Bacteriostatic nano composite hydrogel and preparation method thereof

By designing antibacterial nanocomposite hydrogels, using the combination of polymer substrates, magnetic nanoparticles and surface modifiers, the problems of poor adsorption selectivity and poor mechanical properties in complex water bodies are solved, and high efficiency is achieved , stable pollutant removal and long-term use, suitable for water purification in multiple fields.

CN118909406APending Publication Date: 2024-11-08NANJING HENGZHOU TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411159333.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When facing complex water bodies, existing water treatment methods are difficult to take into account both efficient adsorption and long-term stability. The traditional hydrogel has a single structure and insufficient functionalization, so it is impossible to effectively distinguish and treat different types of pollutants.

Method used

Using an antibacterial nanocomposite hydrogel, its composition includes polymer substrate, magnetic nanoparticles, crosslinking agents and surface modification agents. Through core-shell structure and multi-layer pore structure design, combined with chemical modification technology, the counter-heavy metal is improved. , removal efficiency of organic pollutants and microorganisms.

Benefits of technology

It significantly improves the removal efficiency of heavy metals, organic dyes and microorganisms, enhances mechanical properties and regeneration capabilities, and provides a more comprehensive and reliable water purification solution, suitable for industrial wastewater treatment, municipal water purification and agricultural drainage management.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005005984960000091
    Figure BDA0005005984960000091
  • Figure BDA0005005984960000101
    Figure BDA0005005984960000101
  • Figure BDA0005005984960000121
    Figure BDA0005005984960000121
Patent Text Reader

Abstract

The invention relates to the technical field of water treatment, and discloses a bacteriostatic nano composite hydrogel and a preparation method thereof, the hydrogel comprises the following components by weight: 30-60 wt% of a polymer base material, which is polythiophene, polyacrylonitrile or a combination thereof; 5 to 15 weight percent of magnetic nano particles, wherein the magnetic nano particles are Fe3O4; 0.5 to 5 wt% of a cross-linking agent; 2-10 wt% of a surface modifier; 20 to 40 wt% of deionized water; the hydrogel has a core-shell structure; the surface modifier is selected from one or more of a compound containing a sulfate functional group, a compound containing an amino functional group, a compound containing a carboxyl functional group and a molecularly imprinted polymer with chelating ability. By introducing a core-shell structure and a specific surface modification technology, the removal efficiency of heavy metals, organic dyes and microorganisms is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water treatment, in particular to an antibacterial nano composite hydrogel and a preparation method thereof. Background Art

[0002] With the acceleration of industrialization, water pollution is becoming increasingly serious, especially the harm of heavy metal ions, organic pollutants and pathogenic microorganisms to the water environment, which has become a difficult problem that needs to be solved urgently in the field of global environmental protection. Traditional water treatment methods, such as chemical precipitation, adsorption, membrane separation and biological treatment, although they can remove certain specific pollutants to a certain extent, generally have some limitations. For example, chemical precipitation is prone to produce secondary pollutants; adsorption materials have low selectivity, are easily saturated and difficult to regenerate; although membrane separation technology is effective, it is costly and susceptible to membrane pollution, resulting in poor economic efficiency for long-term use; although biological treatment methods are environmentally friendly, they have limited efficiency when treating complex water bodies and are strictly restricted by operating conditions.

[0003] In the prior art, hydrogels have gradually attracted attention due to their good adsorption properties and controllable structures. However, conventional hydrogels still have obvious defects in practical applications, including poor mechanical properties, easy swelling failure, poor regeneration and other problems. These defects limit the application efficiency and life of hydrogels in treating a variety of complex pollutants. Especially when faced with complex water bodies containing heavy metals, organic pollutants and microorganisms, existing hydrogels often find it difficult to simultaneously take into account efficient adsorption and long-term stability. In addition, the traditional hydrogel has a single structure and insufficient degree of functionalization, which leads to its poor performance when multiple pollutants coexist, and it cannot effectively distinguish and treat different types of pollutants. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides an antibacterial nanocomposite hydrogel and a preparation method thereof. The existing water treatment materials have the problems of poor adsorption selectivity, poor mechanical properties and limited regeneration capacity in complex polluted environments.

[0005] To achieve the above objectives, the present invention is implemented by the following technical scheme: an antibacterial nanocomposite hydrogel, the hydrogel comprising the following components in weight percentage:

[0006] 30-60 wt % of a polymer substrate, wherein the polymer substrate is polythiophene, polyacrylonitrile or a combination thereof;

[0007] 5-15 wt% magnetic nanoparticles, wherein the magnetic nanoparticles are Fe3O4;

[0008] Crosslinking agent 0.5-5wt%;

[0009] Surface modifier 2-10wt%;

[0010] Deionized water 20-40wt%.

[0011] Preferably, the hydrogel has a core-shell structure, the core is Fe3O4 magnetic nanoparticles, and the shell is a cross-linked network of polythiophene, polyacrylonitrile or a combination thereof.

[0012] Preferably, the surface modifier is selected from one or more of a compound containing a sulfate functional group, a compound containing an amino functional group, a compound containing a carboxyl functional group, and a molecularly imprinted polymer having a chelating ability.

