Coal graphite evaluation index determination method based on XRD spectral analysis
By optimizing the pretreatment and peak fitting technology of XRD spectral analysis, the peak shape superposition problem in the determination of graphitization of coal-based graphite is solved, the rapid and efficient grade division of coal-based graphite is achieved, and the evaluation index of coal-based graphite is improved. system.
Patent Information
- Application Number
- CN202410980251.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, there is a problem of peak shape superposition in XRD spectral analysis, making it difficult to accurately determine the graphitization degree of coal-based graphite, and there is a lack of economical and applicable raw coal testing methods, which affects the evaluation accuracy of coal-based graphite.
The coal-based graphite evaluation index determination method based on XRD spectrum analysis includes sample pretreatment, internal standard sample preparation, XRD test analysis and peak fitting. Through the optimization of pretreatment method and peak fitting technology, peak shape superposition is avoided. , improve the accuracy of measurement.
The rapid and efficient grade classification of coal-based graphite has been achieved, the coal-based graphite evaluation index system has been improved, and the determination accuracy and economicality have been improved.
Smart Images

Figure CN118914256A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of dental comprehensive treatment machines, and in particular to a method for determining coal-based graphite evaluation indicators based on XRD spectrum analysis. Background Art
[0002] Graphite is an important strategic non-metallic resource and has been widely developed and utilized in recent years (Sun Shenglin et al., 2014). Most of the graphite resources developed and utilized in industry are flake graphite. With the increasing depletion of flake graphite resources, the development and utilization of coal-based cryptocrystalline graphite resources have received more and more attention (Cao Daiyong et al., 2017). Coal-based graphite is derived from coal metamorphism. Due to the continuous transition between coal-based graphite and high-metamorphic anthracite, it is difficult to effectively distinguish them according to the existing graphite mineral specifications. For a long time, it has been mined, sold and utilized as coal, and the research level is relatively low (Liu Qinfu et al., 2018);
[0003] The graphitization process of coal is accompanied by a series of characteristics such as the ordering of organic matter structure, the uniformity of chemical composition and the disappearance of structural defects (Cao et al., 2009; Li et al., 2020). Previous studies have conducted a lot of research on the microscopic changes of coal macromolecular structure during coal thermal evolution (Ross and Bustin, 1990; Qin Yong, 1998; Qin Yong et al., 1999). It is generally believed that with the increase of coal metamorphism, the change of coal structure is mainly accompanied by the continuous increase of aromatic layer structure and lateral stacking growth. According to An Wenbo et al. (2018) and Wang Chao et al. (2019), Raman and infrared spectroscopy can analyze the functional group characteristics and functional group content of coal with different metamorphic degrees. However, due to the complex composition of coal and the large number of functional groups, analysis and identification are difficult. It is questionable to measure the overall metamorphic effect of coal by only some of the functional groups. X-ray diffraction analysis takes a large amount of samples, and the information obtained directly reflects the microstructure information of coal (Wang et al., 1999). It is one of the important characterization methods for studying the degree of molecular order and determining the microcrystalline structure of coal. The degree of graphitization estimated by XRD is a reliable approximate indicator of metamorphic level (Wada et al., 1994), which is of great significance to reveal the relationship between the order of carbon microcrystal arrangement and the degree of coal metamorphism (Li Jinze et al., 2020).
