Bird nest crack detection method for casting blank
By cutting multiple samples on the casting break sample and analyzing their morphological characteristics, high-temperature oxides and decarbonization layer characteristics, the problem of inaccurate crack detection in the casting bird's nest in the prior art is solved, and the crack source is achieved and accurate judgment of the process improves the accuracy and reliability of the inspection.
Patent Information
- Application Number
- CN202411005057.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is not accurate enough in the detection of cracks in the nest of casting billets, and it is difficult to accurately judge the crack source and production process, resulting in misjudgment.
By cutting the casting piece with bird's nest crack on the casting blank, cutting the break sample, and cutting the first sample, the second sample and the third sample on the break sample, obtaining the broken sample on the side of the broken sample Topomorphic characteristics, high-temperature oxide characteristics and decarbonized layer characteristics are comprehensively analyzed to determine the crack source and timing.
The accuracy of crack detection and reliability of test results of cast-blank bird nests is improved, and the crack source and generation process of nest cracks are accurately judged.
Smart Images

Figure CN118913820A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of casting crack detection, and more specifically, relates to a casting bird's nest crack detection method. Background Art
[0002] To determine the cause of the "bird's nest" cracks in large-section grinding ball steel ingots, the main thing is to find the crack source location of the "bird's nest" cracks, determine the process of the crack source, and provide technical support for optimizing the production process. At present, there are two main sources of the "bird's nest" cracks in ingots.
[0003] One is the "bird's nest" crack of the billet. The crack source is the stress crack located in the core of the billet, which is generated in the steel rolling process. The large-section grinding ball steel billet has a high carbon and alloy content, poor thermal conductivity, and is very sensitive to the heating rate. During the heating process of the cold billet in the heating furnace, the heat conduction is from the surface to the inside, and there is a temperature gradient from the surface to the center of the billet; accordingly, thermal stress is generated inside the billet. As a result of the thermal stress, the surface of the billet is subjected to compressive stress, while the center of the billet is subjected to tensile stress. Since the center of the billet is where low-melting-point components and impurities are enriched, the strength is the lowest, and there are even intermittent shrinkage cavities. For large-section billets, if the temperature rises too quickly, cracks will form in the core of the billet. If cracks have formed in the core or large stresses have formed, the billet will break and crack during the heating and rolling process. When the billet is opened with a large amount of pressure, the cracks in the core of the billet will expand from the inside to the surface, and finally form a "bird's nest" crack or direct break.
[0004] The other is the "Bird's Nest" crack, which is a transverse crack on the surface of the ingot. The crack source is generated in the steelmaking process. The surface cracks of the ingot are mainly generated in the continuous casting process of steelmaking. The main reasons are as follows: (1) Nb, Al, C, and N have a strong affinity. When the continuous casting ingot passes through the straightening zone, the temperature is in the low plasticity zone of 900-700°C. Due to the transformation of γFe→αFe and the large amount of precipitation of AlN, NbN, and NbCN in steels with high Al, Nb, and N content in this temperature range, the grain boundary is brittle, and the arc surface shell inside the ingot cannot resist the straightening force and produces transverse cracks. ; (2) The temperature range of 700-900℃ is the low plasticity temperature zone of steel. If the secondary cooling system of steelmaking continuous casting is not suitable, the billet is straightened in this temperature range, and transverse cracks are very likely to occur in the billet; (3) The frequent fluctuation of the liquid level in the crystallizer leads to uneven thickness of the primary billet shell on the meniscus and deepening of the vibration marks, which is not conducive to reducing transverse cracks. Excessive fluctuations in the pulling speed lead to large fluctuations in the secondary cooling water volume of the billet in the fan-shaped section, causing the straightening temperature of some billets to fall into the brittle zone, which is prone to transverse cracks. Transverse cracks on the billet surface, when the large-section billet is rolled and opened at a large pressure, the surface cracks of the billet will extend from the surface to the core, and finally form a "bird's nest" crack or fracture.
