Preparation method of adjustable PN type SiC photonic crystal

Through electron beam etching and high-temperature ion implantation technology, adjustable PN-type SiC photonic crystals are prepared, which solves the problems of low efficiency and high cost of SiC photonic crystal preparation in the prior art, and realizes the efficient optical performance and large number of optoelectronic devices. Preparation in scale, suitable for high temperature and high radiation environments.

CN118915198AActive Publication Date: 2024-11-08SOUTH CHINA NORMAL UNIV
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410967062.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

The existing SiC photonic crystal preparation methods are inefficient, costly, and difficult to achieve large-scale rapid preparation and optical performance optimization, which limits the application of optoelectronic devices.

Method used

Using electron beam etching and high-temperature ion implantation technology, adjustable PN-type SiC photonic crystals are prepared through selective etching and doping, achieving rapid, large-scale preparation and photonic crystal size adjustment.

Benefits of technology

It improves the preparation efficiency and optical performance of SiC photonic crystals, realizes efficient control and modulation of optoelectronic devices, is suitable for high-temperature and high-radiation environments, and reduces process costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118915198A_ABST
    Figure CN118915198A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of optoelectronic devices, and particularly discloses a preparation method of an adjustable PN type SiC photonic crystal. The method comprises the steps of substrate preparation and mask layer growth, gluing, exposure and development, electron beam etching (ICP) and subsequent processing, high-temperature ion implantation and activation, SiO2 mask layer removal, new SiO2 mask layer growth, photoetching and etching area definition, and electron beam etching to form the photonic crystal. According to the invention, the purpose of preparing different PN-type SiC photonic crystals is explored through ion implantation bias simulation, so that the purpose of preparing the PN-type SiC photonic crystals capable of being adjusted at will is achieved, the photonic crystals can be rapidly and massively prepared, the required photonic crystals can be obtained through laser cutting according to different size requirements, and the production efficiency is improved. In the preparation process of an electronic device, the PN type and the substrate concentration of the photonic crystal can be freely adjusted to a large extent according to requirements, and reliability and convenience are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of optoelectronic devices, and in particular relates to a method for preparing an adjustable PN-type SiC photonic crystal. Background Art

[0002] The research on SiC photonic crystals is to meet the current demand for high-performance optoelectronic devices, especially in high-voltage and high-frequency applications. At the same time, considering the low efficiency and high cost of traditional preparation methods, the demand for SiC photonic crystals has become more urgent.

[0003] First of all, the preparation of SiC photonic crystals needs to be efficient and low-cost. Although the current preparation methods, such as metal organic chemical vapor deposition (MOCVD) and ion implantation, can achieve the preparation of SiC devices, they have problems such as slow deposition rate and low efficiency, and the equipment needs to be cleaned and maintained regularly, which increases the process cost. Therefore, future preparation methods need to improve preparation efficiency and reduce costs while ensuring device quality, thereby promoting the development of SiC photonic crystal technology.

[0004] Secondly, SiC photonic crystals need to have excellent optical properties. The periodic structure of photonic crystals can regulate the propagation and scattering of light, so SiC photonic crystals need to have adjustable optical band gaps, high refractive index and other characteristics to achieve efficient control and modulation of light. Such characteristics will provide greater flexibility and performance advantages for the design and application of optoelectronic devices.

[0005] In summary, the research on SiC photonic crystals needs to take into account the requirements of preparation efficiency, optical performance and scalability. Only by making progress in these aspects can we promote the development of SiC photonic crystal technology and provide better solutions for the application of optoelectronic devices.

[0006] SiC photonic crystals have some significant advantages over Si photonic crystals, which are of great significance in the field of optoelectronic devices. Since SiC has a larger band gap, SiC photonic crystals can achieve a wider photonic band gap, which makes them more flexible and controllable in optical modulation and photon transmission. This means that SiC photonic crystals can achieve a wider range of optical functions, including optical waveguides, optical switches, and optical modulators. Secondly, SiC photonic crystals have higher thermal stability and radiation resistance. SiC material has excellent thermal conductivity and chemical stability, and can maintain stability in high temperature and high radiation environments. In contrast, Si photonic crystals may experience thermal attenuation or optical performance degradation in high temperature or high radiation environments, limiting their application in some special environments.

