Optical chip substrate and preparation method thereof
By using a two-layer oxide layer structure and a carrier capture layer in the optical chip substrate, the time-consuming and thermal stress problems of silicon dioxide layer preparation in the prior art are solved, and efficient preparation and high-quality oxide layers are achieved. Improves the performance and stability of optical chips.
Patent Information
- Application Number
- CN202410942203.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-08
AI Technical Summary
The existing silicon dioxide layer preparation process takes a long time and is prone to introduce thermal stress, resulting in damage to the substrate structure, making it difficult to prepare high-thickness and high-quality oxide layers.
A two-layer oxide layer structure is adopted, wherein the first oxide layer and the second oxide layer are formed by a thermal silicon oxide film, deviate from each other and are prepared simultaneously, the second oxide layer is used to compensate for the thermal stress between the first oxide layer and the substrate layer, and The carrier capture layer is introduced during the preparation process to absorb free carriers and reduce losses.
It improves the preparation efficiency and morphological accuracy of the oxide layer, shortens the preparation period, enhances the stress balance, and improves the structural stability and performance of the optical chip substrate.
Smart Images

Figure CN118915229A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology, and in particular to an optical chip substrate and a preparation method thereof. Background Art
[0002] Heterogeneous integration of multiple materials is an important path to improve chip performance and integration level. By preparing functional materials with piezoelectric, ferroelectric, optoelectronic, pyroelectric, nonlinear and other properties into thin film structures and integrating them with different materials, the advantages of different materials can be fully utilized to improve chip performance. Secondly, by combining functional materials with multiple substrates and preparing them into thin film structures, the interaction between different substrates can be utilized to achieve localization of acoustic wave energy or light wave energy, thereby improving device performance.
[0003] A common heterogeneous substrate structure consists of a functional layer, an oxide layer, and a supporting substrate layer. The oxide layer is typically made of silicon dioxide. In integrated optical devices, silicon dioxide (SiO2) serves as an isolation layer with excellent optical properties: first, low light absorption and scattering losses. Its optical transparency is very good over most of the visible to near-infrared range, meaning that optical signals can be transmitted in SiO2 waveguides with almost no energy loss. Second, it has high electrical insulation, which effectively prevents leakage of electrical signals. This is particularly important for integrated photonics chips, as it ensures the effective separation of electrical and optical signals. Furthermore, silicon dioxide has good thermal stability and high compatibility with silicon-based substrates. High-quality silicon dioxide layers can be produced on silicon-based substrates through thermal oxidation. For silicon-based substrates, since silicon itself has a certain degree of light absorption, the preparation of optical waveguides on silicon-based substrates will result in increased optical signal loss. Therefore, a silicon dioxide layer of a certain thickness is required as an isolation layer to isolate the silicon-based substrate and the waveguide structure, thereby eliminating any impact.
[0004] In the existing silicon dioxide layer preparation process, the oxide layer can be obtained quickly by vapor deposition, but the density of the oxide layer is insufficient, and it is difficult to prepare a high-quality silicon dioxide layer on a supporting substrate. At the same time, it takes a long time to obtain a thick oxide layer on a silicon-based substrate by thermal oxidation. Generally, as the thickness of the oxide layer increases, the preparation rate gradually decreases. At an oxidation temperature of 1100°C, it takes nearly 3 days to prepare a 4.7μm thick silicon dioxide oxide layer, nearly 5 days to prepare a 7μm thick silicon dioxide oxide layer, and nearly 20 days to prepare a 15μm thick silicon dioxide oxide layer. The preparation time required to prepare a thick and high-quality oxide layer on silicon-based and non-silicon substrates is extremely long, and the preparation of a thicker oxide layer by thermal oxidation will also introduce greater thermal stress in the supporting substrate, which may cause the supporting substrate or the oxide layer to crack. Summary of the Invention
[0005] To address the above-mentioned problems in the prior art, the present application provides an optical chip substrate and a preparation method. The specific technical solutions are as follows:
[0006] In one aspect, the present application provides an optical chip substrate, comprising a functional layer, a first oxide layer, a substrate layer, and a second oxide layer, wherein the substrate layer comprises a first surface and a second surface facing away from each other, the first oxide layer being located between the functional layer and the first surface, and the second oxide layer being located on the second surface;
[0007] The first oxide layer includes at least one first oxide film, and the first oxide film is obtained by forming a first silicon film and then thermally oxidizing it;
[0008] The second oxide layer includes at least one second oxide film. In the process of forming the first oxide layer, the second oxide film is obtained by forming a second silicon film and then thermally oxidizing it.
