatment agent, and the treatment agent includes at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, phenol, methyl salicylate, and benzenesulfonamide.

[0022] In an optional embodiment, the alcohol water refers to a mixed solution of alcohol and water, wherein the alcohol includes at least one of ethanol, ethylene glycol, propylene glycol, and glycerol; and the volume percentage of alcohol and water in the alcohol water is 10 to 30%.

[0023] In some embodiments of the present invention, the concentration of the treating agent in the treating agent solution in step three is 0.2 to 2 g / L, preferably 0.8 to 1.2 g / L.

[0024] In some embodiments of the present invention, the first reduction refers to ultrasonic treatment at room temperature for 30 to 60 minutes.

[0025] In some embodiments of the present invention, the solid content of the resin slurry in step 4 is 15% to 28%;

[0026] In some embodiments of the present invention, the resin slurry described in step 4, calculated by mass, includes the following components: 20-40 parts of polyurethane prepolymer, 5-20 parts of soy protein isolate, 0.1-0.8 parts of defoaming agent, 0.1-0.8 parts of ultraviolet absorber, 3-8g of curing agent, 0-0.6 parts of dispersant, and 70-350 parts of water.

[0027] In some embodiments of the present invention, the resin in the island microfiber leather precursor in step 4 is 40% to 70% of the weight of the partially reduced base fabric based on the dry weight of the resin slurry.

[0028] In some embodiments of the present invention, the weight reduction treatment liquid is an alkali solution. In an optional embodiment, the temperature of the weight reduction treatment liquid is 50-90° C., and the weight reduction treatment method includes but is not limited to immersion, stirring, ultrasound, roller pressing, etc.

[0029] The present invention has the following advantages and beneficial effects:

[0030] The present invention provides a method for preparing soft artificial leather, which adopts a two-step reduction process, wherein the first reduction is performed before resin compounding, the purpose of which is to expose part of the ultrafine fibers to increase the contact area between the fibers and the resin slurry, thereby improving the tightness of the combination of the fibers and the resin, and further improving the breaking strength and resilience of the artificial leather; the second reduction is performed after the resin compounding, the purpose of which is to produce a "release" effect between the island component and the polyurethane, which can greatly improve the fluffiness, softness, air permeability and moisture permeability of the ultrafine fiber synthetic leather. Therefore, the artificial leather prepared by the present invention can take into account strength, softness, elasticity and air permeability and moisture permeability, and has good comprehensive performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The present invention provides a process flow chart of a method for preparing soft artificial leather. DETAILED DESCRIPTION

[0032] The present invention is further described in detail below in conjunction with specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0033] The present invention provides a method for preparing soft artificial leather. Figure 1 , including the following steps:

[0034] Step 1: using a composite spinning method to prepare a first island-in-sea type ultrafine fiber and a second island-in-sea type ultrafine fiber, wherein the first island-in-sea type ultrafine fiber comprises a first island component and a first sea component; and the second island-in-sea type ultrafine fiber comprises a second island component and a second sea component;

[0035] Step 2: blending the first sea-island type ultrafine fiber and the second sea-island type ultrafine fiber to obtain a composite fiber yarn, and then weaving the blended fiber yarn to form a base fabric;

[0036] Step 3: placing the base fabric in a treatment agent solution for a first reduction, the purpose of which is to remove the second sea component, thereby obtaining a partially reduced base fabric;

[0037] Step 4: compounding the partially reduced base fabric with resin by a doctor blade method, and obtaining a sea island microfiber leather precursor after heating and curing;

[0038] Step 5: placing the sea island microfiber leather precursor in a weight reduction treatment liquid for a second weight reduction, and then washing and drying to obtain a microfiber synthetic leather base fabric;

[0039] Step 6: The ultrafine fiber synthetic leather base fabric is processed by at least one post-finishing process including dry veneer, surface treatment, polishing, embossing, water kneading, and ironing to obtain soft artificial leather.

[0040] The present invention adds a second sea-island type ultrafine fiber when preparing the base fabric of artificial leather, reduces it before resin compounding, removes the second sea component to obtain a partially reduced base fabric, greatly increases the contact area between the fiber and the resin slurry in the base fabric, thereby increasing the bonding tightness between the fiber and the resin, and further increasing the breaking strength and resilience of the obtained artificial leather.

[0041] The present invention adopts a two-step reduction process. The first reduction is performed before resin compounding, with the purpose of exposing part of the ultrafine fibers to increase the contact area between the fibers and the resin slurry, thereby improving the tightness of the combination of the fibers and the resin, and then improving the fracture strength and resilience of the artificial leather; the second reduction is performed after the resin compounding, with the purpose of producing a "release" effect between the island component and the polyurethane, which can greatly improve the fluffiness, softness, breathability and moisture permeability of the ultrafine fiber synthetic leather. Therefore, the technical effect of the present invention cannot be achieved by reducing the amount completely before resin compounding or reducing the amount completely after resin compounding. The reduction before resin compounding will make the artificial leather feel hardened, have low elongation and poor softness; the reduction after resin compounding will make it impossible to improve the fracture strength of the artificial leather. Under the process of the present invention, the obtained artificial leather has good strength, softness and resilience.