[0005] The existing technology is to make the bird's nest crack of the ingot into a fracture specimen, observe the macroscopic morphology of the bird's nest crack fracture, determine the crack source of the bird's nest crack, cut the specimen at the crack source for fracture analysis, and determine the cause of the bird's nest crack by the fracture morphology characteristics at the crack source. However, the fracture covered by high-temperature iron oxide scale cannot accurately find the crack source, which often leads to misjudgment of the cause of the crack and makes it difficult to accurately determine the process of generating the bird's nest crack. Summary of the invention
[0006] The purpose of the present invention is to provide a method for detecting bird's nest cracks in a casting billet in view of the deficiencies in the prior art, so as to solve the problems that the detection of bird's nest cracks in a casting billet in the prior art is not accurate enough and the detection result is not reliable enough.
[0007] In order to achieve the above object, the present invention provides a method for detecting bird's nest cracks in a casting, comprising:
[0008] Cutting a casting section with bird's nest cracks on the casting;
[0009] Cutting the ingot segment along the cross section of the ingot segment at the bird's nest crack to obtain at least one fracture specimen;
[0010] Cutting a first sample, a second sample and a third sample from a fracture sample, wherein the first sample is close to the opening of the bird's nest crack on the ingot segment, the third sample is located at the core of the fracture sample, and the second sample is located between the first sample and the third sample;
[0011] Inspecting the first sample, the second sample and the third sample to obtain morphological characteristics, high-temperature oxide characteristics and decarburized layer characteristics on one side of the bird's nest crack fracture;
[0012] The crack source and generation timing of the bird's nest crack are determined according to the morphological characteristics, the high temperature oxide characteristics and the decarburized layer characteristics.
[0013] Optionally, cutting a casting billet segment with bird's nest cracks on the casting billet comprises:
[0014] Determine the location of the cracks in the bird's nest;
[0015] A cutting position is set on both sides of the bird's nest crack along the axial direction of the ingot, and the distance between the cutting position and the bird's nest crack is the set distance;
[0016] The ingot segment is cut off along the cutting position.
[0017] Optionally, the ingot segments are cut by sawing.
[0018] Optionally, the ingot segment is cut along a sawing surface by sawing, wherein the sawing surface passes through an opening of the bird's nest crack on the ingot segment.
[0019] Optionally, before cutting the first specimen, the second specimen and the third specimen, the sampling position is marked on one side of the bird's nest crack fracture of the fracture specimen.
[0020] Optionally, the sampling positions of the first sample, the second sample and the third sample are all marked as rectangles.
[0021] Optionally, before inspecting the first specimen, the second specimen and the third specimen, a test surface is selected, the test surface of the first specimen is a cutting surface close to one side of the bird's nest crack fracture and perpendicular to the surface of the opening with the bird's nest crack on the ingot segment, and the test surfaces of the second specimen and the third specimen are coplanar with the test surface of the first specimen.
[0022] Optionally, the method further includes grinding and polishing the detection surface so that the detection surface meets metallographic inspection requirements.
[0023] Optionally, the inspection of the first sample, the second sample and the third sample includes morphological inspection and metallographic inspection, the morphological characteristics include whether the color of the iron oxide scale is uniform, the high-temperature oxide characteristics include whether high-temperature oxides exist, and the decarburization layer characteristics include whether a complete decarburization layer and a semi-decarburization layer exist.
[0024] Optionally, judging the crack source and cause of the bird's nest crack according to the morphological features, the high temperature oxide features and the decarburized layer features includes:
[0025] If the color of the iron oxide scale on one side of the bird's nest crack fracture is uniform, and the structure on one side of the bird's nest crack fracture of the first sample is that there is no complete decarburization layer and no high-temperature oxide, it is determined that the crack source of the bird's nest crack is the stress crack in the core of the ingot, and the bird's nest crack is formed during the rolling process;
[0026] If the color of the iron oxide scale on one side of the bird's nest crack fracture is uneven, the structure of one side of the bird's nest crack fracture of the first sample is that there is a complete decarburization layer, a semi-decarburization layer, and a high-temperature oxide, and the structure of one side of the bird's nest crack fracture of the second sample and the third sample is that there is a complete decarburization layer, a semi-decarburization layer, and a high-temperature oxide, then it is determined that the crack source of the bird's nest crack is the crack on the surface of the ingot, and the bird's nest crack has been formed before the ingot is rolled and heated.