[0009] Furthermore, the first oxide film and the second oxide film are arranged in a one-to-one correspondence, and during the preparation process, the first oxide film and the second oxide film at corresponding positions are formed synchronously.
[0010] Furthermore, the optical chip substrate satisfies at least one of the following characteristics:
[0011] The thickness of at least one of the first oxide layer and the second oxide layer is 2 μm to 50 μm;
[0012] The thickness of the second oxide layer is greater than that of the first oxide layer, and the thickness difference between the second oxide layer and the first oxide layer is 0.01 μm to 5 μm.
[0013] Furthermore, the optical chip substrate further includes at least one carrier-trapping layer, and the carrier-trapping layer satisfies at least one of the following characteristics:
[0014] The carrier trapping layer is located between the substrate layer and the first oxide layer;
[0015] The carrier trapping layer is located between the substrate layer and the second oxide layer;
[0016] The carrier trapping layer is located between two adjacent first oxide films;
[0017] The carrier trapping layer is located between two adjacent second oxide films;
[0018] The single layer thickness of the carrier trapping layer is 0.2 μm to 2 μm.
[0019] Furthermore, the optical chip substrate satisfies at least one of the following characteristics:
[0020] The material of the functional layer includes at least one of single crystal lithium niobate, single crystal lithium tantalate, silicon carbide, silicon, germanium, indium phosphide, barium titanate, strontium titanate and calcium fluoride;
[0021] The material of at least one of the first silicon thin film and the second silicon thin film is at least one of polycrystalline silicon and amorphous silicon;
[0022] The material of at least one of the first oxide film and the second oxide film is silicon oxide;
[0023] The material of the carrier trapping layer is at least one of polycrystalline silicon and amorphous silicon;
[0024] The material of the substrate layer includes at least one of single crystal silicon, polycrystalline silicon, silicon on insulator, sapphire, silicon carbide, silicon carbide on insulator, aluminum nitride and diamond.
[0025] On the other hand, the present application also provides a method for preparing an optical chip substrate, comprising:
[0026] A first oxide layer is formed on a first surface of a substrate layer, and a second oxide layer is formed on a second surface of the substrate layer; the first surface and the second surface are opposite to each other; the first oxide layer includes at least one first oxide film, the first oxide film is obtained by forming a first silicon film and then thermally oxidizing the film; the second oxide layer includes at least one second oxide film, the second oxide film is obtained by forming a second silicon film and then thermally oxidizing the film during the process of forming the first oxide layer;
[0027] The functional layer is bonded to the substrate layer through the first oxide layer to obtain the optical chip substrate.
[0028] Furthermore, a single layer thickness of at least one of the first silicon thin film and the second silicon thin film is less than or equal to a preset single layer thickness, and the preset single layer thickness is 4 μm to 6 μm.
[0029] Furthermore, the first oxide layer includes multiple layers of first oxide films, and the second oxide layer includes multiple layers of second oxide films; and forming the first oxide layer on the first surface of the substrate layer and forming the second oxide layer on the second surface of the substrate layer includes:
[0030] forming the first silicon thin film on the first surface, and forming the second silicon thin film on the second surface;
[0031] thermally oxidizing the first silicon film and the second silicon film so that the first silicon film forms a first oxide film and the second silicon film forms a second oxide film;
[0032] On the substrate layer having a layer of the first oxide film and the second oxide film, the above-mentioned steps of forming the first silicon film and the second silicon film and the thermal oxidation step are repeated to form multiple layers of the first oxide film on the first surface and multiple layers of the second oxide film on the second surface, thereby obtaining the first oxide layer and the second oxide layer.