[0004] At present, the XRD interlaminar spacing d002 parameter is usually used to characterize the graphitization degree of carbon materials (Xu Juliang et al., 2009), and is used as an important indicator for evaluating the grade of coal-based graphite (Cao Daiyong et al., 2017; Li Huantong et al., 2021). The so-called graphitization degree refers to the degree to which the C atomic arrangement reaches or approaches the graphite crystal structure. Usually, the interlaminar spacing d002 is calculated first, and then calculated by the Franklin (Mering-Maire) formula (Qian Chongliang et al., 2001; Sonibare et al., 2010), but this formula needs to be corrected for the case of graphitization degree > 0.8 (Qi Jingyu, 2003);
[0005] However, there are still many details that need to be discussed in the process of obtaining XRD related experimental parameters, such as ① considering that the broad and gentle peak at 2θ is considered to be the superposition of the (002) peak and the (γ) peak, where the (γ) peak is related to the aliphatic carbon (aliphatic chain and aliphatic ring) structure in the molecule, and the lower the degree of metamorphism, the more developed the aliphatic carbon structure. Therefore, in the process of determining the d002 parameter, how to avoid the influence of peak shape superposition (such as the γ peak) on the peak position; ② Compared with the demineralization pretreatment analysis, is there a more economical and applicable raw coal testing method to replace it (such as the internal standard method); ③ How do other XRD spectral parameters respond to the degree of coal graphitization, and whether they can be included in the evaluation system of coal graphitization indicators. Summary of the invention
[0006] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a method for determining coal-based graphite evaluation indicators based on XRD spectral analysis.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] The method for determining the evaluation index of coal-based graphite based on XRD spectrum analysis comprises the following steps:
[0009] S1. Demineralization sample preparation:
[0010] ① Sample pretreatment: Take 50g of fresh cross-section of the above 7 coal samples, grind and sieve to 200 mesh;
[0011] ② Determination of ash content: weigh 1g of coal sample in an ash dish, place it in a muffle furnace, and burn it at 820℃ until the mass is constant; weigh it after cooling, and then place the coal sample in a muffle furnace and burn it at 820℃ for inspection;
[0012] ③ Ash reduction: weigh 62.6g zinc chloride in a beaker, add 100ml deionized water to make a heavy liquid, weigh 10g coal sample in a 250ml beaker, add a small amount of heavy liquid, stir until all wet, then add the remaining heavy liquid, stir well, let stand for 5min; filter and rinse with deionized water;
[0013] ④ Acid washing and deashing: Place the deashed coal sample in a 250ml beaker, add 100ml of 6mol / L hydrochloric acid, place the beaker in a water bath at a rotor speed of 300rpm and 55℃, stir and heat for 1h, filter, rinse with deionized water until the rinse liquid is neutral, place in a 250ml plastic measuring cup, add 100ml of 40% hydrofluoric acid, place the plastic measuring cup in a water bath at a rotor speed of 300rpm and 55℃, stir and heat for 1h, filter, rinse with deionized water until the rinse liquid is neutral, and place in a 55℃ oven for drying;
[0014] ⑤ Determination of ash content of deashed coal sample: weigh 1g of deashed coal sample in an ash dish; place it in a muffle furnace and burn it at 820℃ until the mass is constant; weigh it after cooling, place the coal sample in a muffle furnace and burn it at 820℃ for inspection;
[0015] ⑥ Comparing the above two ash content determination results, samples with an ash removal rate of more than 95% are considered qualified samples and are used for testing;
[0016] S2. Preparation of internal standard sample:
[0017] High metamorphic raw coal samples were selected as experimental objects. 20g of samples were taken from fresh sections, ground to 200 mesh, and mixed with standard Si powder in a certain proportion, and finally made into flat plate samples for testing.
[0018] S3. Industrial analysis and elemental analysis: Fresh coal samples were manually selected, and coal samples with a crushed particle size of less than 0.1 mm were used for vitrinite reflectance testing;
[0019] S4. XRD test and analysis: XRD test and analysis are performed on raw coal samples and demineralized samples with different graphitization degrees by X-ray diffractometer to obtain corresponding XRD spectrum diffraction curves and parameter information;
[0020] S5. Peak fitting: Origin software was used to compare and analyze different peak fitting methods of XRD spectrum diffraction curves.
[0021] Preferably, the method for judging whether the rinsing is clean in step ③ is to add two drops of nitrate solution to the rinsing liquid and water respectively, and the emulsification degree thereof is the same.
[0022] Preferably, the standard Si powder in step S2 is 325 mesh size, analytically pure silicon powder with SiO2 content greater than 99%.
[0023] Preferably, the mixing ratio of the standard Si powder in step S2 is one of 10 / 1, 5 / 1, 4 / 1 and 2 / 1.
[0024] Preferably, the instrument used for the XRD test analysis in step S4 is a PHILIPS X'Pert PRO X-ray diffractometer, with a tube voltage of 60KV (Max), an X-ray tube current of 55mA, a step scan, a step size of 2θ=0.1°, a scanning speed of 2° / min, and a scanning range of 2θ=10-70°.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention uses experimental means such as coal quality analysis, coal vitrinite reflectance and XRD to analyze the influence of different peak fitting methods and different sample pretreatment methods on XRD spectrum parameters, and explores the effective determination method and response law of coal-based graphite evaluation indicators based on XRD spectrum analysis, so as to further improve the evaluation index system of coal-based graphite and provide a basis for constructing a fast and efficient coal-based graphitization grade classification system. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more specifically and intuitively illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.