[0027] The present invention provides a method for detecting bird's nest cracks of a casting billet, which has the beneficial effects that: the method for detecting bird's nest cracks of a casting billet cuts a first sample at a position of the fracture sample close to an opening of the bird's nest crack on the casting billet section, cuts a third sample at the core of the fracture sample, cuts a second sample between the first sample and the third sample, and performs inspection based on the first sample, the second sample and the third sample to obtain morphological characteristics, high-temperature oxide characteristics and decarburization layer characteristics on one side of the bird's nest crack fracture, and comprehensively analyzes the morphological characteristics, high-temperature oxide characteristics and decarburization layer characteristics on one side of the bird's nest crack fracture, so as to accurately determine the crack source of the bird's nest crack and the process in which the bird's nest crack is generated, thereby improving the accuracy of detecting the bird's nest crack of the casting billet and the reliability of the detection result.
[0028] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The above and other objects, features and advantages of the present invention will become more apparent through a more detailed description of exemplary embodiments of the present invention in conjunction with the accompanying drawings, wherein like reference numerals generally represent like components throughout the exemplary embodiments of the present invention.
[0030] Figure 1 A flow chart of a method for detecting bird's nest cracks in a casting according to an embodiment of the present invention is shown.
[0031] Figure 2 A schematic diagram of a bird's nest crack of a casting billet according to an embodiment of the present invention is shown.
[0032] Figure 3 A schematic diagram showing a cutting position of a casting slab according to an embodiment of the present invention.
[0033] Figure 4 A schematic diagram of a saw cut on a cast billet segment according to an embodiment of the present invention is shown.
[0034] Figure 5 A schematic diagram of a fracture specimen according to an embodiment of the present invention is shown.
[0035] Figure 6 A schematic diagram showing sampling positions and detection surfaces of a first sample, a second sample, and a third sample according to an embodiment of the present invention is shown.
[0036] Description of reference numerals:
[0037] 11. Ingot; 12. Opening; 13. Linear crack; 21. Cutting position; 31. Saw cut surface; 32. Fracture specimen; 33. Bird's nest crack fracture; 34. Fracture section; 41. First specimen; 42. Second specimen; 43. Third specimen; 44. Inspection surface. DETAILED DESCRIPTION
[0038] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.
[0039] like Figures 1 to 6 As shown, the present invention provides a method for detecting bird's nest cracks in a casting, comprising:
[0040] Cutting a casting segment with a bird's nest crack from the casting 11;
[0041] Cutting the ingot segment along the cross section of the ingot segment at the bird's nest crack to obtain at least one fracture sample 32;
[0042] A first sample 41, a second sample 42 and a third sample 43 are cut from a fracture sample 32, the first sample 41 is close to the opening 12 of the bird's nest crack on the ingot segment, the third sample 43 is in the core of the fracture sample 32, and the second sample 42 is between the first sample 41 and the third sample 43;
[0043] The first sample 41, the second sample 42 and the third sample 43 are inspected to obtain the morphological characteristics, high temperature oxide characteristics and decarburized layer characteristics of one side of the bird's nest crack fracture 33;
[0044] According to the morphological characteristics, high-temperature oxide characteristics and decarburization layer characteristics, the crack source and occurrence time of the bird's nest crack are determined.
[0045] Specifically, in order to solve the problem that the detection of bird's nest cracks in the ingot 11 in the prior art is not accurate enough and the detection results are not reliable enough, the bird's nest crack detection method for the ingot 11 provided by the present invention cuts a first sample 41 at a position of the fracture sample 32 close to the opening 12 of the bird's nest crack on the ingot section, cuts a third sample 43 at the core of the fracture sample 32, and cuts a second sample 42 between the first sample 41 and the third sample 43. The first sample 41, the second sample 42 and the third sample 43 are inspected to obtain the morphological characteristics, high-temperature oxide characteristics and decarburization layer characteristics of one side of the bird's nest crack fracture 33. The morphological characteristics, high-temperature oxide characteristics and decarburization layer characteristics of one side of the bird's nest crack fracture 33 are comprehensively analyzed, so as to accurately determine the crack source of the bird's nest crack and the process in which the bird's nest crack is generated, thereby improving the accuracy of the detection of the bird's nest crack in the ingot 11 and the reliability of the detection results.