[0013] Preferably, the surface modifier of the hydrogel is combined with the surface of the hydrogel through a chemical reaction.

[0014] Preferably, the hydrogel has a multi-level pore structure, and the average diameter of the pores is 10 to 100 nanometers.

[0015] Preferably, the cross-linking agent is selected from glutaraldehyde, glyoxal, epichlorohydrin, diisocyanate or copper sulfate.

[0016] The present invention also provides a method for preparing an antibacterial nanocomposite hydrogel, comprising the following steps:

[0017] 1) dissolving polythiophene or polyacrylonitrile monomer in an anhydrous solvent, adding a crosslinking agent to the solution under nitrogen protection, heating the mixture to 60-80° C., stirring and reacting for 12-24 hours to obtain a solution containing a polymer substrate;

[0018] 2) adding Fe3O4 nanoparticles to the obtained solution and dispersing them by ultrasonic treatment for 10 to 30 minutes;

[0019] 3) placing the mixture obtained in step 2) in a mold, freeze-drying it at -20°C to -80°C for 48 to 72 hours, and then subjecting it to temperature gradient or chemical cross-linking at room temperature to form a multi-level pore structure inside the hydrogel;

[0020] 4) soaking the hydrogel obtained in step 3) in a surface modifier solution at a concentration of 0.01 to 0.5 mol / L at room temperature and reacting for 6 to 12 hours;

[0021] 5) The hydrogel modified in step 4) is repeatedly washed with deionized water to remove unreacted modifying agent and residues, and then dried at 50-70° C. to finally obtain an antibacterial nanocomposite hydrogel.

[0022] Preferably, the solvent is N,N-dimethylformamide with a concentration of 10-50 wt%.

[0023] Preferably, the pH value of the modification reaction in step 4) is controlled at 4-9.

[0024] The present invention also provides application of the antibacterial nanocomposite hydrogel in water purification, wherein the hydrogel is used for removing heavy metal ions, organic pollutants and harmful microorganisms in water.

[0025] The present invention provides an antibacterial nanocomposite hydrogel and a preparation method thereof. It has the following beneficial effects:

[0026] 1. The present invention significantly improves the removal efficiency of heavy metals, organic dyes and microorganisms by introducing a core-shell structure and a specific surface modification technology. This design enables the hydrogel to not only capture pollutants through physical adsorption, but also enhance the selectivity and adsorption capacity of specific pollutants through chemical reactions such as ion exchange and complex reactions. This feature is particularly important because it allows the hydrogel to maintain high efficiency and specificity when treating complex water bodies with multiple pollutants, thereby providing a more comprehensive and reliable water purification solution.

[0027] 2. The present invention exhibits excellent mechanical properties, including high breaking strength and elongation, through a carefully designed material combination and structural configuration. These properties mean that the hydrogel can maintain its integrity and function under various environmental conditions, avoiding rupture or disintegration under physical stress, thereby ensuring long-term and effective use. In addition, good mechanical properties also allow these hydrogels to be used in complex industrial applications, such as in flowing water systems or occasions that require frequent movement and replacement, significantly improving their practicality and economic benefits.

[0028] 3. The hydrogel design of the present invention takes into account the sustainable development needs of the environment, and reduces operating costs and environmental impacts through the material characteristics of easy regeneration and reuse. The hydrogel can be regenerated by simple chemical or physical methods to restore its adsorption capacity and thus be recycled many times. This regeneration ability not only reduces the need for new materials, but also means that higher material and energy efficiency can be achieved when treating pollutants.

[0029] 4. The hydrogels of the present invention have broad application prospects in many fields due to their excellent purification performance and safe material properties. They are not only suitable for industrial wastewater treatment and municipal water purification, but can also be applied to agricultural drainage management and emergency environmental response, such as responding to sudden chemical or biological pollution incidents. In addition, these hydrogels may also be used in non-aqueous purification systems, such as air purifiers and soil remediation projects, demonstrating their cross-domain technical scalability. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0031] Example 1: Preparation of polythiophene-based antibacterial nanocomposite hydrogel

[0032] Step 1: Preparation of polymer substrate

[0033] 40 g of polythiophene monomer was dissolved in 160 mL of anhydrous N,N-dimethylformamide (DMF) at a solvent concentration of 25 wt %.

[0034] Under nitrogen protection, 2 g of glutaraldehyde was added to the solution as a cross-linking agent.

[0035] The mixture was heated to 70° C. and stirred for reaction for 18 hours to obtain a solution containing a polymer matrix.

[0036] Step 2: Dispersion of Nanoparticles

[0037] 8 g of Fe3O4 nanoparticles were added to the solution obtained in step 1.

[0038] The nanoparticles were evenly dispersed in the solution by ultrasonic treatment (power 300 W, frequency 30 kHz) for 20 minutes.

[0039] Step 3: Formation of porous structure

[0040] The mixture obtained in step 2 was placed in a mold and freeze-dried at -60°C for 72 hours.

[0041] Subsequently, temperature gradient cross-linking was carried out at room temperature to form a multi-level pore structure with an average pore size of 50 nanometers inside the hydrogel.

[0042] Step 4: Surface modification

[0043] The hydrogel obtained in step 3 was immersed in a 0.3 mol / L ethylenediamine solution and reacted for 8 hours, and the pH value was adjusted to 7.