[0028] Figure 1 This is a graph showing the influence of different peak fitting methods proposed in the present invention on the positions of 002 and γ peaks;
[0029] Figure 2 The broad and gentle peak at 2θ proposed by the present invention should be a superimposed peak curve of (002) and γ;
[0030] Figure 3 A bar graph showing the influence of different peak fitting methods proposed in the present invention on the lattice spacing d002 value of the aromatic layer;
[0031] Figure 4 The graph is a graph showing the influence of the raw coal and demineralization treatment on the peak positions of the spectral parameters (002), (100) and the like proposed by the present invention;
[0032] Figure 5 It is a curve diagram showing the variation of 2θ value, half-width FWHM and interplanar spacing d002 under the peak fitting condition proposed by the present invention;
[0033] Figure 6 It is a bar graph showing the variation of 2θ value, half-width FWHM and interplanar spacing d002 under the peak fitting conditions proposed by the present invention;
[0034] Figure 7 This is the XRD spectrum of the sample after adding Si powder to the raw coal proposed by the present invention;
[0035] Figure 8XRD patterns of different raw coal / SiO2 ratios proposed in the present invention;
[0036] Fig. 9 This is a comparison diagram of the peak fitting effects of different raw coal / SiO2 ratios proposed in the present invention;
[0037] Fig.10 The graph of the change of 2θ values of Si(111) plane and C(002) plane under different raw coal / SiO2 ratios proposed by the present invention;
[0038] Fig.11 This is a relationship diagram between different raw coal / SiO2 ratios proposed in the present invention and the corrected (002) peak 2θ value;
[0039] Fig.12 Response curve 1 of different coal quality indicators to XRD spectrum parameter d002 proposed by the present invention;
[0040] Fig.13 The second response curve of different coal quality indicators to XRD spectrum parameter d002 proposed by the present invention;
[0041] Fig.14 This is the response law of different XRD spectrum parameters proposed in the present invention to coal graphitization. DETAILED DESCRIPTION
[0042] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0043] 1. Experimental part:
[0044] 1.1 Sample pretreatment:
[0045] (1) Demineralization sample preparation
[0046] ① Sample pretreatment: Take 50g of fresh cross-section of the above 7 coal samples, grind and sieve to 200 mesh;
[0047] ② Determination of ash content: weigh 1g of coal sample into an ash dish, place it in a muffle furnace, burn it at 820℃ until the mass is constant, weigh it after cooling, and then place the coal sample in a muffle furnace and burn it at 820℃ for inspection;
[0048] ③ Ash reduction: weigh 62.6g zinc chloride in a beaker, add 100ml deionized water to make a heavy liquid; weigh 10g coal sample in a 250ml beaker, add a small amount of heavy liquid, stir until all wet, then add the remaining heavy liquid, stir well, let stand for 5min, filter, and rinse with deionized water (the sign of rinsing clean: add two drops of nitrate solution to the rinse liquid and water respectively, and the degree of turbidity is the same);
[0049] ④ Acid washing and deashing: Place the deashed coal sample in a 250ml beaker and add 100ml 6mol / L hydrochloric acid; place the beaker in a water bath at a rotor speed of 300rpm and 55℃, stirring and heating for 1h; filter, rinse with deionized water until the rinse liquid is neutral, place in a 250ml plastic measuring cup, add 100ml 40% hydrofluoric acid, place the plastic measuring cup in a water bath at a rotor speed of 300rpm and 55℃, stirring and heating for 1h; filter, rinse with deionized water until the rinse liquid is neutral, and place in a 55℃ oven to dry;
[0050] ⑤ Determination of ash content of deashed coal sample: weigh 1g of deashed coal sample in an ash dish; place it in a muffle furnace and burn it at 820℃ until the mass is constant, weigh it after cooling, place the coal sample in a muffle furnace and burn it at 820℃ for inspection;
[0051] ⑥ Comparing the above two ash determination results, samples with an ash removal rate of more than 95% are considered qualified samples and used for XRD test analysis.
[0052] 2) Preparation of internal standard sample
[0053] In order to study the effect of different ratios of coal and standard Si powder on improving the height of the diffraction peak of Si (111) plane of the sample and the peak fitting, high metamorphic coal samples were selected as experimental objects, 20 g of samples were taken from the fresh section and ground into 200 mesh; the purchased standard Si powder (325 mesh, analytical grade, SiO2 content greater than 99%) was mixed evenly in certain proportions (10 / 1, 5 / 1, 4 / 1 and 2 / 1), and finally made into flat plate samples for testing.