[0007] In the current preparation process of photonic crystal materials, it is generally only present in metal oxides, such as ZnO, SnO 2 Most of them are made by chemical etching or high-temperature sintering, which limits the large-scale, rapid and reproducible preparation of photonic crystals. Summary of the invention

[0008] The object of the present invention is to provide a method for preparing a PN-type SiC photonic crystal to solve the problems raised in the above background technology.

[0009] To achieve the above object, the present invention provides the following technical solutions:

[0010] A method for preparing a SiC photonic crystal with adjustable PN type,

[0011] The following steps are involved:

[0012] S1. Substrate preparation and mask layer growth:

[0013] Choose N-type Si substrate: Make sure the substrate surface is clean and free of impurities;

[0014] Vertical LPCVD growth of SiO 2 Mask layer:

[0015] Control the growth conditions to ensure that SiO 2 The thickness of the layer is 2um and covers the Si substrate;

[0016] S2. Gluing, exposure and development:

[0017] Glue coating: on SiO 2 A layer of photoresist is evenly coated on the mask layer to ensure that there are no bubbles or impurities;

[0018] Exposure: Use a photolithography machine to perform exposure and transfer the pattern of the area to be etched to the photoresist;

[0019] Development: The exposed photoresist is removed by a developer, leaving the pattern of the area to be etched;

[0020] S3. Electron beam etching (ICP) and subsequent processing;

[0021] ICP etching:

[0022] The selective etching characteristics of electron beam etching are used to remove SiO2 that is not blocked by photoresist. 2 part;

[0023] During the electron beam etching process, the parameters of the etcher are as follows:

[0024] Pressure: 3mTorr

[0025] Helium Pressure: 4Torr

[0026] PN 2 (Nitrogen flow): 200sccm

[0027] CHF 3 (Trifluoromethane flow): 50sccm

[0028] Duration: 2300s

[0029] Control etching conditions to ensure etching depth and uniformity;

[0030] Acid removal of photoresist:

[0031] Use piranha solution and acid wash to remove residual photoresist on the surface.

[0032] The solution ratio is H 2 SO 4 :H 2 O 2 =3:1, pickling time is 15min to avoid damage to the SiO2 layer;

[0033] Leave the injection window:

[0034] A clear injection window pattern is formed on the SiO2 layer after removing the photoresist and etching;

[0035] Check the integrity and accuracy of the pattern to ensure that it meets the subsequent process requirements;

[0036] S4. High temperature ion implantation and activation:

[0037] Aluminum (Al) ions are implanted into an N-type silicon (Si) substrate at high temperature using an implanter;

[0038] The injected Al ions will change the conductivity type of the original N-type Si, causing its local area to become P-type, thus achieving a PN-type conversion;

[0039] Through the high-temperature activation process, it is ensured that the injected ions can be effectively doped into the silicon crystal and become effective carriers;

[0040] The PN type conversion is achieved through a pre-set process recipe:

[0041] Step 1: Dose: 3.8e13cm^-2; Energy: 370keV; Tilt: 0°; Rotation: 0°; Temperature: 500°C. Heating helps reduce implant damage.

[0042] Step 2: Dose: increased to 1.3e14cm^-2, energy: reduced to 250keV, control the implantation depth; tilt and rotation angles: kept unchanged, 0° and 0° respectively; temperature (temp): maintained at 500℃;

[0043] Step 3: Dose: adjusted to 3.6e13cm^-2; Energy: further reduced to 100keV; Tilt and rotation angles: still 0° and 0°; Temperature: 500℃, the same as the previous step;

[0044] S5. Removal of SiO 2 Mask layer:

[0045] This SiO layer is removed by dry etching and BOE wet immersion. 2 Mask;

[0046] S6. Growth of new SiO 2 Mask layer:

[0047] After removing the old SiO 2 After the layer, a new 1 μm thick SiO layer was grown on the N-type Si substrate using vertical low pressure chemical vapor deposition (LPCVD). 2 Mask layer.