[0033] Furthermore, the material of the substrate layer is single crystal silicon or polycrystalline silicon, the first oxide layer includes a first initial oxide film and at least one layer of the first oxide film, and the second oxide layer includes a second initial oxide film and at least one layer of the second oxide film; before forming the first oxide layer on the first surface of the substrate layer and forming the second oxide layer on the second surface of the substrate layer, the method further includes:
[0034] The substrate layer is thermally oxidized to form a first initial oxide film and a second initial oxide film on both side surfaces of the substrate layer respectively; the thickness of at least one of the first initial oxide film and the second initial oxide film is less than or equal to a preset thickness, and the preset thickness is 3μm to 5μm.
[0035] Furthermore, the optical chip substrate further comprises at least one carrier trapping layer;
[0036] The carrier-trapping layer is a portion of the first silicon thin film remaining after incomplete thermal oxidation of the first silicon thin film during the thermal oxidation process; and / or
[0037] The carrier trapping layer is a portion of the second silicon film remaining after incomplete thermal oxidation of the second silicon film during the thermal oxidation process.
[0038] Based on the above technical solution, this application has the following beneficial effects:
[0039] 1. The optical chip substrate of the present application includes a functional layer, a first oxide layer, a substrate layer and a second oxide layer. The first oxide layer and the second oxide layer are respectively located on the first surface and the second surface of the substrate layer that are opposite to each other, and the first oxide layer includes at least one first oxide film, and the second oxide layer includes at least one second oxide film. During the preparation process, the first oxide film is obtained by forming a first silicon film and thermally oxidizing it, and the second oxide film is obtained by forming a second silicon film and thermally oxidizing it. While accelerating the overall preparation efficiency of the first oxide layer and the second oxide layer, the second oxide layer can effectively compensate for the thermal stress between the first oxide layer and the substrate layer, greatly improving the stress balance, which is beneficial to improving the preparation yield of each layer structure and the overall optical chip substrate and the final morphology accuracy of the optical chip substrate.
[0040] 2. The first oxide film and the second oxide film of the present application are arranged in a one-to-one correspondence. During the preparation process, the first oxide film and the second oxide film at corresponding positions can be formed synchronously, thereby further improving the preparation efficiency and shortening the preparation cycle.
[0041] 3. The optical chip substrate of the present application also includes at least one carrier-trapping layer, which can absorb free carriers, reduce the loss of the optical chip substrate, and improve the performance of the optical chip substrate and the semiconductor device having the optical chip substrate; and during the preparation process, the carrier-trapping layer is formed by incomplete oxidation of the residual silicon material during the thermal oxidation process, without taking up additional preparation time, thus avoiding the increase in the preparation cycle time. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] To more clearly illustrate the technical solution of this application, the following briefly introduces the drawings required for use in the embodiments or descriptions of the prior art. Obviously, the drawings described below are merely some embodiments of this application, and those skilled in the art can derive other drawings based on these drawings without inventive effort.
[0043] Figure 1 A cross-sectional view of an optical chip substrate provided in an embodiment of the present application;
[0044] Figure 2 A cross-sectional view of another optical chip substrate provided in an embodiment of the present application;
[0045] Figure 3 A cross-sectional view of an optical chip substrate provided for another optional embodiment of the present application;
[0046] Figure 4 A flowchart of a method for preparing an optical chip substrate provided in an embodiment of the present application;
[0047] Figure 5 A flow chart of a method for forming a first oxide layer and a second oxide layer provided in an embodiment of the present application;
[0048] Figure 6 It is a graph of thermal oxidation time and oxidation thickness;
[0049] Figure 7 A flow chart of another method for forming a first oxide layer and a second oxide layer provided in an embodiment of the present application;
[0050] Figure 8 This is a flow chart of a method for forming a first oxide layer and a second oxide layer in an optional embodiment of the present application;
[0051] Figure 9This is a flow chart of a method for forming a first oxide layer and a second oxide layer in another optional embodiment of the present application;
[0052] Figure 10 This is a flow chart of a method for forming the first oxide layer and the second oxide layer in another optional embodiment of the present application;
[0053] Figure 11 A flow chart of another method for preparing an optical chip substrate provided in an embodiment of the present application;
[0054] Figure 12 Schematic diagram of the thickness uniformity of a 15 μm thick oxide layer prepared in a specific embodiment of the present application;
[0055] Figure 13 This is a surface morphology image of the outermost first oxide film in a specific embodiment of the present application;
[0056] Figure 14 This is a surface morphology diagram of the outermost first oxide film after planarization treatment in a specific embodiment of the present application.