[0042] In some embodiments of the present invention, the second sea component is a water-soluble spinnable polymer or a composition containing a water-soluble spinnable polymer; the water-soluble spinnable polymer has two characteristics of water solubility and spinnability, and meets the water-solubility condition so that it can be distinguished from the first sea component, and can achieve weight reduction in a neutral aqueous solution environment, thereby achieving the purpose of reducing the weight before resin composite; meeting the spinnability so that it can adopt a composite spinning method and the second island component adopts a fixed island method for melt spinning; some water-soluble polymers do not meet the spinnability requirements, and need to add additives to improve their spinnability, so the second sea component may be a composition containing a water-soluble spinnable polymer.

[0043] In some embodiments of the present invention, the first island component and the second island component are independently selected from one of the following: polyamide or its derivatives, polyester or its derivatives, polyethylene, polystyrene or polypropylene; wherein the polyamide or its derivatives include at least one of polyamide 6, polyamide 56, polyamide 510, polyamide 511, polyamide 512, polyamide 513, polyamide 514, polyamide 515, polyamide 516 or polyamide copolymers; preferably polyamide 6 and polyamide 56; the polyester or its derivatives include polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate or copolymers of the above polyesters; the polyethylene includes high-density polyethylene, etc.

[0044] In some embodiments of the present invention, the second sea component includes at least one of polyvinyl pyrrolidone or a composition thereof, polyvinyl alcohol or a composition thereof; polyvinyl pyrrolidone and polyvinyl alcohol are both water-soluble spinnable polymers with good water solubility; in some embodiments of the present invention, an auxiliary agent needs to be added to the second sea component to improve the spinning performance of the polymer, so the second sea component sea may be a composition containing the polyvinyl pyrrolidone or polyvinyl alcohol.

[0045] In some embodiments of the present invention, the first sea component includes at least one of polyester or its derivatives, polyurethane or its derivatives; wherein the polyester or its derivatives include at least one of polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate or copolymers of the above polyesters, high shrinkage polyester (HSPET), and water-soluble multi-copolyester (COPET); the polyurethane or its derivatives include at least one of water-based polyurethane and elastic polyurethane.

[0046] It should be noted that, although the names of the listed types of island components and sea components partially overlap, the names are general terms for this type of polymers, including polymers of different viscosities and specifications. Polymers with different specifications and viscosities can be used as sea components or island components respectively, for example, high-density polyethylene can be used as an island component, while linear low-density polyethylene can be used as a sea component; low-viscosity polyester can be used as a sea component, while high-viscosity polyester can be used as an island component; in addition, polymers of the same specifications, when combined with different island or sea components, can be used as sea or island components, for example, polyethylene as a sea component and polyamide as an island component are combined with toluene for reduction, and polyethylene as an island component and polyester as a sea component are combined with alkali solution for reduction; therefore, whether a certain type of polymer is used as a sea component or an island component needs to be determined according to the specific plan.

[0047] In some embodiments of the present invention, the mass ratio of the first sea component to the first island component is (20:80) to (80:20), preferably (40:60) to (60:40).

[0048] In some embodiments of the present invention, the mass ratio of the second sea component to the second island component is (20:80) to (80:20), preferably (40:60) to (60:40).

[0049] The mass ratio of the sea component to the island component has an impact on the mechanical properties, softness and resilience of artificial leather. Specifically, the mass ratio of the second sea component to the second island component affects the partial weight reduction, which in turn affects the degree of bonding between the resin and the fiber, thereby affecting the mechanical properties, softness and resilience of artificial leather; if the sea component is too high, the softness of artificial leather decreases; if the sea component is too low, the breaking strength and resilience of artificial leather decrease.

[0050] In some embodiments of the present invention, the number of islands of the first sea-island type microfiber and the second sea-island type microfiber independently ranges from 16 to 500. Preferably, the number of islands ranges from 37 to 51.

[0051] In some embodiments of the present invention, in step 2, the mass ratio of the blend of the first sea-island type microfiber and the second sea-island type microfiber is (90:10) to (50:50), preferably 70:30.

[0052] In some embodiments of the present invention, the treatment agent solution in step three is an alcohol aqueous solution of the treatment agent, and the treatment agent includes at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, phenol, methyl salicylate, and benzenesulfonamide; the type of the treatment agent is selected according to the type of the island component. Specifically, when the island component is polyamide or a derivative thereof, the treatment agent is preferably N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and benzenesulfonamide; when the island component is polyester or a derivative thereof, the treatment agent is N-methylpyrrolidone, phenol, and methyl salicylate; when the island component is polyolefin, the treatment agent is N,N-dimethylacetamide and phenol.

[0053] In an optional embodiment, the alcohol water refers to a mixed solution of alcohol and water, and the alcohol includes at least one of ethanol, ethylene glycol, propylene glycol, and glycerol; the volume percentage of alcohol and water in the alcohol water is 10-30%.

[0054] In some embodiments of the present invention, the concentration of the treating agent in the treating agent solution in step three is 0.2 to 2 g / L, preferably 0.8 to 1.2 g / L.

[0055] The treatment agent solution provided by the present invention plays a role in partial weight reduction and plasticizing and softening the island component. Specifically, alcohol water is used as a solvent environment to reduce and dissolve the second sea component. The treatment agent can penetrate into the island component fiber according to the principle of like dissolves like to plasticize and soften it, thereby improving the softness and elasticity of the artificial leather. The type of treatment agent and its concentration in the solution affect the performance of the artificial leather. If the concentration of the treatment agent solution is too high, the breaking strength of the artificial leather decreases. If the concentration of the treatment agent solution is too low, the softness and elongation of the artificial leather decrease.