[0046] Optionally, cutting a casting billet segment with a bird's nest crack on the casting billet 11 comprises:
[0047] Determine the location of the cracks in the bird's nest;
[0048] A cutting position 21 is set on both sides of the bird's nest crack along the axial direction of the ingot 11, and the distance between the cutting position 21 and the bird's nest crack is a set distance;
[0049] The strand segment is cut off along the cutting position 21 .
[0050] Specifically, the location of the bird's nest crack can be determined by observation, such as Figure 2 As shown, the bird's nest crack on the ingot 11 forms an opening 12 on the surface of the ingot 11, and a bird's nest-shaped cavity is formed inside the opening 12. Some of the surfaces of the ingots 11 also have linear cracks 13 formed after the openings 12 are pressed together. After determining the location of the bird's nest crack, two cutting positions 21 can be determined, such as Figure 3 As shown, the cutting position 21 can be 100-110 mm away from the bird's nest crack; after the cutting position 21 is determined, the ingot 11 can be cut along the cutting position 21 to cut off the ingot section with the bird's nest crack.
[0051] Optionally, the ingot segments are cut by sawing.
[0052] Specifically, when cutting the ingot segment with the bird's nest crack, sawing can be used.
[0053] Optionally, the ingot segment is cut along a sawing surface 31 by sawing, and the sawing surface 31 passes through an opening 12 of the bird's nest crack on the ingot segment.
[0054] Specifically, after obtaining the billet segment with the bird's nest crack, it is necessary to set the sawing surface 31, and the sawing surface 31 needs to pass through the opening 12 formed by the bird's nest crack on the surface of the billet segment, such as Figure 4 As shown, the ingot segment can be cut along the cross section of the ingot segment at a position approximately in the middle of the opening 12, so that at least one fracture sample 32 can be obtained; Figure 5 As shown, the interior of the fracture sample 32 is a bird's nest crack fracture 33, that is, a bird's nest-shaped cavity, and there are fracture sections 34 at the four corners of the bird's nest-shaped cavity, that is, the cross section of the ingot 11 cut along the sawing surface 31.
[0055] Optionally, before cutting the first sample 41 , the second sample 42 and the third sample 43 , a sampling position is marked on one side of the bird's nest crack fracture 33 of the fracture sample 32 .
[0056] Specifically, the sampling positions can be marked by drawing marking lines to facilitate subsequent cutting to form the first sample 41 , the second sample 42 , and the third sample 43 .
[0057] In this embodiment, one side surface of the first specimen 41 is the surface of the ingot segment with the opening 12, the second specimen 42 is at one quarter of the bird's nest crack fracture 33, and the third specimen 43 is at the center of the bird's nest crack fracture 33, that is, the center of the third specimen 43 is on the first center line of the cross section of the ingot segment. If a second center line of the cross section of half the ingot segment is made on one side of the first center line, then the center of the second specimen 42 is on the second center line, so that the second specimen 42 is at one quarter of the bird's nest crack fracture 33.
[0058] Optionally, the sampling positions of the first sample 41 , the second sample 42 and the third sample 43 are all marked as rectangles.
[0059] Specifically, the sampling positions of the first sample 41, the second sample 42 and the third sample 43 can be drawn into a rectangle of 20 mm×20 mm, and can be sawed by a band saw to form block samples of approximately 20 mm×20 mm×20 mm.
[0060] Optionally, before inspecting the first specimen 41, the second specimen 42 and the third specimen 43, a detection surface 44 is selected, the detection surface 44 of the first specimen 41 is a cutting surface close to one side of the bird's nest crack fracture 33 and perpendicular to the surface of the opening 12 with the bird's nest crack on the ingot segment, and the detection surfaces 44 of the second specimen 42 and the third specimen 43 are coplanar with the detection surface 44 of the first specimen 41.
[0061] Specifically, for the first sample 41, Figure 6 As shown, the selection of the detection surface 44 requires selecting a cutting surface close to the side of the bird's nest crack fracture 33 and perpendicular to the outer surface of the side of the ingot segment with the opening 12. There are two such cutting surfaces. For the second sample 42 and the third sample 43, the selection of the detection surface 44 can be based on the orientation of the detection surface 44 of the first sample 41.
[0062] Optionally, the detection surface 44 is further ground and polished to make the detection surface 44 meet the metallographic inspection requirements.