[0044] Surface modification was performed to enhance its adsorption capacity for heavy metal ions.

[0045] Step 5: Wash and dry

[0046] The modified hydrogel was repeatedly washed with deionized water to remove the unreacted modifying agent.

[0047] After drying at 60°C, the antibacterial nanocomposite hydrogel was finally obtained.

[0048] Example 2: Preparation of polyacrylonitrile-based antibacterial nanocomposite hydrogel

[0049] Step 1: Preparation of polymer substrate

[0050] 50 g of polyacrylonitrile monomer was dissolved in 100 mL of anhydrous N,N-dimethylformamide (DMF) at a solvent concentration of 33 wt %.

[0051] Under nitrogen protection, 1.5 g of epichlorohydrin was added as a cross-linking agent.

[0052] The mixture was heated to 65° C. and stirred for reaction for 24 hours to obtain a polymer substrate solution.

[0053] Step 2: Dispersion of Nanoparticles

[0054] 6 g of Fe3O4 nanoparticles were added into the solution.

[0055] Ultrasonic treatment (power 250 W, frequency 25 kHz) was used for 15 minutes to make it uniformly dispersed.

[0056] Step 3: Formation of porous structure

[0057] The mixture was placed in a mold and freeze-dried at -40°C for 48 hours.

[0058] Chemical cross-linking treatment is carried out at room temperature to form a multi-level pore structure with an average pore size of 80 nanometers inside the hydrogel.

[0059] Step 4: Surface modification

[0060] The modified samples were immersed in 0.5 mol / L thioglycolic acid solution for 4 hours, and the pH value was controlled at 6.

[0061] After modification, Hg + and Cd + Hydrogels with high adsorption capacity.

[0062] Step 5: Wash and dry

[0063] The modified hydrogel was washed with deionized water.

[0064] After drying at 50°C, the desired antibacterial nanocomposite hydrogel is finally obtained.

[0065] Example 3: Preparation of antibacterial nanocomposite hydrogel based on polythiophene / polyacrylonitrile composite substrate

[0066] Step 1: Preparation of polymer substrate

[0067] 30 g of polythiophene and 30 g of polyacrylonitrile monomer were mixed in a ratio of 1:1 and dissolved in 200 mL of anhydrous N,N-dimethylformamide (DMF) with a solvent concentration of 30 wt%.

[0068] Under nitrogen protection, 2.5 g of glyoxal was added as a cross-linking agent.

[0069] The mixture was heated to 75° C. and stirred for reaction for 12 hours to obtain a solution containing a composite polymer matrix.

[0070] Step 2: Dispersion of Nanoparticles

[0071] 9 g of Fe3O4 nanoparticles were added to the solution.

[0072] Ultrasonic treatment (power 350 W, frequency 35 kHz) was used for 25 minutes to ensure uniform dispersion of the particles.

[0073] Step 3: Formation of porous structure

[0074] The mixture was placed in a mold and freeze-dried at -70°C for 72 hours.

[0075] Temperature gradient cross-linking was carried out at room temperature to form a multi-level porous structure with an average pore size of 30 nanometers.

[0076] Step 4: Surface modification

[0077] The hydrogel was immersed in 0.4 mol / L aminosilane (APTES) solution with pH value controlled at 8 for 6 hours.

[0078] Get Pb 2 + and Cu2+ with high selective adsorption capacity of hydrogel.

[0079] Step 5: Wash and dry

[0080] Wash several times with deionized water to remove unreacted modifying agent.

[0081] The antibacterial nanocomposite hydrogel was obtained by drying at 55°C.

[0082] Example 4: Preparation of molecularly imprinted antibacterial nanocomposite hydrogel with chelating ability

[0083] Step 1: Preparation of polymer substrate

[0084] 45 g of polythiophene monomer was dissolved in 150 mL of anhydrous N,N-dimethylformamide (DMF) at a solvent concentration of 30 wt %.

[0085] Under nitrogen protection, 3 g of diisocyanate was added as a cross-linking agent.

[0086] The mixture was heated to 70° C. and stirred for reaction for 20 hours to obtain a polymer substrate solution.

[0087] Step 2: Dispersion of Nanoparticles

[0088] 7 g of Fe3O4 nanoparticles were added to the solution.

[0089] Ultrasonic treatment (power 200 W, frequency 20 kHz) was used for 10 minutes to ensure uniform dispersion.

[0090] Step 3: Formation of porous structure

[0091] The mixture was placed in a mold and freeze-dried at -30°C for 48 hours.

[0092] Chemical cross-linking treatment is carried out at room temperature to form a multi-level porous structure with an average pore size of 40 nanometers.

[0093] Step 4: Surface modification

[0094] The hydrogel was immersed in a 0.25 mol / L molecular imprinting polymer solution, the pH value was controlled at 7, and the reaction was carried out for 10 hours.

[0095] After modification, a hydrogel with high chelating ability for various heavy metal ions is obtained.

[0096] Step 5: Wash and dry

[0097] The unreacted molecular imprinting polymer was removed by washing with deionized water for several times.

[0098] After drying at 65°C, a highly effective antibacterial nanocomposite hydrogel was finally obtained.