[0054] 1.2 Industrial analysis and elemental analysis:
[0055] The moisture, ash and volatile matter in coal are determined according to GB / T 212-2008 "Industrial Analysis Methods of Coal"; the elements in coal are determined according to GB / T 31391-2015 "Elemental Analysis of Coal"; fresh coal samples are manually selected, and the coal samples with a crushing particle size of less than 0.1mm are used for vitrinite reflectance test, and the sample preparation complies with the provisions of GB / T16773-2008 "Preparation Methods for Coal and Rock Analysis Samples"; the vitrinite reflectance of coal is determined according to GB / T6948-2008 "Microscopic Determination Method of Vitrinite Reflectance of Coal"; the above experimental test work was completed at Jiangsu Geology and Mineral Resources Design and Research Institute, and the test results are shown in Table 1:
[0056] Table 1 Deterioration Degree of Coal and Test Results of Industrial Analysis and Elemental Analysis
[0057]
[0058] Note: ad: air dried basis; d: dry basis; daf: dry ash-free basis; LL: Luling Coal Mine; QD: Qidong Coal Mine; YY: Yuanyi Coal Mine; WLH: Wolonghu Coal Mine; ZZ: Zhuzhuang Coal Mine; LQ: Liuqiao No. 2 Coal Mine; SL: Shuanglong Coal Mine.
[0059] 1.3XRD test analysis:
[0060] Table 2 Test and analysis results of XRD spectral parameters
[0061]
[0062]
[0063] Note: FWHM: half-width; d002: aromatic layer spacing; Lc: average aromatic layer stacking thickness; La: ductility of the aromatic layer; N: number of carbon atom network stacking layers; G: degree of graphitization.
[0064] X-ray diffraction analysis was completed in the Physical and Chemical Experiment Center of the University of Science and Technology of China. The experimental instrument was a PHILIPS X'Pert PRO X-ray diffractometer with a tube voltage of 60KV (Max) and an X-ray tube current of 55mA. The step-by-step scanning method was adopted, with a step size of 2θ=0.1°, a scanning speed of 2° / min, and a scanning range of 2θ=10-70°. XRD tests and analyses were carried out on raw coal and demineralized samples of different graphitization degrees in the Huaibei coalfield. The XRD spectrum parameter test and analysis results of the demineralized samples are shown in Table 2. The (002) peak and (γ) peak in Table 2 are fitted by the broad and gentle peaks near 26° (fitted by sampling Origin software). The parameters such as d002, Lc, and La were mainly calculated using the Bragg equation and the Scherre formula (Sonibare et al., 2010). The graphitization degree G was calculated using the modified formula of Mering and Marie (1958).
[0065] 2. Results and Discussion
[0066] 2.1 The influence of different peak fitting methods on XRD spectrum parameters:
[0067] The peak fitting of XRD spectrum can obtain the corresponding peak position, diffraction intensity and half-peak width. Combined with Bragg equation and Scherre formula, the structural unit parameters such as aromatic layer spacing d002, layer extension La and stacking degree Lc can be calculated. In particular, the reasonable determination of the (002) peak position is more critical. However, different peak fitting methods have different degrees of influence on the acquisition of spectral parameters, such as whether to subtract the background, whether to consider the influence of superimposed peaks, and whether the peak separation results are unique. Relevant scholars have pointed out that the selection of the method for subtracting the background has a greater impact on the final experimental results; since the existence of the γ band peak is not considered (the broad and gentle peak at 2θ is considered by most scholars to be the superposition of the (002 peak) and the (γ) band), the peak value taken as the highest point when measuring d002 is often inaccurate, and the peak at 44°2θ should be the superposition peak of the (100) peak and the (101) peak.
[0068] In order to solve the above problems, the demineralized samples of Wolonghu Coal Mine (No.: WLH) in Huaibei Coalfield were taken as an example, and different peak fitting methods were compared and analyzed using Origin2018 software. Figure 1-3 It can be seen that different peak fitting methods have a great influence on the determination of the (002) peak position, as shown in the following:
[0069] Depend on Figure 1 , Figure 2 It can be seen that after deducting the bottom, the broad peak at 2θ does have two peaks superimposed, namely, one is the information (γ) peak band generated by the side chains formed by various functional groups, alicyclic hydrocarbons and other aliphatic structures connected to the condensation aromatic core, and the other is the microcrystalline structure (002) peak band in the usual sense formed by the accumulation of condensation aromatic cores (Wang Chao et al., 2019);
[0070] Whether the background and baseline are removed or not has a great influence on the determination of the (002) peak position. Failure to remove the background and baseline will result in a relatively smaller 2θ value of the (002) peak, and a corresponding decrease in the inter-reticular spacing d002 of the aromatic layers.
[0071] Referring to the identification standard of coal-based graphite by Cao Daiyong et al. (2022), the critical value of d002 for coal (anthracite) and semi-graphite is 0.344nm. Figure 3 It can be seen that different peak fitting methods for the same coal sample have a greater impact on the evaluation grade of coal-based graphite. Compared with whether the baseline is removed, whether the bottom back is subtracted has a more obvious impact on the experimental results.