[0056] In some embodiments of the present invention, the first reduction refers to ultrasonic treatment at room temperature for 30 to 60 minutes.

[0057] In some embodiments of the present invention, the solid content of the resin slurry in step 4 is 15% to 28%;

[0058] In some embodiments of the present invention, the resin slurry in step 4 includes the following components, calculated by weight: 20-40 parts of polyurethane prepolymer, 5-20 parts of soy protein isolate, 0.1-0.8 parts of defoaming agent, 0.1-0.8 parts of ultraviolet absorber, 3-8g of curing agent, 0-0.6 parts of dispersant, and 70-350 parts of water;

[0059] In an optional embodiment, the steps of preparing the resin slurry are as follows:

[0060] (1) mixing polyol, polyisocyanate, catalyst and hydrophilic chain extender for reaction, and finally adding neutralizing agent for neutralization to obtain polyurethane prepolymer;

[0061] (2) adding a dispersant and soy protein isolate to the polyurethane prepolymer, stirring evenly, and then adding deionized water and a curing agent to obtain a soy protein modified polyurethane emulsion;

[0062] (3) adding a defoaming agent and an ultraviolet absorber to the soy protein modified polyurethane emulsion, and adding deionized water to adjust the solid content, thereby obtaining a protein modified polyurethane slurry.

[0063] In an optional embodiment, the molar ratio of the polyether polyol, the hydrophilic chain extender and the polyisocyanate is 1:(1-2):(5-6), preferably 1:(1.3-1.7):(5.2-5.5).

[0064] In an optional embodiment, the mass of the catalyst is 1% to 2% of the mass of the polyisocyanate, preferably 1%.

[0065] In an optional embodiment, the polyol includes at least one of polyester polyol, polyether polyol, and a mixed polymer polyol of polyether and polyester. Preferably, the polyol includes at least one of polyethylene glycol, polyoxypropylene glycol, polytetramethylene glycol, polybutylene succinate, and polyhexane adipate.

[0066] In an optional embodiment, the number average molecular weight of the polyol is 1000 to 5000 g / mol, preferably 1200 to 2400 g / mol.

[0067] In an optional embodiment, the polyisocyanate includes at least one of toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), and dicyclohexylmethane diisocyanate (HMDI); preferably, the polyisocyanate includes isophorone diisocyanate (IPDI) and toluene diisocyanate (TDI).

[0068] In an optional embodiment, the catalyst is stannous octoate or dibutyltin dilaurate.

[0069] In an optional embodiment, the hydrophilic chain extender includes at least one of 2,2-dihydroxymethylbutyric acid, dihydroxymethylpropionic acid, sodium ethylenediaminoethanesulfonate, sodium diaminobenzenesulfonate, diaminopropionic acid, diaminobutyric acid, N-methyldiethanolamine, diethanolamine, and triethanolamine; preferably at least one of N-methyldiethanolamine, diethanolamine, and triethanolamine.

[0070] In an optional embodiment, the neutralizing agent is at least one of triethylamine, hydrochloric acid, acetic acid, glycolic acid, and methacrylic acid.

[0071] In an optional embodiment, the curing agent includes at least one of ethylenediamine, hexamethylenediamine, phenylenediamine, diethylenetriamine, and m-phenylenediamine; preferably ethylenediamine.

[0072] In an optional embodiment, the dispersant includes at least one of Tween, alkylphenol polyoxyethylene ether, benzylphenol polyoxyethylene ether, phenethylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, alkyl sulfate, alkyl sulfonate, alkyl naphthalene sulfonate or alkyl benzene sulfonate.

[0073] In some embodiments of the present invention, in step 4, the resin in the island microfiber leather precursor accounts for 40% to 70% of the weight of the partially reduced base fabric based on the dry weight of the resin slurry.

[0074] In some embodiments of the present invention, the weight reduction treatment liquid is an alkali solution, which is determined according to the type of the first sea component. In an optional embodiment, the temperature of the weight reduction treatment liquid is 50-90°C, and the weight reduction treatment method includes but is not limited to immersion, stirring, ultrasound, roller pressing, etc.

[0075] Example 1

[0076] A method for preparing soft artificial leather comprises the following steps:

[0077] Step 1: Preparation of island-type microfibers

[0078] The first sea-island type ultrafine fiber and the second sea-island type ultrafine fiber are prepared respectively according to the following process: the island component and the sea component resin are respectively added to the feeding barrel of the screw extruder for heating and melting, the two melts are transported to the spinning manifold through the melt pipe, and after being accurately measured by the metering pump, they are injected into the sea-island type composite assembly in the spinning manifold, and evenly distributed through the distribution pipe in the assembly. Finally, the two melts are merged and extruded at the entrance of the spinneret; the extruded fibers are cooled, oiled, stretched, shaped, and wound to obtain the sea-island type ultrafine fibers.