[0099] Example 5: Preparation of antibacterial nanocomposite hydrogel modified with mercaptopropionic acid

[0100] Step 1: Preparation of polymer substrate

[0101] 35 g of polythiophene and 25 g of polyacrylonitrile monomer were mixed and dissolved in 150 mL of anhydrous N,N-dimethylformamide (DMF) at a solvent concentration of 28 wt %.

[0102] Under nitrogen protection, 1.8 g of glutaraldehyde was added as a cross-linking agent.

[0103] The mixture was heated to 60° C. and stirred for reaction for 24 hours to obtain a polymer substrate solution.

[0104] Step 2: Dispersion of Nanoparticles

[0105] 5 g of Fe3O4 nanoparticles were added to the solution.

[0106] Ultrasonic treatment (power 150 W, frequency 28 kHz) was used for 30 minutes to ensure that the particles were evenly dispersed.

[0107] Step 3: Formation of porous structure

[0108] The mixture was placed in a mold and freeze-dried at -50°C for 60 hours.

[0109] Chemical cross-linking treatment is carried out at room temperature to form a multi-level porous structure with an average pore size of 60 nanometers.

[0110] Step 4: Surface modification

[0111] The hydrogel was immersed in a 0.2 mol / L mercaptopropionic acid solution with the pH value controlled at 6 for 6 hours.

[0112] Get a variety of heavy metal ions such as Hg 2+ 、Cd + Hydrogels with highly selective adsorption capacity.

[0113] Step 5: Wash and dry

[0114] The unreacted modifier was removed by repeated washing with deionized water.

[0115] After drying at 60°C, the desired antibacterial nanocomposite hydrogel was finally obtained.

[0116] Experiment 1: Antibacterial performance comparison experiment

[0117] Objective: To evaluate the antibacterial effects of antibacterial nanocomposite hydrogels in different embodiments against common pathogens.

[0118] Experimental design:

[0119] Strain selection: Three common pathogens were selected: Escherichia coli (E.co li), Staphylococcus aureus (S.aureus) and Pseudomonas aeruginosa (P.aeruginosa).

[0120] Samples: Five antibacterial nanocomposite hydrogels of Examples were used.

[0121] Experimental methods:

[0122] 1. Cut each hydrogel sample into small pieces of the same size (about 0.5 g).

[0123] 2. Add each hydrogel sheet into a sterile test tube containing 10 mL of bacterial solution. The initial concentration of the bacterial solution is 10 6 CFU / mL.

[0124] 3. Incubate the tubes at 37°C for 24 hours.

[0125] 4. After sampling and dilution, culture the samples on nutrient agar plates by plate spreading method and incubate at 37°C for 24 hours.

[0126] 5. The number of remaining bacteria was calculated by colony counting method (CFU / mL) to determine the antibacterial effect of the hydrogel.

[0127] Control group: A control group without any hydrogel was set up as a comparison benchmark.

[0128] Experimental steps:

[0129] 1. Sample preparation:

[0130] The hydrogel samples of the five embodiments were cut into small pieces of the same size, each piece weighing about 0.5 g, and divided into 5 groups.

[0131] Each group included tests of 3 strains, for a total of 15 experimental samples.

[0132] 2. Bacterial culture:

[0133] E. coli, S. aureus and P. aeruginosa were cultured in LB medium until the logarithmic growth phase and the bacterial concentration was adjusted to 10 6 CFU / mL.

[0134] 3. Antibacterial experiment:

[0135] Each hydrogel sheet was placed in a sterile test tube containing 10 mL of different bacterial solutions.

[0136] Incubate at 37°C for 24 hours.

[0137] 4. Colony count:

[0138] After incubation, samples were taken for 10-fold serial dilution and spread on nutrient agar plates using the plate spreading method.

[0139] After incubation at 37°C for 24 h, the number of colonies was counted.

[0140] The experimental results are shown in Table 1:

[0141] Table 1: Antibacterial performance test data of antibacterial nanocomposite hydrogels in different embodiments

[0142]

[0143]

[0144] According to the results of the comparative experiment, the antibacterial nanocomposite hydrogels of all examples showed significant antibacterial effects, with the antibacterial rates ranging from 94% to 98.85%. This result clearly shows that the combination of substances in the formula of the present invention can effectively inhibit common pathogens.

[0145] In all embodiments, polythiophene and polyacrylonitrile are used as polymer substrates. These polymers not only provide structural support, but also have an inhibitory effect on microorganisms due to their special chemical properties. Polythiophene is particularly suitable for combination with antimicrobial agents because it can produce antimicrobial activity through redox reactions, which is why it exhibits a high inhibition rate against S. aureus.

[0146] The core-shell structure in the embodiment, in which the core is Fe3O4 magnetic nanoparticles and the shell is a cross-linked network of polythiophene / polyacrylonitrile, enhances the functional diversity of the hydrogel. The addition of Fe3O4 not only provides magnetic recovery, but also indirectly participates in antibacterial activity by generating a local redox environment. In addition, this structural design enhances the mechanical stability and durability of the hydrogel, making it more suitable for long-term use.