[0072] 2.2 Effect of different pretreatment methods on XRD spectrum parameters:
[0073] Considering that the presence of minerals in raw coal will interfere with the XRD spectrum, demineralization is the most commonly used method to obtain XRD spectrum parameters (d002, d100, FWHM, La / Lc, etc.). At present, the methods for removing minerals from coal can be divided into physical washing and chemical purification. Among them, the chemical purification method has a better effect on the removal of minerals in coal, but in this process, the organic structure of the coal itself may also be affected to a certain extent. In order not to destroy the structure of the coal itself, but to reduce the pre-treatment cost and accurately reflect the XRD spectrum information, Xu Juliang et al. (2009) ) proposed the internal standard method, that is, by mixing raw coal and standard Si powder in a certain proportion and conducting XRD spectrum test and analysis, the diffraction peak of Si (111) crystal plane is used to correct the position of the carbon material (002) peak, which helps to eliminate the system error. Therefore, based on the above understanding, this time, on the basis of comparing the influence of different pretreatment methods on XRD spectrum parameters, the optimal ratio of raw coal and standard Si powder in practical application of the internal standard method is discussed and determined, aiming to provide a method reference for simply and quickly obtaining coal XRD spectrum parameters such as d002, as detailed as follows:
[0074] (1) Demineralization
[0075] Depend on Figure 4 It can be seen that without considering the (γ) peak, the 2θ values at the (002) peak of the raw coal and demineralized samples are 25.565° and 25.628° respectively; considering the (γ) peak, the 2θ values at the (002) peak of the raw coal and demineralized samples are 25.845° and 26.074° respectively, and show a trend of gradual increase; therefore, different pretreatment methods have a greater influence on the 2θ value at the (002) peak of the sample, and the fitting of the (γ) peak has a greater impact on the experimental analysis results; compared with the raw coal, the demineralized sample has a (100) peak near 2θ of 43°, and the peak fitting effect is better, while the XRD spectrum curve of the raw coal cannot effectively fit the (100) peak to convergence;
[0076] Figure 5 , Figure 6 The variation of (002) peak 2θ value, half-width FWHM and interplanar spacing d002 under different pre-treatment and peak fitting conditions;
[0077] Depend on Figure 5 It can be seen that in the process of XRD peak fitting, the superposition of (γ) peak and demineralization factors has a positive correlation with the 2θ value of (002) peak, but a negative correlation with the half-height width FWHM value;
[0078] Depend on Figure 6It can be seen that different pretreatment methods have a great influence on the important parameter index d002 of coal-based graphite, which directly affects the classification and identification of the graphitization grade of the sample (that is, under conditions A, B and C, referring to the identification standard of coal-based graphite by Cao Daiyong et al. (2022), the degree of graphitization of the sample is not high, and it is bituminous coal or anthracite; under conditions D, the degree of graphitization of the sample can be identified as semi-graphite).
[0079] (2) Internal standard method
[0080] The XRD spectrum of the coal sample after adding standard Si powder is shown in Figure 7 , where n is the shape of the amorphous bulge of the ungraphitized carbon material, which is the widest, and the (γ) peak band; c is the diffraction peak of the graphitized C(002) crystal plane; Si is the diffraction peak of the internal standard phase Si(111) crystal plane, which is the sharpest, and the position of the standard Si(111) crystal plane diffraction peak is 28.443°(2θ); the outermost contour line is formed by the superposition of the three, that is, the diffraction spectrum obtained in the sample test; when determining d002, the diffraction spectrum is firstly separated and fitted by the peak fitting software to solve 2θC(002) and 2θSi(111), and then corrected by [2θC(002)-2θSi(111)+28.443°] and inserted into the Bragg equation 2dsinθ=λ to calculate the accurate d002; this time, the XRD spectrum curve analysis under different raw coal and standard Si powder ratio conditions aims to explore the appropriate ratio of raw coal and standard Si powder and the feasibility of the internal standard method in actual operation;
[0081] Depend on Figure 8 It can be seen that as the proportion of standard Si powder added to the raw coal gradually increases, the diffraction peak height of the sample Si (111) plane gradually increases, and the diffraction peak height from the C (002) plane gradually decreases (see D1 to D4 in the figure), especially after raw coal / SiO2 < 4:1, the diffraction peak height difference decreases significantly, showing that the diffraction peak heights are roughly the same;
[0082] In addition, in order to further verify the feasibility of the internal standard method, the peak fitting effects of demineralized samples and different raw coal / standard Si powder ratios were compared ( Fig. 9 ),Depend on Fig.10 It can be seen that as the proportion of standard Si powder added to the raw coal gradually increases, the performance is as follows:
[0083] ①The change trends of Si(111) and C(002) peak positions are relatively consistent, with the inflection point at raw coal / SiO2=4:1;
[0084] ② By using the formula [2θC(002)-2θSi(111)+28.443°] for correction, it is found that the corrected C(002) peak value shows a trend of gradually increasing, especially when the raw coal / SiO2 ratio is greater than 4:1, the C(002) peak value increases significantly and is close to the (002) peak value of the demineralized sample (2θ=25.911°); in addition, in order to further clarify the ratio of raw coal to standard Si powder in the internal standard method and improve the feasibility and accuracy of the internal standard method in actual application, the corrected C(002) peak position values under different raw coal / SiO2 conditions are fitted with polynomials ( Fig.11 );
[0085] Depend on Fig.11 It can be seen that compared with the demineralization method, under the condition of a mass ratio of raw coal / SiO2=3:1, the internal standard method can effectively determine the 2θ value of the sample (002) peak, and calculate the accurate d002 according to the Bragg equation 2dsinθ=λ, so as to achieve the purpose of quickly, efficiently and low-costly classification of coal-based graphite grades.