[0048] The SiO grown this time 2 The layer is to prepare for the next photonic crystal etching step;

[0049] S7. Photolithography defines the etching area:

[0050] In SiO 2 Photoresist is coated on the mask layer, and then the area to be etched is defined through exposure and development.

[0051] S8. Electron beam etching to form photonic crystals:

[0052] Use inductively coupled plasma (ICP) etching technology and electron beam etching to selectively remove SiO 2 Mask layer, in this process, the SiO2 not protected by the photoresist 2 The area will be etched away, while the Si material will be retained;

[0053] The final result is a Si photonic crystal structure with a specific pattern.

[0054] Compared with the prior art, the present invention has the following beneficial effects:

[0055] The present invention proposes to use electron beam etching to prepare regular periodic photonic crystals, and can be prepared on a large scale and used for laser cutting, and verified on Si wafers to pave the way for the subsequent preparation of SiC photonic crystals. Furthermore, the purpose of preparing SiC photonic crystals of different PN types is explored through ion implantation bias simulation to achieve the goal of preparing a SiC photonic crystal with PN type that can be adjusted at will. Photonic crystals can be prepared quickly and in large quantities, and the size of photonic crystals required can be laser cut according to different size requirements. In the process of preparing electronic devices, the PN type and substrate concentration of this photonic crystal can be freely adjusted according to the needs to a large extent, which is reliable and convenient. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 This is a schematic diagram of the electron beam etching process of the Si substrate of the present invention;

[0057] Figure 2 It is a schematic diagram of the change of doping concentration with position and the process of N-type silicon to P-type silicon in the present invention;

[0058] Figure 3 It is a schematic diagram of forming a mask layer on the Si substrate of the present invention and applying the glue after exposure and development;

[0059] Figure 4 This is a schematic diagram of the photonic crystal of the present invention. DETAILED DESCRIPTION

[0060] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0061] Example:

[0062] A method for preparing an adjustable PN-type SiC photonic crystal comprises the following steps:

[0063] S1. Substrate preparation and mask layer growth:

[0064] Choose N-type Si substrate: make sure the substrate surface is clean and free of impurities;

[0065] Vertical LPCVD growth of SiO 2 Mask layer:

[0066] Controlling growth conditions to ensure SiO 2 The thickness of the layer is 2um and covers the Si substrate;

[0067] S2. Gluing, exposure and development:

[0068] Gluing: In SiO 2 A layer of photoresist is evenly coated on the mask layer to ensure that there are no bubbles or impurities;

[0069] Exposure: Use a photolithography machine to perform exposure and transfer the pattern of the area to be etched to the photoresist;

[0070] Development: The exposed photoresist is removed by a developer, leaving the pattern of the area to be etched;

[0071] S3. Electron beam etching (I CP) and subsequent processing;

[0072] I CP etching:

[0073] The selective etching characteristics of electron beam etching are used to remove SiO2 that is not blocked by photoresist. 2 part;

[0074] During the electron beam etching process, the parameters of the etcher are as follows:

[0075] Pressure: 3mTorr; Helium Pressure: 4Torr

[0076] PN 2 (Nitrogen flow): 200sccm; CHF 3 (Trifluoromethane flow): 50sccm; Duration: 2300s Control etching conditions to ensure etching depth and uniformity;

[0077] Acid pickling to remove photoresist: Use piranha solution for acid pickling to remove residual photoresist on the surface.

[0078] The solution ratio is H 2 SO 4 :H 2 O 2 =3:1, the pickling time is 15min to avoid damage to the SiO2 layer; leave an injection window: form a clear injection window pattern on the SiO2 layer after removing the photoresist and etching; check the integrity and accuracy of the pattern to ensure that it meets the subsequent process requirements;

[0079] S4. High temperature ion implantation and activation:

[0080] Aluminum (Al) ions are implanted into an N-type silicon (Si) substrate at high temperature using an implanter;

[0081] The injected Al ions will change the conductivity type of the original N-type Si, causing its local area to become P-type, thus achieving a PN-type conversion;

[0082] Through the high-temperature activation process, it is ensured that the injected ions can be effectively doped into the silicon crystal and become effective carriers;

[0083] The PN type conversion is achieved through a pre-set process recipe:

[0084] Step 1: Dose: 3.8e13cm^-2; Energy: 370keV; Tilt: 0°; Rotation: 0°; Temperature: 500°C. Heating helps reduce implant damage.