[0147] The present invention enhances the target specificity of the hydrogel by introducing modifiers with specific functional groups (such as molecular imprinting polymers containing amino, carboxyl, sulfate functional groups and chelating ability) on the surface of the hydrogel. These functional groups can interact with specific components of the bacterial cell wall, thereby inhibiting its growth. For example, modifiers containing amino functional groups interfere with bacterial cellular processes by mimicking the mode of action of natural antibiotics.

[0148] Examples 3 and 5 showed relatively high inhibitory effects on P. aeruginosa, which was related to the surface modification with mercaptopropionic acid and aminosilane. The additional functionality provided by these two compounds interacted more effectively with specific targets in the cell structure of P. aeruginosa.

[0149] Examples 1 and 3 are particularly effective in inhibiting S. aureus due to the synergistic effect of the polythiophene and polyacrylonitrile composite material and the efficient redox properties, which have a stronger influence on Gram-positive bacteria.

[0150] In summary, the present invention not only provides a strong antibacterial effect but also increases the recyclability of the material and the wide range of applications by combining the unique design of polymer substrate, core-shell structure and surface modifier.

[0151] Experiment 2: Comparative experiment on heavy metal adsorption capacity

[0152] Objective: To evaluate the adsorption efficiency and selectivity of different examples of antibacterial nanocomposite hydrogels for common heavy metal ions.

[0153] Experimental design:

[0154] Pollutant selection: Select three common heavy metal ions: lead ion (Pb 2+ ), mercury ion (Hg 2+ ) and cadmium ions (Cd 2+ ).

[0155] Samples: Five antibacterial nanocomposite hydrogels of Examples were used.

[0156] Experimental methods:

[0157] 1. Preparation of 100ppm Pb 2+ , Hg 2+ and Cd 2+ 100mL of each solution.

[0158] 2. Each hydrogel sample (0.5 g) was added to each heavy metal solution and stirred at room temperature for 24 hours.

[0159] 3. Take samples through filtration, use atomic absorption spectrometer (AAS) to determine the concentration of remaining heavy metal ions in the solution, and calculate the adsorption amount of heavy metal ions by hydrogel.

[0160] Experimental steps:

[0161] 1. Sample preparation:

[0162] Weigh 0.5 g of the hydrogel of each example and put it into marked beakers, for a total of 15 samples.

[0163] 2. Preparation of heavy metal solution:

[0164] Prepare a concentration of 100ppm Pb 2+ , Hg 2+ and Cd 2+ Solution, 100mL each.

[0165] 3. Adsorption experiment:

[0166] The hydrogel samples were added to the respective heavy metal solutions and stirred at room temperature (about 25° C.) for 24 hours.

[0167] 4. Sample filtration and determination:

[0168] The hydrogel was separated from the solution by a filter.

[0169] Atomic absorption spectrometer (AAS) was used to determine the Pb content in the filtered solution. 2+ , Hg 2+ and Cd 2+ The concentration is recorded.

[0170] The experimental data are shown in Table 2:

[0171] Table 2: Antibacterial nanocomposite hydrogels of different embodiments for heavy metal ions (Pb 2+ , Hg 2+ 、Cd 2+ ) adsorption experimental data

[0172]

[0173]

[0174] The data in Table 2 show that all the examples can effectively adsorb and remove heavy metal ions in water, proving the significant effectiveness of the present invention in treating heavy metal pollution.

[0175] Polythiophene and polyacrylonitrile, as polymer substrates, play a key role in all examples. They not only provide the necessary structural stability for the hydrogel, but also enhance the adsorption capacity of the hydrogel for heavy metal ions due to their good chemical stability and relatively large surface area. In particular, in Example 3, these polymers act together with the surface modifier to show the highest adsorption rate for all tested heavy metal ions.

[0176] The core-shell structure introduced in the embodiment, especially the Fe3O4 magnetic nanoparticle core and polymer shell, not only simplifies the recovery process of the hydrogel, but also increases the contact opportunities with heavy metal ions by providing more active sites. This structural arrangement enables the hydrogel to effectively capture and fix heavy metal ions while maintaining good fluidity.

[0177] Surface modifiers play a decisive role in improving the performance of hydrogels. Surface modifiers such as mercaptopropionic acid and aminosilane used in Examples 3 and 5 significantly improve the adsorption capacity of hydrogels by forming stable complexes with heavy metal ions. Mercaptopropionic acid is particularly suitable for soft metal ions such as Hg due to its strong chelating ability. 2+ and Cd 2+ The formation of a stable complex explains the 2+ and Cd 2+ The higher adsorption rate was shown in the test.

[0178] Each example shows the effect of Pb 2+ , Hg 2+ and Cd 2+The different adsorption efficiencies of the hydrogels reflect the specific effects of different surface modifiers and core-shell structures on the adsorption performance. Example 3 exhibits high adsorption capacity for all three metal ions due to its unique core-shell structure and surface modification strategy. This shows that by optimizing the physical and chemical properties of the hydrogel, its removal efficiency for specific pollutants can be significantly improved.

[0179] The present invention demonstrates an efficient, recyclable and economical solution to treat heavy metal pollution in water through a uniquely designed polymer substrate, core-shell structure and targeted surface modifier. The preparation method and material selection of these hydrogels provide a new direction for environmental remediation technology, especially in the treatment of industrial wastewater and the protection of water resources, showing great application potential.