[0079] The first sea component of the first sea-island type ultrafine fiber is water-soluble multi-component copolyester (COPET), the first island component is polyamide (PA6), the mass ratio of the sea component to the island component is 40:60, and the number of islands is 37;

[0080] The second sea component of the second sea-island type ultrafine fiber is polyvinyl alcohol, the second island component is polyamide (PA6), the mass ratio of the sea component to the island component is 50:50, and the number of islands is 37;

[0081] The screw temperatures of the first island component and the second island component are as follows: Zone 1 230°C → Zone 2 250°C → Zone 3 270°C → Zone 4 290°C → Zone 5 280°C;

[0082] The screw temperature of the first sea component is as follows: Zone 1 180°C → Zone 2 220°C → Zone 3 240°C → Zone 4 260°C → Zone 5 240°C;

[0083] The screw temperature of the second sea component is as follows: Zone 1 120°C → Zone 2 150°C → Zone 3 170°C → Zone 4 190°C → Zone 5 170°C;

[0084] Side blowing is used for cooling, with a wind speed of 0.6 m / s and a wind temperature of 25°C; the amount of oil applied is 0.5 wt% of the fiber; the stretching multiple is 2.5, the setting temperature is 160°C, and the winding speed is 2500 m / min.

[0085] Step 2: Prepare the base fabric

[0086] The first sea-island type ultrafine fiber and the second sea-island type ultrafine fiber are mixed in a mass ratio of 70:30, and are opened, carded, and spun to obtain a composite fiber line, which is used as warp and weft to form a base fabric through plain weaving.

[0087] Step 3: Prepare partially reduced base fabric

[0088] The obtained base fabric was placed in a treatment agent solution for ultrasonic treatment for 60 minutes with a bath ratio of 1:30, then taken out and soaked in normal temperature water for washing for 5 minutes and the washing step was repeated 3 times to obtain a partially reduced base fabric, and the moisture content of the partially reduced base fabric was controlled to be less than 20% by hanging drying.

[0089] The treatment agent solution is an alcohol aqueous solution of benzenesulfonamide with a benzenesulfonamide concentration of 1 g / L.

[0090] The alcohol is ethanol, and the volume ratio of ethanol to water is 20%:1.

[0091] Step 4: Preparation of island microfiber leather precursor

[0092] A resin slurry is scraped on the surface of a portion of the reduced base fabric using a roller coater. The resin slurry includes the following components: 30 parts of polyurethane prepolymer, 12 parts of soy protein isolate, 0.5 parts of silicone defoamer, 0.4 parts of ultraviolet absorber UV-326, 5g of ethylenediamine, and 210 parts of water.

[0093] The resin slurry preparation method is as follows:

[0094] (1) Under nitrogen protection, 60 g of polytetramethylene glycol (number average molecular weight of 2000 g / mol), 34.5 g of isophorone diisocyanate, 0.35 g of dibutyltin dilaurate, and 4.65 g of N-methyldiethanolamine were mixed and heated to 80° C. and stirred for reaction until the NCO content reached a stable level. Hydrochloric acid was added for neutralization to obtain a polyurethane prepolymer.

[0095] (2) Add soy protein isolate to the polyurethane prepolymer, stir evenly, add deionized water, and finally add ethylenediamine, and shear and disperse for 1 hour to obtain a soy protein modified polyurethane emulsion.

[0096] (3) adding an organosilicon defoamer and an ultraviolet absorber to the soy protein modified polyurethane emulsion, stirring and mixing at 800 rpm, and then adding deionized water to control the solid content to 18%, thereby obtaining a resin slurry.

[0097] The resin in the obtained sea island microfiber leather precursor accounts for 57% of the weight of the partially reduced base fabric based on the dry weight of the slurry.

[0098] The heating and drying temperature was 120°C.

[0099] Step 5: Preparation of microfiber synthetic leather base fabric

[0100] The sea island microfiber leather precursor was placed in a 3% sodium hydroxide aqueous solution at a temperature of 50°C for 45 minutes with a bath ratio of 1:20, and then washed with water to neutrality and dried at 130°C to obtain a microfiber synthetic leather base cloth.

[0101] Step 6: Prepare the artificial leather

[0102] The ultrafine fiber synthetic leather base fabric is processed through dry veneer, surface treatment, polishing, embossing, water kneading and ironing to produce soft artificial leather.

[0103] Example 2

[0104] A method for preparing soft artificial leather comprises the following steps:

[0105] Step 1: Preparation of island-type microfibers

[0106] The difference from Example 1 is that the first sea component of the first sea-island type ultrafine fiber is water-soluble multi-component copolyester (COPET), the first island component is high-density polyethylene, the mass ratio of the sea component to the island component is 30:70, and the number of islands is 51;

[0107] The second sea component of the second sea-island type ultrafine fiber is polyvinyl alcohol, the second island component is polyamide (PA56), the mass ratio of the sea component to the island component is 70:30, and the number of islands is 37;

[0108] The screw temperatures of the first island component are as follows: zone 1 200°C → zone 2 220°C → zone 3 240°C → zone 4 265°C → zone 5 260°C;

[0109] The screw temperatures of the second island component are as follows: Zone 1 230°C → Zone 2 250°C → Zone 3 270°C → Zone 4 290°C → Zone 5 285°C;

[0110] The screw temperature of the first sea component is as follows: Zone 1 180°C → Zone 2 220°C → Zone 3 240°C → Zone 4 260°C → Zone 5 240°C;

[0111] The screw temperature of the second sea component is as follows: Zone 1 120°C → Zone 2 150°C → Zone 3 170°C → Zone 4 190°C → Zone 5 170°C;

[0112] Step 2: Prepare the base fabric

[0113] Same as Example 1.

[0114] Step 3: Prepare partially reduced base fabric

[0115] The difference from Example 1 is that:

[0116] The treatment agent solution is an alcohol aqueous solution of N-methylpyrrolidone with a concentration of 1 g / L.

[0117] The alcohol is ethylene glycol, and the volume ratio of ethylene glycol to water is 10%:1.