[0086] 2.3 Analysis of the response of different coal quality parameters to XRD spectrum parameter d002:
[0087] During the coalification and graphitization stages, with the continuous degradation and gradual aromatization of aromatic compounds in coal, the coal quality parameters such as coal vitrinite reflectance, volatile matter, H / C, etc. also show different change patterns; among them, the maximum reflectance Ro,max index of coal vitrinite is closely related to the degree of condensation of aromatic fused rings and carbon atom density in coal, and is often used as an important index to determine coal rank and distinguish coalification and graphitization; the dry ash-free volatile matter Vdaf, as a thermal decomposition product of coal, can indirectly reflect the thermal degradation degree of small molecules such as side chains and functional groups in the coal structure; because this index is The universality, ease and low cost of coal quality testing can be used as a reference indicator for preliminary judgment of the degree of coal graphitization; the hydrogen-carbon atomic ratio H / C reflects the dehydrogenation and carbon-enrichment evolution process in the process of coalification and graphitization, and is simple and practical, and has been initially applied in the classification of coal graphitization grades at home and abroad; fixed carbon FCad, also a thermal decomposition product of coal, is an important parameter indicator for classifying graphite grades in the current "Specifications for Geological Exploration of Graphite and Broken Mica Minerals" (FCad ≥ 65% is the boundary grade of graphite), but the classification and identification of coal-based cryptocrystalline graphite remains to be discussed.
[0088] Considering that XRD spectrum parameter d002 is an important index for identifying coal-based graphite and classifying coal-based graphite types, in order to explore the response characteristics of different coal quality indicators of the main coal mines in Huaibei Coalfield to XRD spectrum parameter d002, Ro, max, Vdaf, H / C and FCad were selected for correlation analysis with d002; considering that d002 = 0.344nm is the starting point of graphitization of carbon materials, and d002 = 0.3554nm is the end point of ideal graphite (Franklin, 1951), this paper focuses on the quantitative analysis of coal quality parameter indicators at d002 = 0.344nm;
[0089] Depend on Fig.12 , Fig.13 It can be seen that the maximum reflectance of the vitrinite group Ro,max, H / C and d002 are negatively correlated (the correlation coefficients R2 are 0.65 and 0.80, respectively), and Vdaf, FCad and d002 are positively correlated (R2 are 0.81 and 0.75, respectively), that is, the influence of different coal quality indicators on the XRD spectrum parameter d002 is ranked as Vdaf>H / C>FCad>Ro,max, as can be seen from the above ranking;
[0090] (1) Vdaf, H / C and d002 parameters are highly correlated and can be used as reference indicators for preliminary identification of the degree of coal graphitization in theory. Considering that Vdaf mainly comes from thermal decomposition products of inorganic minerals and some small molecular organic matter and attachments, and H / C is mainly a physical change in the graphitization stage, and has no strict correspondence with the ordering of the aromatic layer structure, Vdaf and H / C coal quality parameter indicators may lack universal applicability to some extent (for example, according to Cao Daiyong et al. (2021), the Vdaf data of semi-graphite and graphite samples in coal series in Hunan, Fujian, Jiangxi, Shaanxi and other places are mostly concentrated in 2.5-6.5%). However, for local areas, they can still be recommended as the main coal quality parameter indicators for the identification of coal series graphite in Huaibei Coalfield;
[0091] (2) FCad and Ro,max have a low correlation with the d002 parameter and are not theoretically used as reference indicators for preliminary judgment of the degree of coal graphitization. The reasons are as follows: first, FCad can only reflect the quality characteristics of coal and coal-based graphite and has nothing to do with the degree of coal graphitization; second, affected by the randomness and anisotropy of the arrangement of coal-based graphite microcrystals, the dispersion of Ro,max at different graphitization stages is large, which greatly reduces the sensitivity of Ro,max as a coal graphitization indicator.