[0063] Specifically, the inspection surfaces 44 of the first sample 41 , the second sample 42 and the third sample 43 need to be ground and polished on a grinding and polishing machine, and the inspection surfaces 44 after grinding and polishing meet the metallographic inspection requirements, that is, no scratches and contamination are allowed.
[0064] Optionally, the inspections performed on the first sample 41, the second sample 42 and the third sample 43 include morphological inspection and metallographic inspection, the morphological characteristics include whether the color of the iron oxide scale is uniform, the high-temperature oxide characteristics include whether high-temperature oxides exist, and the decarburization layer characteristics include whether a complete decarburization layer and a semi-decarburization layer exist.
[0065] Specifically, the morphology inspection can check whether the color of the oxidized iron scale is uniform, the metallographic inspection of the detection surface 44 before corrosion can check whether high-temperature oxides exist, and the metallographic inspection of the detection surface 44 after corrosion can check whether a completely decarburized layer and a semi-decarburized layer exist.
[0066] In this embodiment, the inspection surfaces of the first sample 41, the second sample 42 and the third sample 43 are subjected to morphological inspection and metallographic inspection before corrosion to obtain morphological characteristics and high-temperature oxide characteristics. Thereafter, the inspection surfaces are corroded with 4% nitric acid alcohol solution for 10 seconds and then blown dry to perform metallographic inspection after corrosion to obtain the characteristics of the decarburized layer.
[0067] Optionally, judging the crack source and cause of the bird's nest crack based on the morphological characteristics, high temperature oxide characteristics and decarburized layer characteristics includes:
[0068] If the color of the iron oxide scale on one side of the bird's nest crack fracture 33 is uniform, and the structure on one side of the bird's nest crack fracture 33 of the first sample 41 is that there is no complete decarburization layer and no high-temperature oxide, it is determined that the crack source of the bird's nest crack is the stress crack in the core of the ingot 11, and the bird's nest crack is formed during the rolling process;
[0069] If the color of the iron oxide scale on one side of the bird's nest crack fracture 33 is uneven, the structure of one side of the bird's nest crack fracture 33 of the first sample 41 is that there is a complete decarburization layer, a semi-decarburization layer, and a high-temperature oxide, and the structure of one side of the bird's nest crack fracture 33 of the second sample 42 and the third sample 43 is that there is a complete decarburization layer, a semi-decarburization layer, and a high-temperature oxide, then it is determined that the crack source of the bird's nest crack is the crack on the surface of the ingot 11, and the bird's nest crack has been formed before the ingot 11 is rolled and heated.
[0070] Specifically, the cause of the bird's nest cracks in the ingot 11 is determined by comprehensively analyzing the macroscopic morphological inspection and metallographic inspection results of the first sample 41, the second sample 42 and the third sample 43; if the color of the iron oxide scale on one side of the bird's nest crack fracture 33 is uniform, and the structure on one side of the bird's nest crack fracture 33 of the first sample 41 is free of a completely decarburized layer and high-temperature oxides, it is determined that the bird's nest cracks are formed in the rolling process, and the crack source of the bird's nest cracks is the stress cracks in the core of the ingot 11, that is, the bird's nest cracks are generated in the steel rolling process. If the color of the iron oxide scale on one side of the bird's nest crack fracture 33 is uneven, the structure of one side of the bird's nest crack fracture 33 of the first sample 41 is a full decarburization layer + a semi-decarburization layer (the thickness is close to the matrix semi-decarburization layer) + a high-temperature oxide, and the structure of one side of the bird's nest crack fracture 33 of the second sample 42 and the third sample 43 is a full decarburization layer + a slight semi-decarburization layer + a small amount of high-temperature oxide, then it is determined that the bird's nest crack is a crack that already existed in the ingot 11 before rolling and heating, that is, the crack source of the bird's nest crack is the surface crack of the ingot 11, which is generated in the steelmaking process.
[0071] In summary, the bird's nest crack detection method for the ingot 11 provided by the present invention cuts the first sample 41, the second sample 42 and the third sample 43 from the opening 12 of the bird's nest crack of the fracture sample 32, one quarter of the bird's nest crack fracture 33 and the core of the bird's nest crack fracture 33 respectively, and comprehensively analyzes whether the bird's nest crack is generated in the steelmaking or steel rolling process and the causes of the bird's nest crack of the ingot 11 based on the morphological characteristics, high-temperature oxide characteristics and decarburization layer characteristics of the first sample 41, the second sample 42 and the third sample 43, so that the detection of the bird's nest crack of the ingot 11 is more accurate and reliable.