[0118] Step 4: Preparation of island microfiber leather precursor

[0119] A roller coater is used to scrape resin slurry on the surface of a portion of the weight-reduced base fabric. The resin slurry includes the following components: 20 parts of polyurethane prepolymer, 5 parts of soy protein isolate, 0.1 parts of silicone defoamer, 0.1 parts of ultraviolet absorber UV-326, 3 parts of hexamethylenediamine, 0.2 parts of Tween-80, and 70 parts of water.

[0120] The resin slurry preparation method is as follows:

[0121] (1) Under nitrogen protection, 30 g of poly(hexanediol adipate) (number average molecular weight of 3000 g / mol), 18 g of polyethylene glycol (number average molecular weight of 1200 g / mol), 24 g of toluene diisocyanate, 0.24 g of stannous octoate, and 3.5 g of diethanolamine were mixed and heated to 80° C. and stirred for reaction until the NCO content reached a stable level. Acetic acid was added for neutralization to obtain a polyurethane prepolymer.

[0122] (2) Add dispersant Tween-80 and soy protein isolate to the polyurethane prepolymer, stir evenly, add deionized water, and finally add hexamethylenediamine for shear dispersion for 1 hour to obtain a soy protein modified polyurethane emulsion.

[0123] (3) adding an organosilicon defoamer and an ultraviolet absorber to the soy protein modified polyurethane emulsion, stirring and mixing at 800 rpm, and then adding deionized water to control the solid content to 28%, thereby obtaining a resin slurry.

[0124] The resin in the obtained sea island microfiber leather precursor accounts for 70% of the weight of the partially reduced base fabric based on the dry weight of the slurry.

[0125] The heating and drying temperature was 120°C.

[0126] Step 5: Preparation of microfiber synthetic leather base fabric

[0127] The sea island microfiber leather precursor was placed in a 3% sodium hydroxide aqueous solution at a temperature of 50°C for 45 minutes with a bath ratio of 1:20, and then washed with water to neutrality and dried at 130°C to obtain a microfiber synthetic leather base cloth.

[0128] Step 6: Prepare the artificial leather

[0129] The ultrafine fiber synthetic leather base fabric is processed through dry veneer, surface treatment, polishing, embossing, water kneading and ironing to produce soft artificial leather.

[0130] Example 3

[0131] A method for preparing soft artificial leather comprises the following steps:

[0132] Step 1: Preparation of island-type microfibers

[0133] The difference from Example 1 is that the first sea component of the first sea-island type ultrafine fiber is water-soluble multi-component copolyester (COPET), the first island component is high-density polyethylene, the mass ratio of the sea component to the island component is 20:80, and the number of islands is 51;

[0134] The second sea component of the second sea-island type ultrafine fiber is polyvinyl pyrrolidone, the second island component is high-density polyethylene, the mass ratio of the sea component to the island component is 80:20, and the number of islands is 37;

[0135] The screw temperatures of the first and second island components are as follows: Zone 1 200°C → Zone 2 220°C → Zone 3 240°C → Zone 4 265°C → Zone 5 260°C;

[0136] The screw temperature of the first sea component is as follows: Zone 1 180°C → Zone 2 220°C → Zone 3 240°C → Zone 4 260°C → Zone 5 240°C;

[0137] The screw temperature of the second sea component is as follows: Zone 1 150°C → Zone 2 170°C → Zone 3 190°C → Zone 4 220°C → Zone 5 210°C;

[0138] Step 2: Prepare the base fabric

[0139] Same as Example 1.

[0140] Step 3: Prepare partially reduced base fabric

[0141] The difference from Example 1 is that:

[0142] The treatment agent solution is an alcohol aqueous solution of butyl salicylate with a butyl salicylate concentration of 1 g / L.

[0143] The alcohol is propylene glycol, and the volume ratio of the alcohol to water is 30%:1.

[0144] Step 4: Prepare sea island microfiber leather precursor.

[0145] A roller coater is used to scrape resin slurry on the surface of a portion of the reduced base fabric. The resin slurry includes the following components: 40 parts of polyurethane prepolymer, 20 parts of soy protein isolate, 0.8 parts of silicone defoamer, 0.8 parts of ultraviolet absorber UV-326, 8 parts of ethylenediamine, 0.6 parts of fatty alcohol polyoxyethylene ether AEO-3, and 350 parts of water.

[0146] The resin slurry preparation method is as follows:

[0147] (1) Under nitrogen protection, 30 g of poly(hexane adipate) (number average molecular weight of 4000 g / mol), 35 g of poly(oxypropylene glycol) (number average molecular weight of 2000 g / mol), 34 g of dicyclohexylmethane diisocyanate, 0.34 g of stannous octoate, and 6.3 g of triethanolamine were mixed and heated to 80° C. and stirred for reaction until the NCO content reached a stable level. Hydrochloric acid was added for neutralization to obtain a polyurethane prepolymer.

[0148] (2) Add dispersant AEO-3 and soy protein isolate to the polyurethane prepolymer, stir evenly, add deionized water, and finally add ethylenediamine for shear dispersion for 1 hour to obtain a soy protein modified polyurethane emulsion.

[0149] (3) adding an organosilicon defoamer and an ultraviolet absorber to the soy protein modified polyurethane emulsion, stirring and mixing at 800 rpm, and then adding deionized water to control the solid content to 15%, thereby obtaining a resin slurry.