[0180] Experiment 3: Regeneration and reuse performance comparison experiment

[0181] Objective: To evaluate the regeneration ability of antibacterial nanocomposite hydrogels of different embodiments during multiple uses and the stability of their adsorption properties.

[0182] Experimental design:

[0183] Pollutant selection: Select lead ion (Pb 2 +) were used as representative heavy metal ions for regeneration and reuse experiments.

[0184] Samples: Five antibacterial nanocomposite hydrogels of Examples were used.

[0185] Experimental methods:

[0186] 1. Each hydrogel sample (0.5 g) was first exposed to 100 ppm of Pb 2+ Adsorption experiments were carried out in solution.

[0187] 2. After adsorption, it was eluted with an acidic solution (0.1 M HCl) and then washed with deionized water until neutral.

[0188] 3. Repeat the above adsorption-elution cycle for 10 times and record the Pb after each adsorption. 2+ Adsorption amount.

[0189] Experimental steps:

[0190] 1. Sample preparation:

[0191] Take 0.5 g of the hydrogel sample of each example, a total of 5 groups.

[0192] 2. Adsorption experiment:

[0193] The hydrogel samples were added with 100 ppm of Pb 2+ The solution was stirred at room temperature (25°C) for 24 hours.

[0194] 3. Elution and regeneration:

[0195] The adsorption-saturated hydrogel sample was eluted using 0.1 M HCl solution for 2 h.

[0196] The hydrogel was washed with deionized water until the pH returned to neutral.

[0197] 4. Repeated use experiment:

[0198] The regenerated hydrogel sample was placed in fresh 100 ppm Pb 2+ The adsorption and elution process was repeated for 10 cycles.

[0199] The experimental data are shown in Table 3:

[0200] Table 3: Experimental data on the regeneration and reuse performance of antibacterial nanocomposite hydrogels in different embodiments

[0201] Cycle times Sample No. <![CDATA[Pb 2+ Adsorption capacity (mg / g)]]> Adsorption rate decrease (%) 1st time Example 1 18.3 - 1st time Example 2 17.9 - 1st time Example 3 19.1 - 1st time Example 4 17.2 - 1st time Example 5 18.7 - 2nd Example 1 17.6 3.83 2nd Example 2 17.2 3.91 2nd Example 3 18.8 1.57 2nd Example 4 16.7 2.91 2nd Example 5 18.4 1.6 5th Example 1 16.3 10.93 5th Example 2 15.8 11.73 5th Example 3 17.7 7.33 5th Example 4 15.4 10.47 5th Example 5 17.2 8.02 10th Example 1 14.9 18.58 10th Example 2 14.4 19.55 10th Example 3 16.6 13.09 10th Example 4 14.2 17.44 10th Example 5 15.8 15.51

[0202] The data in Table 3 show the excellent regeneration ability and stability of the adsorption performance of the antibacterial nanocomposite hydrogel of the present invention in continuous heavy metal ions.

[0203] Example 3 showed the best regeneration and durability of adsorption performance, which was attributed to its core-shell structural design. The Fe3O4 nanoparticles as the core not only provided the convenience of magnetic recovery, but also promoted the effective binding of heavy metal ions to the polymer shell through its surface characteristics. This structural design ensured that the functional components of the hydrogel remained stable during repeated use and elution, thereby maintaining high adsorption capacity.

[0204] The surface modifiers used in Examples 3 and 5, especially mercaptopropionic acid and aminosilane, have strong chelating ability and high affinity for heavy metals. They significantly improve the adsorption capacity and stability of the hydrogel by forming stable chemical bonds with metal ions. This explains why these two examples show a small decrease in adsorption rate during repeated use.

[0205] The advantage of Example 3 is partly due to its unique material combination, namely the organic combination of core-shell structure and surface modifier. This design not only improves the adsorption efficiency, but also optimizes the overall performance and regeneration capacity of the hydrogel by reducing the loss of functional materials. In addition, although the adsorption performance of Example 5 is slightly lower than that of Example 3, the regeneration stability it exhibits also illustrates the importance of surface modifier selection for improving reuse efficiency.

[0206] From Example 1 to Example 4, it can be observed that the adsorption performance gradually decreases with the increase in the number of cycles, especially the performance decay is more significant in Example 4. This may be due to the insufficient compatibility of the selected surface modifier with the polymer substrate or the poor stability of the modifier itself in an acidic environment, resulting in the gradual shedding of the modifier during repeated elution.

[0207] The present invention not only improves the heavy metal ion removal efficiency of the hydrogel, but also significantly improves the regeneration ability and service life of the material through carefully designed material selection and structural configuration, especially the application of core-shell structure and surface modifier.

[0208] Experiment 4: Mechanical properties comparison experiment

[0209] Objective: To evaluate the mechanical strength and toughness of antibacterial nanocomposite hydrogels from different embodiments to ensure their stability and durability in practical applications.

[0210] Experimental design:

[0211] Samples: Five antibacterial nanocomposite hydrogels of Examples were used.

[0212] Experimental methods:

[0213] 1. Prepare standard test sample strips (approximately 50 mm x 10 mm x 2 mm in size) from each example.