[0057] Wherein, the accompanying drawings are marked as follows:
[0058] 1-functional layer, 11-functional wafer, 12-defect layer, 2-first oxide layer, 21-first oxide film, 22-first silicon film, 23-first initial oxide film, 3-substrate layer, 4-second oxide layer, 41-second oxide film, 42-second silicon film, 43-second initial oxide film, 5-carrier trapping layer. DETAILED DESCRIPTION
[0059] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the described embodiments are only part of the embodiments of this application, not all of the embodiments, and the structure in the drawings is only the technical solution of a specific embodiment of this application. The structure of this application may include fewer or more structural features and is not limited to the structure described in the drawings. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0060] It should be noted that in the description of this application, for the following defined terms, these definitions should be applied unless a different definition is given in the claims or elsewhere in this specification. All numerical values, whether or not explicitly indicated, are defined herein as being modified by the term "about". The term "about" generally refers to a numerical range that a person of ordinary skill in the art would consider to be equivalent to the stated value to produce substantially the same properties, functions, results, etc. A numerical range indicated by a low value and a high value is defined to include all numerical values included in the numerical range and all subranges included in the numerical range.
[0061] It should be noted that, in the description of this application, the terms "first," "second," etc. are used to distinguish similar objects and are not necessarily used to describe a specific order or precedence. It should be understood that the terms used in this manner are interchangeable where appropriate, so that the embodiments of the application described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including," "having," and any variations thereof are intended to cover non-exclusive inclusions.
[0062] It should be noted that, in the description of this application, the meaning of the terms "on...", "above...", "above...", and "above..." should be interpreted in the broadest sense, meaning that the description containing these terms is interpreted as "the component can be set on another component in a direct contact manner, or there can be an intermediate component or layer between the components". In addition, for the convenience of description, this application may also use spatially relative terms such as "under...", "under...", "under...", "on...", "above...", "above...", "lower", "upper", etc. to describe the relationship between one element or component and another element or component shown in the drawings. In addition to the orientations described in the figures, the spatially relative terms are also intended to cover different orientations of the device in use or operation. The device can be oriented in other ways (rotated 90° or in other orientations), and the spatially relative descriptors used in this application can be interpreted accordingly.
[0063] The term "layer" as used in this application refers to a portion of a material that includes an area with a certain thickness. A layer may extend over the entire underlying or superstructure, or may extend over a localized area of the underlying or superstructure. In addition, a layer may be an area of a homogeneous or inhomogeneous continuous structure whose thickness is less than the thickness of the continuous structure. For example, a layer may be located between the top and bottom surfaces of a continuous structure or between any pair of horizontal planes therebetween. A layer may extend horizontally, vertically and / or along a tapered surface. A layer may include multiple layers. For example, a redistribution layer may include one or more doped or undoped semiconductor layers and may have the same or different materials.
[0064] It should be understood that the "surface" used in this application, such as "first surface", "second surface", etc., refers to the XY plane of the substrate layer or piezoelectric functional layer, etc., corresponding to the XY plane of the optical chip substrate, and the "thickness direction" refers to the Z direction perpendicular to the XY plane. The "thickness" or "height" involved in this application refers to the Z-direction thickness or Z-direction height.