[0150] The resin in the obtained sea island microfiber leather precursor accounts for 40% of the weight of the partially reduced base fabric based on the dry weight of the slurry.

[0151] The heating and drying temperature was 120°C.

[0152] Step 5: Preparation of microfiber synthetic leather base fabric

[0153] The sea island microfiber leather precursor was placed in a 3% sodium hydroxide aqueous solution at a temperature of 50°C for 45 minutes with a bath ratio of 1:20, and then washed with water to neutrality and dried at 130°C to obtain a microfiber synthetic leather base cloth.

[0154] Step 6: Prepare the artificial leather

[0155] The ultrafine fiber synthetic leather base fabric is processed through dry veneer, surface treatment, polishing, embossing, water kneading and ironing to produce soft artificial leather.

[0156] Example 4

[0157] The difference from Example 1 is that in step 2: the first sea-island type ultrafine fiber and the second sea-island type ultrafine fiber are mixed in a mass ratio of 90:10 to blend and prepare a composite fiber line.

[0158] Example 5

[0159] The difference from Example 1 is that in step 2: the first sea-island type ultrafine fiber and the second sea-island type ultrafine fiber are mixed in a mass ratio of 50:50 to blend and prepare a composite fiber line.

[0160] Example 6

[0161] The difference from Example 1 is that in step 3, the treatment agent solution is an alcohol aqueous solution of benzenesulfonamide with a benzenesulfonamide concentration of 0.2 g / L.

[0162] Example 7

[0163] The difference from Example 1 is that in step three, the treatment agent solution is an alcohol aqueous solution of benzenesulfonamide with a benzenesulfonamide concentration of 2 g / L.

[0164] Comparative Example 1

[0165] The difference from Example 1 is that step three is not performed, that is, the base fabric prepared in step two is directly subjected to resin compounding and curing to obtain the island microfiber leather precursor, and then the weight reduction is performed in step four.

[0166] Therefore, the components reduced in step 4 include the first sea component and the second sea component.

[0167] Comparative Example 2

[0168] The difference from Example 1 is that the second sea-island type ultrafine fiber is not added in step 2, that is, the first sea-island type ultrafine fiber is used as the warp and weft yarns to weave the base fabric.

[0169] Comparative Example 3

[0170] The difference from Example 1 is that the first sea component and the second sea component of the base fabric are both reduced in step 3, so step 5 is not performed. The specific steps are as follows:

[0171] Step 1 and step 2 are the same as in Example 1;

[0172] Step 3: Place the obtained base fabric into a 50°C treatment agent solution for ultrasonic treatment for 60 minutes with a bath ratio of 1:30, then take it out and soak it in normal temperature water for 5 minutes and repeat the washing step 5 times to obtain a reduced base fabric. The moisture content of the reduced base fabric is controlled to be less than 20% by hanging drying.

[0173] The solvent of the treatment agent solution is an ethanol aqueous solution (the volume ratio of ethanol to water is 20%:1), and the components of the treatment agent solution include: 1g / L benzenesulfonamide and 30g / L NaOH.

[0174] Step 4 and step 6 are the same as those in Example 1.

[0175] Comparative Example 4

[0176] The difference from Example 1 is that in step 3, no treatment agent is added, that is, an alcohol-water solution is used to perform the first weight reduction on the base fabric.

[0177] Comparative Example 5

[0178] The difference from Example 1 is that in step 3, the treatment agent benzenesulfonamide is not added, and in step 5, the treatment agent benzenesulfonamide is added, that is, the base fabric is subjected to the first reduction using an alcohol aqueous solution, and the treatment agent benzenesulfonamide is added to the reduction treatment solution in step 5 for the second reduction.

[0179] The solvent of the reduction treatment liquid in step five is water, and the components of the reduction treatment liquid include: 1 g / L benzenesulfonamide and 30 g / L NaOH.

[0180] The artificial leathers prepared in the examples and comparative examples were subjected to performance tests.

[0181] Test Example 1

[0182] The softness of artificial leather was evaluated according to the standard NF G52-033-2012 "Determination of softness of leather by physical and mechanical tests". The test used a shrink ring with a diameter of 35 mm.

[0183] Test Example 2

[0184] The flexural rigidity of artificial leather was tested according to the standard GB / T 18318.1-2009 “Determination of flexural properties of textiles Part 1: Inclined plane method”.

[0185] Test Example 3

[0186] The mechanical properties of artificial leather were tested according to the standard GB / T24218.3-2010 "Test methods for textile nonwovens Part 3: Determination of breaking strength and elongation at break (strip method)", the breaking strength and elongation of the test sample were tested at a gauge of 20 cm and a tensile speed of 100 mm / min.

[0187] Test Example 4

[0188] The stretching rebound speed of artificial leather was tested, and the following two indicators were specifically measured: ① the recovery rate 1s after the warp elongation was 10%; ② the recovery rate 1s after the weft elongation was 30%; the measurement method of the above two indicators is as follows: prepare the cloth sample, put it into the clamp of the tensile machine from the warp and weft directions respectively, with a spacing of 20cm and a stretching speed of 100mm / min. Release one side of the clamp after the elongation of the warp stretch reaches 10% or the elongation of the weft stretch reaches 30%, record the process with a camera, and analyze and calculate the elongation of the cloth sample 1s after release relative to before stretching.

[0189] The test results of Test Examples 1 to 4 are listed in Table 1.