[0214] 2. Perform tensile tests using a universal material testing machine to determine the breaking strength and elongation of each sample.

[0215] 3. Record the maximum load and corresponding elongation of each sample before fracture.

[0216] Experimental steps:

[0217] 1. Sample preparation:

[0218] The hydrogels of each example were prepared and cut into test strips of standard size.

[0219] 2. Tensile test:

[0220] Fix the specimen at both ends of the universal materials testing machine.

[0221] The specimen was stretched at a speed of 5 mm / min until it broke.

[0222] The maximum load achieved and the corresponding elongation are recorded.

[0223] 3. Data Recording:

[0224] Tensile data including breaking strength (MPa) and elongation at break (%) were collected for all specimens.

[0225] The experimental results are shown in Table 4:

[0226] Table 4: Mechanical properties test results of antibacterial nanocomposite hydrogels in different embodiments

[0227] Sample No. Breaking strength(MPa) Elongation(%) Remark Example 1 1.9 120 - Example 2 2.2 130 - Example 3 2.5 140 High toughness Example 4 1.7 115 Low elongation Example 5 2.3 135 - Example 1 1.8 118 Repeat the test Example 2 2.1 128 Repeat the test Example 3 2.4 138 Repeat the test Example 4 1.6 112 Repeat the test Example 5 2.1 132 Repeat the test

[0228] According to the data in Table 4, it can be observed that each embodiment exhibits different mechanical properties in the tensile test.

[0229] Example 3 significantly exhibited the highest breaking strength and elongation, which can be attributed to its optimized core-shell structure design. This design not only enhances the overall structure of the hydrogel, but also improves its tensile strength through effective stress distribution. The core Fe3O4 nanoparticles increase the overall density and cross-linking degree of the composite material, while the polymer shell provides sufficient elasticity and plasticity, thereby showing a high elongation when stretched.

[0230] The different cross-linking agents used in each example directly affect the mechanical properties of the hydrogel. For example, Example 3 may have used a cross-linking agent that is more suitable for forming a stable cross-linked network, such as glutaraldehyde or a more efficient chemical cross-linking agent, which supports its excellent performance in mechanical testing.

[0231] Although mainly used to improve antibacterial and adsorption properties, the use of surface modifiers also indirectly affects the mechanical strength of hydrogels. By introducing additional functional groups such as amino or thiol groups on the polymer surface, the internal cohesion of the material can be enhanced, thereby providing better resistance to mechanical stress.

[0232] The superior performance of Example 3 shows that the correct configuration of the core-shell structure is crucial to achieving high mechanical properties. This structure not only improves the uniformity of the material, but also optimizes the distribution of internal stress, so that the force can be dispersed more evenly when stretched, reducing the possibility of fracture.

[0233] Experiment 5: Comprehensive experiment on water purification

[0234] Objective: To evaluate the comprehensive purification ability of antibacterial nanocomposite hydrogels of different embodiments in complex water bodies, targeting the removal efficiency of heavy metal ions, organic dyes, and microorganisms.

[0235] Experimental design:

[0236] Samples: Five antibacterial nanocomposite hydrogels of Examples were used.

[0237] Pollutants: Select lead ions (Pb 2+ ), methyl orange (organic dye), and Escherichia coli (E. co li) were used as test pollutants.

[0238] Experimental methods:

[0239] 1. Prepare a solution containing 100ppm Pb 2+ , 50ppm methyl orange and 10 6 CFU / mL E.co li's simulated sewage.

[0240] 2. Add 0.5 g of the hydrogel of each example to each sewage, and stir the reaction at room temperature for 24 hours.

[0241] 3. Evaluate the Pb content in purified water by atomic absorption spectrometry, UV-Vis spectrometry and microbial counting method 2+ , methyl orange and E. coli concentrations.

[0242] Experimental steps:

[0243] 1. Preparation of simulated sewage:

[0244] According to the above concentration standard, the 2+ , methyl orange and E. coli simulated sewage.

[0245] 2. Add hydrogel:

[0246] The hydrogels of various examples were added into simulated sewage respectively.

[0247] 3. Stirring and reaction:

[0248] Stir at 200 rpm for 24 hours at room temperature to ensure sufficient contact and reaction.

[0249] 4. Separation and determination:

[0250] Separate the hydrogel using a filter or centrifuge.

[0251] Use the corresponding instrument to determine Pb in water 2+ , methyl orange and the residual concentrations of E. coli.

[0252] The experimental results are shown in Table 5:

[0253] Table 5: Test results of purification performance of antibacterial nanocomposite hydrogels in simulated sewage treatment according to different embodiments

[0254] Sample No. <![CDATA[Pb 2+ Removal rate (%)]]> Methyl orange removal rate (%) E.coli removal rate (%) Example 1 82.3 76.4 99 Example 2 85.7 78.1 99.1 Example 3 88.9 80.2 99.4 Example 4 80.6 74.9 98.6 Example 5 84.1 79.5 99.3 Example 1 81.9 75.6 98.9 Example 2 85.3 77.9 99.2 Example 3 89.2 81.5 99.5 Example 4 79.8 73.8 98.5 Example 5 83.7 78.9 99.2

[0255] From the data in Table 5, it can be seen that the hydrogel of the present invention exhibits a significant multi-pollutant removal capability and effectively purifies water bodies containing heavy metals, organic dyes and biological pollution.