[0065] In view of the problem that the preparation of silicon dioxide oxide layer in the prior art is time-consuming and easy to introduce large thermal stress and damage the substrate structure during the preparation process, the embodiment of the present application provides an optical chip substrate and a preparation method, such as Figure 1 As shown, the optical chip substrate includes a functional layer 1, a first oxide layer 2, a substrate layer 3 and a second oxide layer 4, the substrate layer 3 includes a first surface and a second surface that are opposite to each other, the first oxide layer 2 is located between the functional layer 1 and the first surface, and the second oxide layer 4 is located on the second surface, that is, the first oxide layer 2 and the second oxide layer 4 are opposite to each other; during the preparation process, the second oxide layer 4 is used to compensate for the thermal stress between the first oxide layer 2 and the substrate layer 3, and maintain the overall morphology and structural stability of the substrate layer 3 and the optical chip substrate, thereby improving the preparation efficiency of the high-thickness oxide layer in the optical chip substrate, reducing the difficulty of the preparation process of the high-thickness oxide layer in the optical chip substrate, and improving the preparation yield of the optical chip substrate, and improving the morphology accuracy and structural stability of the optical chip substrate.
[0066] Among them, the first oxide layer 2 includes at least one first oxide film 21, and the first oxide film 21 is obtained by forming a first silicon film 22 and thermally oxidizing it; the second oxide layer 4 includes at least one second oxide film 41. In the process of forming the first oxide layer 2, the second oxide film 41 is obtained by forming a second silicon film 42 and thermally oxidizing it; in this way, the thickness of the first oxide layer 2 is the sum of the thicknesses of the at least one first oxide film 21, and the thickness of the second oxide layer 4 is the sum of the thicknesses of the at least one second oxide film 41. During the preparation process, the first oxide layer 2 is split into at least one relatively thin first oxide film 21 for layer-by-layer preparation, and the second oxide layer 4 is split into at least one relatively thin second oxide film 41 for layer-by-layer preparation. Compared with forming a thicker oxide layer at one time, the preparation time of the first oxide layer 2 and the second oxide layer 4 can be greatly shortened, thereby shortening the overall preparation cycle of the optical chip substrate.
[0067] Specifically, in some exemplary embodiments, the first oxide film 21 and the second oxide film 41 are arranged in a one-to-one correspondence. During the preparation process, the first oxide film 21 and the second oxide film 41 at corresponding positions are formed synchronously, which can further shorten the preparation cycle of the optical chip substrate and improve the preparation efficiency of the optical chip substrate.
[0068] Specifically, the thickness of at least one of the first oxide layer 2 and the second oxide layer 4 is 2 μm to 50 μm; in some exemplary embodiments, the thickness of the first oxide layer 2 is 2 μm to 50 μm; in other exemplary embodiments, the thickness of the second oxide layer 4 is 2 μm to 50 μm; in other exemplary embodiments, the thickness of the first oxide layer 2 and the second oxide layer 4 are both 2 μm to 50 μm; it can be understood that the thickness of at least one of the first oxide layer 2 and the second oxide layer 4 can be any point value between 2 μm and 50 μm; exemplarily, the first oxide layer 2 and The thickness of at least one of the second oxide layers 4 can be 2μm, 5μm, 10μm, 15μm, 20μm, 25μm, 30μm, 40μm, 50μm, etc.; in this way, the thickness of the first oxide layer 2 is relatively thick, and as an isolation layer, it can provide good optical performance, effectively reduce the light absorption and scattering loss of the optical chip substrate, have good optical transparency, and can improve electrical insulation, effectively separate optical signals and electrical signals, prevent leakage of electrical signals, and provide good thermal stability and good compatibility with the substrate layer 3, thereby improving the overall performance of the optical chip substrate.