[0190] Table 1

[0191]

[0192] From the results in Table 1, it can be seen that in Comparative Example 1, since the base fabric is not partially opened by the treatment agent solution before resin compounding, the obtained artificial leather has lower softness and strength than that in Example 1. By comparing Examples 1, 4, 5 and Comparative Example 2, it can be seen that the ratio of the first sea island microfiber to the second sea island microfiber in the base fabric has an impact on the softness and mechanical strength of the artificial leather. Specifically, the higher the proportion of the second sea island microfiber, the lower the softness of the artificial leather. The reason is that: the excessively high proportion of the second sea island microfiber leads to a higher degree of partial opening, a higher degree of bonding between the resin slurry and the fiber, and the limited mobility of the resin layer, thereby reducing the softness of the artificial leather and making it feel hard. The higher the proportion of the second sea island microfiber, the breaking strength of the artificial leather shows a trend of increasing first and then decreasing. The reason is that the higher the proportion of the second sea island microfiber, the higher the degree of partial fiber opening, and the higher the degree of bonding between the resin slurry and the fiber. Therefore, the higher the strength of the artificial leather, the lower the elongation at break; but the proportion of the second sea island microfiber is too high, resulting in the lower content of the island component and the less fiber content in the artificial leather, which leads to the decrease in the strength of the artificial leather and the increase in the elongation at break. The higher the proportion of the second sea island microfiber, the elongation at break of the artificial leather first increases and then decreases. The reason is that the higher the proportion of the second sea island microfiber, the higher the degree of fiber opening of the artificial leather as a whole, and the lower the island content, which leads to the enhancement of the activity of the leather and the increase of the elongation at break. However, the proportion of the second sea island microfiber is too high, resulting in the excessive degree of bonding between the resin slurry and the fiber, which in turn limits the activity of the leather and leads to a decrease in the elongation at break.

[0193] Comparative Example 1 and Comparative Example 3, the base cloth is completely opened and then resin compounded, resulting in the resin slurry and the fiber being too tightly bonded, and the mobility of the resin layer is limited, thereby reducing the softness of the artificial leather and making it feel stiff. At the same time, the resulting artificial leather has a high breaking strength and a low breaking elongation.

[0194] By comparing Examples 1, 6, 7 and Comparative Example 4, it can be seen that the higher the concentration of the treating agent in the treating agent solution, the higher the softness of the artificial leather but the lower the breaking strength, and the higher the breaking elongation. The reason is that the treating agent has a plasticizing effect on the island component, which can increase the activity of the island component molecular chain, thereby improving the softness of the artificial leather, thereby reducing its breaking strength and increasing its breaking elongation.

[0195] By comparing Example 1 and Comparative Example 5, it can be seen that the treatment agent is added when the fibers are opened after resin compounding, which has a better effect on improving the softness of the artificial leather, but reduces the mechanical strength of the artificial leather. The reason is that the treatment agent also has a certain degree of softening effect on the resin layer, which reduces the mechanical strength of the artificial leather.

[0196] The present invention evaluates the elasticity of artificial leather from two dimensions. On the one hand, it lies in the elongation of artificial leather, which reflects the deformation ability of the material; on the other hand, it lies in the rebound speed of artificial leather after stretching, which reflects the ability of the material to return to its original state after being subjected to force. The present invention evaluates the rebound speed of artificial leather by the recovery rate of 1s after the warp elongation is 10% and the recovery rate of 1s after the weft elongation is 30%. Analysis of the data in Table 1 shows that the higher the proportion of the second sea island microfiber, the rebound speed of artificial leather shows a trend of first increasing and then decreasing. The reason is that the higher the proportion of the second sea island microfiber, the higher the degree of partial fiber opening, the higher the degree of bonding between the resin slurry and the fiber, the worse the activity of the artificial leather structure, and the rigid rebound, so the rebound speed is faster; when the proportion of the second sea island microfiber is too high, the island component content decreases, the activity of the artificial leather structure increases, the rigidity of the material is lower, and the rebound speed slows down. The higher the concentration of the treating agent in the treating agent solution, the slower the rebound speed of the artificial leather, because as the concentration of the treating agent increases, the rigidity of the artificial leather decreases, and thus the rebound speed becomes slower.

[0197] Test Example 5

[0198] The air permeability of artificial leather was tested according to the standard GB / T 24218.15-2018 "Test methods for textile nonwovens Part 15: Determination of air permeability". The experimental pressure difference was 100Pa and the test area was 20cm 2 .

[0199] Test Example 6

[0200] The moisture permeability of artificial leather was tested according to the standard FZ / T 98020-2019 "Fabric Moisture Permeability Tester". The test environment temperature was (38±2)℃ and the humidity was (50±2)%. The moisture permeability was calculated as follows: Where m1 and m0 are the masses of the sample before and after the test, respectively, in g; A is the effective test area of ​​the sample, in m 2 ; T is the test time, in hours.

[0201] The present invention tests the air permeability and moisture permeability of Example 1 and Comparative Examples 1 to 5, and the results are listed in Table 2.