[0072] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A method for detecting bird's nest cracks in a casting, characterized in that: include: Cutting a casting section with bird's nest cracks on the casting; Cutting the ingot segment along the cross section of the ingot segment at the bird's nest crack to obtain at least one fracture specimen; Cutting a first sample, a second sample and a third sample from a fracture sample, wherein the first sample is close to the opening of the bird's nest crack on the ingot segment, the third sample is located at the core of the fracture sample, and the second sample is located between the first sample and the third sample; Inspecting the first sample, the second sample and the third sample to obtain morphological characteristics, high-temperature oxide characteristics and decarburized layer characteristics on one side of the bird's nest crack fracture; The crack source and generation timing of the bird's nest crack are determined according to the morphological characteristics, the high-temperature oxide characteristics and the decarburized layer characteristics.
2. The method for detecting bird's nest cracks in a casting according to claim 1, characterized in that: The ingot sections with bird's nest cracks cut from the ingot include: Determine the location of the cracks in the bird's nest; A cutting position is set on both sides of the bird's nest crack along the axial direction of the ingot, and the distance between the cutting position and the bird's nest crack is the set distance; The ingot segment is cut off along the cutting position.
3. The method for detecting bird's nest cracks in a casting according to claim 2, characterized in that: The ingot segments are cut by sawing.
4. The method for detecting bird's nest cracks in a casting according to claim 1, characterized in that: The ingot segment is cut along a sawing surface by sawing, and the sawing surface passes through the opening of the bird's nest crack on the ingot segment.
5. The method for detecting bird's nest cracks in a casting according to claim 1, characterized in that: Before cutting the first, second and third specimens, the sampling position is marked on the side of the bird's nest crack fracture of the fracture specimen.
6. The method for detecting bird's nest cracks in a casting according to claim 5, characterized in that: The sampling positions of the first sample, the second sample and the third sample are all marked as rectangles.
7. The method for detecting bird's nest cracks in a casting according to claim 1, characterized in that: Before inspecting the first specimen, the second specimen and the third specimen, a detection surface is selected. The detection surface of the first specimen is a cutting surface close to one side of the bird's nest crack fracture and perpendicular to the surface of the opening with the bird's nest crack on the ingot segment. The detection surfaces of the second specimen and the third specimen are coplanar with the detection surface of the first specimen.
8. The method for detecting bird's nest cracks in a casting according to claim 7, characterized in that: The method also includes grinding and polishing the detection surface so that the detection surface meets the metallographic inspection requirements.
9. The method for detecting bird's nest cracks in a casting according to claim 1, characterized in that: The inspections performed on the first sample, the second sample and the third sample include morphological inspection and metallographic inspection. The morphological characteristics include whether the color of the iron oxide scale is uniform, the high-temperature oxide characteristics include whether high-temperature oxides exist, and the decarburization layer characteristics include whether a complete decarburization layer and a semi-decarburization layer exist.
10. The method for detecting bird's nest cracks in a casting according to claim 9, characterized in that: According to the morphological features, the high temperature oxide features and the decarburized layer features, the crack source and the cause of the Bird's Nest crack are judged as follows: If the color of the iron oxide scale on one side of the bird's nest crack fracture is uniform, and the structure on one side of the bird's nest crack fracture of the first sample is that there is no complete decarburization layer and no high-temperature oxide, it is determined that the crack source of the bird's nest crack is the stress crack in the core of the ingot, and the bird's nest crack is formed during the rolling process; If the color of the iron oxide scale on one side of the bird's nest crack fracture is uneven, the structure of one side of the bird's nest crack fracture of the first sample is that there is a complete decarburization layer, a semi-decarburization layer, and a high-temperature oxide, and the structure of one side of the bird's nest crack fracture of the second sample and the third sample is that there is a complete decarburization layer, a semi-decarburization layer, and a high-temperature oxide, then it is determined that the crack source of the bird's nest crack is the crack on the surface of the ingot, and the bird's nest crack has been formed before the ingot is rolled and heated.