[0085] Step 2: Dose: increased to 1.3e14cm^-2, energy: reduced to 250keV, control the implantation depth; tilt and rotation angles: kept unchanged, 0° and 0° respectively; temperature (temp): maintained at 500℃;

[0086] Step 3: Dose: adjusted to 3.6e13cm^-2; Energy: further reduced to 100keV; Tilt and rotation angles: still 0° and 0°; Temperature: 500℃, the same as the previous step;

[0087] S5. Removal of SiO 2 Mask layer:

[0088] This SiO layer is removed by dry etching and BOE wet immersion. 2 Mask;

[0089] S6. Growth of new SiO 2 Mask layer:

[0090] After removing the old SiO 2 After the layer, a new 1 μm thick SiO layer was grown on the N-type Si substrate using vertical low pressure chemical vapor deposition (LPCVD). 2 Mask layer.

[0091] The SiO grown this time 2 The layer is to prepare for the next photonic crystal etching step;

[0092] S7. Photolithography defines the etching area:

[0093] In SiO 2 Photoresist is coated on the mask layer, and then the area to be etched is defined through exposure and development.

[0094] S8. Electron beam etching to form photonic crystals:

[0095] Use inductively coupled plasma (ICP) etching technology and electron beam etching to selectively remove SiO 2 Mask layer, in this process, the SiO2 not protected by the photoresist 2 The area will be etched away, while the Si material will be retained;

[0096] The final result is a Si photonic crystal structure with a specific pattern.

[0097] Electron beam etching (Electron Beam Etching, referred to as EBE) in the present invention is a high-precision technology commonly used in nano-processing and microelectronics manufacturing. The working principle of electron beam etching is mainly to use a high-speed electron beam to process the surface of the target object. The specific process is as follows: Generation and control of the electron beam: First, high-energy electrons are emitted by an electron gun. After these electrons are accelerated by an accelerator, they obtain sufficient energy. Then, the electron flow is precisely focused by an electron mirror system, and finally an electron beam with a smaller diameter is formed. Interaction with the target material: When the high-energy electron beam bombards the surface of the target material, it transfers energy and causes ionization or excitation of the target material, thereby achieving local material removal.

[0098] Piranha solution, also known as piranha solution, is a strong oxidizing agent made from a mixture of concentrated sulfuric acid and hydrogen peroxide.

[0099] Dry etching mainly uses plasma to achieve the etching process. The chemical activity of the gas in the plasma is much stronger than that in normal conditions. Depending on the different materials being etched, the appropriate gas can be selected to react with the etched material more quickly to achieve the purpose of removal. BOE (Buffered Oxide Etch) is a commonly used wet etching solution, mainly composed of hydrofluoric acid (HF) and a buffer (such as NH4F). HF and SiO 2 Reaction to generate soluble hexafluorosilicic acid (H2SiF6) and water, thereby achieving the removal of SiO2.

[0100] Inductively coupled plasma (ICP) etching technology is a high-precision, high-efficiency dry etching technology that is widely used in microelectronics manufacturing, nano-processing and other fields.

[0101] Inductively coupled plasma (ICP) etching technology uses a high-energy ion beam generated by a high-frequency power supply to etch materials. Its basic principle is to use magnetic fields and radio frequency electric fields to generate plasma in a vacuum chamber, and focus the plasma beam on the surface of the material to be etched by inductive coupling, thereby achieving precise etching of the material.

[0102] The present invention can prepare photonic crystals quickly and in large quantities by combining with existing equipment, and can cut photonic crystals of different sizes by laser according to different size requirements. In addition, in the process of preparing electronic devices, the PN type and substrate concentration of the photonic crystals can be freely adjusted according to the requirements to a large extent, which is reliable and convenient.