[0202] Table 2

[0203] sample <![CDATA[Air permeability, L·(m 2 ·s) -1 > <![CDATA[Water vapor transmission rate, g·(m 2 ·h) -1 <!-- 12 -->]]> Example 1 27 202 Comparative Example 1 28 213 Comparative Example 2 26 206 Comparative Example 3 20 172 Comparative Example 4 27 211 Comparative Example 5 25 197

[0204] It can be seen from the data in Table 2 that the air permeability and moisture permeability of Comparative Example 1 is greater than that of Example 1. The reason is that in Example 1, the resin and the fiber are more tightly combined and the bonding area is larger, so the obtained artificial leather has better mechanical properties but sacrifices some air permeability and moisture permeability; the base fabric of Comparative Example 2 does not contain the second sea island ultrafine fiber. Since the content of the island component in the final artificial leather is higher than that in Example 1 and Comparative Example 1, the air permeability and moisture permeability is slightly lower; Comparative Example 3 reduces all sea components before resin compounding, so the air permeability and moisture permeability are the worst; Comparative Example 4 does not add a treatment agent during the first reduction, but it has little effect on the air permeability and moisture permeability of the artificial leather; In Comparative Example 5, the treatment agent is added only during the second reduction, which reduces the air permeability and moisture permeability of the artificial leather.

[0205] The above contents are further detailed descriptions of the present invention in combination with specific preferred technical solutions, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For professionals and technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention.

Claims

1. A method for preparing soft artificial leather, characterized in that: The following steps are involved: Step 1: using a composite spinning method to prepare a first island-in-sea type ultrafine fiber and a second island-in-sea type ultrafine fiber, wherein the first island-in-sea type ultrafine fiber comprises a first island component and a first sea component; and the second island-in-sea type ultrafine fiber comprises a second island component and a second sea component; Step 2: blending the first sea-island type ultrafine fiber and the second sea-island type ultrafine fiber to obtain a composite fiber yarn, and then weaving the blended fiber yarn to form a base fabric; Step 3: placing the base fabric in a treatment agent solution for a first reduction, the purpose of which is to remove the second sea component, thereby obtaining a partially reduced base fabric; Step 4: compounding the partially reduced base fabric with resin by a doctor blade method, and obtaining a sea island microfiber leather precursor after heating and curing; Step 5: placing the sea island microfiber leather precursor in a weight reduction treatment liquid for a second weight reduction, and then washing and drying to obtain a microfiber synthetic leather base fabric; Step 6: The ultrafine fiber synthetic leather base fabric is processed by at least one post-finishing process including dry veneer, surface treatment, polishing, embossing, water kneading, and ironing to obtain soft artificial leather.

2. The preparation method according to claim 1, characterized in that: The second sea component is a water-soluble spinnable polymer or a composition containing a water-soluble spinnable polymer.

3. The preparation method according to claim 1 or 2, characterized in that: The step 1 has at least one of the following characteristics: Feature 1: The first island component and the second island component are independently selected from one of the following: polyamide or its derivatives, polyester or its derivatives, polystyrene, polyethylene or polypropylene; Feature 2: The second sea component comprises at least one of polyvinyl pyrrolidone or a combination thereof, polyvinyl alcohol or a combination thereof; Feature 3: The first sea component includes at least one of polyester or its derivatives, polyurethane or its derivatives; Feature 4: The mass ratio of the first sea component to the first island component is (20:80) to (80:20); Feature 5: The mass ratio of the second sea component to the second island component is (20:80) to (80:20); Feature 6: The number of islands of the first sea-island type ultrafine fiber and the second sea-island type ultrafine fiber independently ranges from 16 to 500.

4. The preparation method according to claim 1, characterized in that: In the step 2, the mass ratio of the blended first sea-island type ultrafine fiber and the second sea-island type ultrafine fiber is (90:10) to (50:50).

5. The preparation method according to any one of claims 1 to 3, characterized in that: The treatment agent solution is an alcohol aqueous solution of the treatment agent, and the treatment agent includes at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, phenol, methyl salicylate, and benzenesulfonamide.

6. The preparation method according to any one of claims 1 or 5, characterized in that: The concentration of the treating agent in the treating agent solution is 0.2-2 g / L.

7. The preparation method according to claim 1, characterized in that: The first reduction refers to ultrasonic treatment at room temperature for 30 to 60 minutes.

8. The preparation method according to claim 1, characterized in that: The resin slurry in step 4 has at least one of the following characteristics: Feature 7: The solid content of the resin slurry is 15%~28%; Feature 8: The resin slurry, calculated by mass, includes the following components: 20-40 parts of polyurethane prepolymer, 5-20 parts of soy protein isolate, 0.1-0.8 parts of defoaming agent, 0.1-0.8 parts of ultraviolet absorber, 3-8g of curing agent, 0-0.6 parts of dispersant, and 70-350 parts of water.

9. The preparation method according to claim 1, characterized in that: In step 4, the resin in the island microfiber leather precursor accounts for 40% to 70% of the weight of the partially reduced base fabric based on the dry weight of the resin slurry.

10. The preparation method according to claim 1, characterized in that: The weight reduction treatment liquid is an alkali solution.

Citation Information

Patent Citations

  • Elastic superfine fiber synthetic leather and environmentally friendly preparation method thereof

    CN107604533A

  • Production process of sheepskin-imitated gold-stamped sofa fabric

    CN115233454A

  • Production of woven or knitted fabric having good touch feeling

    JP1997067765A

  • Suede style knitted fabric and manufacturing method thereof

    KR1020000002238A

  • Y-shaped rayon fiber and method for producing it

    KR1020020080828A

Cited By

  • High-fluffiness sea island-high-shrinkage polyester composite filament and preparation method thereof

    CN122039289A

  • High loft sea island - high shrinkage polyester composite filament and method of making same

    CN122039289B