[0256] Example 3 showed the highest lead ion (Pb 2+) removal rate reached 89.2%. This remarkable effect is due to its core-shell structure design, in which the core magnetic Fe3O4 nanoparticles enhance the hydrogel's attraction to heavy metal ions, while the polymer shell provides sufficient functional groups (such as sulfate and amino groups) to form stable complexes with heavy metal ions, thereby effectively fixing these ions.

[0257] Each example shows a good removal effect on methyl orange, among which Example 3 also performs best, with a removal rate of 81.5%. This effect may be due to the structure of the hydrogel surface modifier, which can capture organic molecules through adsorption or intermolecular forces. In addition, the pore structure of the hydrogel may also provide sufficient surface area and paths to promote the penetration and fixation of dye molecules.

[0258] In terms of removing E. coli, all examples showed extremely high efficiency, especially Example 3, with a removal rate of up to 99.5%. This reflects the high efficiency of the antibacterial functional groups (such as silver or copper nanoparticles) on the surface of the hydrogel in inhibiting and killing bacteria, as well as the ability of its physical structure to restrict the passage of bacteria.

[0259] In a series of comprehensive performance tests, the antibacterial nanocomposite hydrogels of each embodiment demonstrated excellent purification capabilities and mechanical properties. The experimental results show that these hydrogels not only effectively remove heavy metal ions, organic dyes and microorganisms in water, but also show excellent mechanical strength and reusability. In particular, Example 3 continued to show the best performance in multiple cycle tests, and its unique core-shell structure and surface modification strategy optimized the adsorption efficiency and structural stability of the material. These experiments verified the high efficiency and reliability of hydrogels in practical applications, especially in the face of complex environmental pollution conditions, demonstrating its broad application prospects and potential market value.

[0260] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An antibacterial nanocomposite hydrogel, characterized in that: The hydrogel comprises the following components in weight percentage: 30-60 wt % of a polymer substrate, wherein the polymer substrate is polythiophene, polyacrylonitrile or a combination thereof; 5-15 wt% magnetic nanoparticles, wherein the magnetic nanoparticles are Fe3O4; Crosslinking agent 0.5-5wt%; Surface modifier 2-10wt%; Deionized water 20-40wt%.

2. The antibacterial nanocomposite hydrogel according to claim 1, characterized in that: The hydrogel has a core-shell structure, the core is Fe3O4 magnetic nanoparticles, and the shell is a cross-linked network of polythiophene, polyacrylonitrile or a combination thereof.

3. The antibacterial nanocomposite hydrogel according to claim 1, characterized in that: The surface modifier is selected from one or more of a compound containing a sulfate functional group, a compound containing an amino functional group, a compound containing a carboxyl functional group and a molecular imprinting polymer having a chelating ability.

4. The antibacterial nanocomposite hydrogel according to claim 1, characterized in that: The surface modifier of the hydrogel is combined with the surface of the hydrogel through a chemical reaction.

5. The antibacterial nanocomposite hydrogel according to claim 1, characterized in that: The hydrogel has a multi-level pore structure, and the average diameter of the pores is 10 to 100 nanometers.

6. The antibacterial nanocomposite hydrogel according to claim 1, characterized in that: The cross-linking agent is selected from glutaraldehyde, glyoxal, epichlorohydrin, diisocyanate or copper sulfate.

7. A method for preparing an antibacterial nanocomposite hydrogel, comprising preparing the antibacterial nanocomposite hydrogel according to any one of claims 1 to 6, characterized in that: The following steps are involved: 1) dissolving polythiophene or polyacrylonitrile monomer in an anhydrous solvent, adding a crosslinking agent to the solution under nitrogen protection, heating the mixture to 60-80° C., stirring and reacting for 12-24 hours to obtain a solution containing a polymer substrate; 2) adding Fe3O4 nanoparticles to the obtained solution and dispersing them by ultrasonic treatment for 10 to 30 minutes; 3) placing the mixture obtained in step 2) in a mold, freeze-drying it at -20°C to -80°C for 48 to 72 hours, and then subjecting it to temperature gradient or chemical cross-linking at room temperature to form a multi-level pore structure inside the hydrogel; 4) soaking the hydrogel obtained in step 3) in a surface modifier solution at a concentration of 0.01 to 0.5 mol / L at room temperature and reacting for 6 to 12 hours; 5) The hydrogel modified in step 4) is repeatedly washed with deionized water to remove unreacted modifying agent and residues, and then dried at 50-70° C. to finally obtain an antibacterial nanocomposite hydrogel.

8. The preparation method according to claim 7, characterized in that: The solvent is N,N-dimethylformamide, and the concentration is 10-50 wt %.

9. The preparation method according to claim 7, characterized in that: The pH value of the modification reaction in step 4) is controlled at 4-9.

10. Use of the antibacterial nanocomposite hydrogel according to any one of claims 1 to 6 in water purification, characterized in that: The hydrogel is used for removing heavy metal ions, organic pollutants and harmful microorganisms in water.