[0103] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a PN-type SiC photonic crystal, characterized in that: The following steps are involved: S1. Substrate preparation and mask layer growth: Choose N-type Si substrate: Make sure the substrate surface is clean and free of impurities; Vertical LPCVD growth of SiO2 mask layer: Control the growth conditions to ensure that the thickness of the SiO2 layer is 2um and covers the Si substrate; S2. Gluing, exposure and development: Glue coating: evenly coat a layer of photoresist on the SiO2 mask layer to ensure there are no bubbles or impurities; Exposure: Use a photolithography machine to perform exposure and transfer the pattern of the area to be etched to the photoresist; Development: The exposed photoresist is removed by a developer, leaving the pattern of the area to be etched; S3. Electron beam etching (ICP) and subsequent processing; ICP etching: The selective etching characteristics of electron beam etching are used to remove the SiO2 portion not blocked by the photoresist; During the electron beam etching process, the parameters of the etcher are as follows: Pressure: 3mTorr Helium Pressure: 4Torr PN2 (nitrogen flow): 200sccm CHF3 (trifluoromethane flow): 50sccm Duration: 2300s Control etching conditions to ensure etching depth and uniformity; Acid removal of photoresist: Use piranha solution to pickle and remove residual photoresist on the surface; The solution ratio is H2SO4:H2O2=3:1, and the pickling time is 15min to avoid damage to the SiO2 layer; Leave the injection window: A clear injection window pattern is formed on the SiO2 layer after removing the photoresist and etching; Check the integrity and accuracy of the pattern to ensure that it meets the requirements of subsequent processes; S4. High temperature ion implantation and activation: Aluminum (Al) ions are implanted into an N-type silicon (Si) substrate at high temperature using an implanter; The injected Al ions will change the conductivity type of the original N-type Si, causing its local area to become P-type, thus achieving a PN-type conversion; Through the high-temperature activation process, it is ensured that the injected ions can be effectively doped into the silicon crystal and become effective carriers; The PN type conversion is achieved through a pre-set process recipe: Step 1: Dose: 3.8e13 cm^-2; Energy: 370keV; Tilt: 0°; Rotation: 0°; Temperature: 500°C; Heating helps reduce implant damage; Step 2: Dose: increased to 1.3e14 cm^-2, energy: reduced to 250keV, control the implantation depth; tilt and rotation angles: kept unchanged, 0° and 0° respectively; temperature (temp): maintained at 500℃; Step 3: Dose: adjusted to 3.6e13 cm^-2; Energy: further reduced to 100keV; Tilt and rotation angles: still 0° and 0°; Temperature: 500℃, the same as the previous step; S5. Removal of SiO2 mask layer: Remove this SiO2 mask by dry etching and BOE wet soaking; S6. Growth of a new SiO2 mask layer: After removing the old SiO2 layer, a new 1 μm thick SiO2 mask layer is grown on the N-type Si substrate again using vertical low-pressure chemical vapor deposition (LPCVD); The SiO2 layer grown this time is to prepare for the next photonic crystal etching step; S7. Photolithography defines the etching area: Coat the SiO2 mask layer with photoresist, and then define the area to be etched by exposure and development; S8. Electron beam etching to form photonic crystals: Use inductively coupled plasma (ICP) etching technology and electron beam etching to selectively remove the SiO2 mask layer. In this process, the SiO2 area not protected by the photoresist will be etched away, while the Si material will be retained; The final result is a Si photonic crystal structure with a specific pattern.

Citation Information

Patent Citations

  • Method for manufacturing photonic crystal light-emitting diode of waveguiding structures

    CN103904175A

  • Silicon carbide high-voltage MPS diode manufacturing method

    CN105931950A

  • SiC photonic crystal manufacturing method

    CN106547039A

  • Manufacturing method for SiC MOSFET device and SiC MOSFET device

    CN112701151A

  • Method for reducing silicon carbide ion implantation damage

    CN116053117A