[0092] In addition, by analyzing the coal quality parameter indicators at d002=0.344nm, the main coal quality parameter boundaries of anthracite and semi-graphite in Huaibei Coalfield were indirectly obtained, that is, the sample coal quality indicators Vdaf<20% and H / C>0.035 can be used as critical signs that the coal metamorphism in Huaibei Coalfield enters the semi-graphite and graphitization stages. The above coal quality indicators provide a reference basis for quickly and easily identifying and identifying the graphite grade of coal series in Huaibei Coalfield.
[0093] 2.4 Analysis of the response of different XRD spectrum parameters to coal graphitization:
[0094] There are many spectral parameters for characterizing the graphitization degree of coal based on XRD, such as 2θ, d002, FWHM, Lc, La, La / Lc, stacking layer number N and graphitization degree G; with the increase of coal metamorphism, the aromatic layer structure gradually becomes regular and orderly, the d002 diffraction peak width becomes narrower, and d002 also tends to decrease; however, due to the influence of the newly formed components with different graphitization degrees in the coal graphitization process, d002 is not enough to represent the maximum evolution degree of the sample, and it is necessary to comprehensively consider the comprehensive characterization of other microcrystalline parameters (such as Lc, La, La / Lc and N); the formation of coal-based graphite is the result of the combined action of internal coal quality, external temperature, pressure and mineral catalysis, as shown in the above XRD parameters. Among the indexes, La is related to the heating temperature of coal, and Lc is related to the stress (extrusion pressure and static pressure) environment of coal; in order to explore the response law of different XRD spectral parameters to coal graphitization, the XRD spectral parameters (d002, γ peak 2θ and FWHM, Lc, La, La / Lc, N) of 7 coals with different metamorphic degrees in Huaibei coalfield under demineralization treatment and considering (γ) peak conditions were statistically analyzed (Table 2). Among them, LL and QD samples cannot effectively fit the (100) peak near 2θ of 43° due to the low degree of coal metamorphism (Ro, max are 0.79% and 1.01%, respectively), so the corresponding XRD spectral parameters La and La / Lc cannot be statistically analyzed. Through the analysis of the response law of different XRD spectral parameters to coal graphitization, it can be seen that ( Fig.14 ), the fitting effect of La, La / Lc and γ peak 2θ and d002 is good (R2 is between 0.78-0.97, and the correlation is La>La / Lc>γ peak 2θ), and the fitting effect of other XRD spectrum parameters is not good (R2 is between 0.32-0.34). Therefore, it is preliminarily concluded that XRD spectrum parameters such as La, La / Lc and γ peak 2θ can also be considered as important coal structure indicators for evaluating the degree of graphitization of coal;
[0095] In addition, as mentioned above, by analyzing other XRD spectral parameters at d002=0.344nm, the boundaries of other XRD spectral parameters of anthracite and semi-graphite in Huaibei coalfield can be indirectly obtained, that is, La≈4nm; La / Lc≈1; γ peak 2θ=24.4°; in view of the fact that the correlation coefficient between La and La / Lc parameters and d002 is greater than 90%, La, La / Lc and d002 indicators can be recommended as the main structural indicators for evaluating the grade of coal-based graphite, that is, samples La<4nm, La / Lc<1, d002<0.344nm are semi-graphite and graphitized stages of coal. The above coal structural indicators combined with coal quality indicators provide a data basis for the construction of a rapid and efficient coal-based graphitization grade classification system.
[0096] 3. Conclusion
[0097] (1) Different peak fitting methods have a great influence on the evaluation grade of coal-based graphite. Compared with whether the baseline is removed, whether the background is removed has a more obvious impact on the experimental results.
[0098] (2) Compared with the raw coal, the demineralized sample has a (100) peak near 2θ of 43°, and the peak fitting effect is better, while the XRD spectrum curve of the raw coal cannot effectively fit the (100) peak to convergence; the fitting of the (γ) peak has a greater impact on the experimental analysis results, and directly affects the classification and identification results of the graphitization degree of the sample.
[0099] (3) Under the condition of a mass ratio of raw coal / SiO2=3:1, the internal standard method can effectively determine the 2θ value of the (002) peak of the raw coal sample. The experimental effect is equivalent to that of the demineralization method, which provides a way to simply and quickly obtain coal XRD spectral parameters such as d002.
[0100] (4) The influence of different coal quality indicators on XRD spectrum parameter d002 is ranked as Vdaf>H / C>FCad>Ro,max, among which Vdaf and H / C can be recommended as the main coal quality parameter indicators for the identification of coal-bearing graphite in Huaibei Coalfield; the sample coal quality indicators Vdaf<20% and H / C>0.035 can be used as critical signs that the coal metamorphism in Huaibei Coalfield enters the semi-graphite and graphitization stages.
[0101] (5) The fitting effect of La, La / Lc and γ peak 2θ and d002 is good (R2 is between 0.78-0.97, and the correlation is ranked as La>La / Lc>γ peak 2θ). La, La / Lc and d002 can be recommended as the main structural parameter indicators for the identification of coal-bearing graphite in Huaibei Coalfield. The sample structural indicators La<4nm, La / Lc<1, d002<0.344nm can be used as the critical signs of coal metamorphism entering the semi-graphite and graphitization stages in Huaibei Coalfield. By organically combining the above-mentioned recommended coal structural indicators with coal quality indicators, a basis is provided for the construction of a rapid and efficient coal-bearing graphitization grade classification system.
[0102] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for determining coal-based graphite evaluation index based on XRD spectral analysis, characterized in that: The following steps are involved: S1. Demineralization sample preparation: ① Sample pretreatment: Take 50g of fresh cross-section of the above 7 coal samples, grind and sieve to 200 mesh; ② Determination of ash content: weigh 1g of coal sample into an ash dish, place it in a muffle furnace, and burn it at 820℃ until the mass is constant; After cooling, weigh it, and then place the coal sample in a muffle furnace and burn it at 820℃ for inspection; ③ Ash reduction: weigh 62.6g zinc chloride into a beaker, add 100ml deionized water to make a heavy liquid, weigh 10g coal sample into a 250ml beaker, add a small amount of heavy liquid, stir until all wet, then add the remaining heavy liquid, stir well, let stand for 5min; filter and rinse with deionized water; ④ Acid washing and deashing: Place the deashed coal sample in a 250ml beaker, add 100ml of 6mol / L hydrochloric acid, place the beaker in a water bath at a rotor speed of 300rpm and 55℃, stir and heat for 1h, filter, rinse with deionized water until the rinse liquid is neutral, place in a 250ml plastic measuring cup, add 100ml of 40% hydrofluoric acid, place the plastic measuring cup in a water bath at a rotor speed of 300rpm and 55℃, stir and heat for 1h, filter, rinse with deionized water until the rinse liquid is neutral, and place in a 55℃ oven for drying; ⑤ Determination of ash content of deashed coal sample: weigh 1g of deashed coal sample in an ash dish; place it in a muffle furnace and burn it at 820℃ until the mass is constant; After cooling, weigh it and place the coal sample in a muffle furnace and inspect the burning at 820℃; ⑥ Comparing the above two ash content determination results, samples with an ash removal rate of more than 95% are considered qualified samples and are used for testing; S2. Preparation of internal standard sample: High metamorphic raw coal samples were selected as experimental objects. 20g of samples were taken from fresh sections, ground to 200 mesh, and mixed with standard Si powder in a certain proportion, and finally made into flat plate samples for testing. S3. Industrial analysis and elemental analysis: Fresh coal samples were manually selected, and coal samples with a crushed particle size of less than 0.1 mm were used for vitrinite reflectance testing; S4. XRD test and analysis: XRD test and analysis are performed on raw coal samples and demineralized samples with different graphitization degrees by X-ray diffractometer to obtain corresponding XRD spectrum diffraction curves and parameter information; S5. Peak fitting: Origin software was used to compare and analyze different peak fitting methods of XRD spectrum diffraction curves.
2. The method for determining coal-based graphite evaluation index based on XRD spectrum analysis according to claim 1, characterized in that: The method for judging whether the rinsing is clean in step ③ is to add two drops of nitrate solution to the rinsing liquid and water respectively, and the emulsification degree of the two drops of nitrate solution is the same.
3. The method for determining coal-based graphite evaluation index based on XRD spectrum analysis according to claim 1, characterized in that: The standard Si powder in step S2 is 325 mesh size, analytically pure, and has a SiO2 content greater than 99%.
4. The method for determining coal-based graphite evaluation index based on XRD spectrum analysis according to claim 3, characterized in that: The mixing ratio of the standard Si powder in step S2 is one of 10 / 1, 5 / 1, 4 / 1 and 2 / 1.
5. The method for determining coal-based graphite evaluation index based on XRD spectrum analysis according to claim 1, characterized in that: The instrument used for the XRD test analysis in step S4 is a PHILIPS X'Pert PRO X-ray diffractometer, with a tube voltage of 60KV (Max), an X-ray tube current of 55mA, a step scan, a step size of 2θ=0.1°, a scanning speed of 2° / min, and a scanning range of 2θ=10-70°.