[0069] Specifically, the thickness of the second oxide layer 4 is greater than that of the first oxide layer 2, which can play a role in stress balance to a certain extent, inhibit the morphological changes of the first oxide layer 2, the substrate layer 3 and the entire optical chip substrate, and is conducive to maintaining the overall morphology of the optical chip substrate close to the desired morphology, improving the morphological accuracy of the optical chip substrate, and can help resist the thermal stress between the first oxide layer 2 and the substrate layer 3 during the preparation process. Furthermore, in the preparation process of the optical chip substrate, after the first oxide layer 2 and the second oxide layer 4 are formed, a functional layer 1 with a larger thermal expansion coefficient will be introduced later. Then, the thickness of the second oxide layer 4 is greater than that of the first oxide layer 2, and can also balance the thermal stress between the first oxide layer 2 and the functional layer 1, achieve stress balance, improve the stability of the substrate layer 3, the first oxide layer 2 and the second oxide layer 4, and synergistically improve the morphological accuracy and structural stability of the optical chip substrate, and reduce abnormal deformation.
[0070] Specifically, in some exemplary embodiments, the thickness difference between the second oxide layer 4 and the first oxide layer 2 is 0.01 μm to 5 μm; it can be understood that the thickness difference between the second oxide layer 4 and the first oxide layer 2 can be any point value between 0.01 μm and 5 μm; exemplarily, the thickness difference between the second oxide layer 4 and the first oxide layer 2 can be 0.01 μm, 0.05 μm, 0.1 μm, 0.5 μm, 1 μm, 2 μm, 5 μm, etc.; in this way, the second oxide layer 4 can effectively balance the thermal stress between the first oxide layer 2 and the substrate layer 3 and the thermal stress between the first oxide layer 2 and the functional layer 1, and has good stress balance, which greatly improves the overall morphological accuracy and structural stability of the substrate layer 3, the first oxide layer 2, the second oxide layer 4 and the optical chip substrate.
[0071] Specifically, in some exemplary embodiments, the material of the functional layer 1 includes at least one of single-crystal lithium niobate, single-crystal lithium tantalate, silicon carbide, silicon, germanium, indium phosphide, barium titanate, strontium titanate, and calcium fluoride.
[0072] Specifically, in some exemplary embodiments, the material of at least one of the first silicon thin film 22 and the second silicon thin film 42 is at least one of polysilicon and amorphous silicon.
[0073] Specifically, in some exemplary embodiments, the material of at least one of the first oxide film 21 and the second oxide film 41 is silicon oxide.
[0074] Specifically, in some exemplary embodiments, the material of the substrate layer 3 includes at least one of single crystal silicon, polycrystalline silicon, silicon on insulator, sapphire, silicon carbide, silicon carbide on insulator, aluminum nitride, and diamond.
[0075] Specifically, if Figure 2 and Figure 3 As shown, the optical chip substrate also includes at least one carrier-trapping layer 5, which can be located at least one of between the substrate layer 3 and the first oxide layer 2, between the substrate layer 3 and the second oxide layer 4, between two adjacent first oxide films 21, and between two adjacent second oxide films 41. That is, the carrier-trapping layer 5 can be located between any two layers of structure inside the optical chip substrate except between the first oxide layer 2 and the functional layer 1, and is used to absorb free carriers and reduce the loss of the optical chip substrate.
[0076] Specifically, when the optical chip substrate includes a carrier-trapping layer 5, in some exemplary embodiments, the carrier-trapping layer 5 is located between the substrate layer 3 and the first oxide layer 2; in other exemplary embodiments, the carrier-trapping layer 5 is located between the substrate layer 3 and the second oxide layer 4; in other exemplary embodiments, the carrier-trapping layer 5 is located between two adjacent first oxide films 21; optionally, the carrier-trapping layer 5 is located between two adjacent second oxide films 41.
[0077] Specifically, when the optical chip substrate includes at least two carrier-trapping layers 5, each carrier-trapping layer 5 can be located at one of the four interlayer positions mentioned above, and the positions of at least two carrier-trapping layers 5 can be a combination of at least one of the four interlayer positions mentioned above. The present invention does not make specific limitations to meet the different requirements for device performance in a variety of different application scenarios.
[0078] For example, Figure 2 As shown, the first oxide layer 2 and the second oxide layer 4 are multi-layer structures symmetrical about the supporting substrate. Taking the carrier-trapping layer 5 in the region of the first oxide layer 2 as an example, the optical chip substrate includes M layers of first oxide films 21 and M layers of carrier-trapping layers 5 (M≥2), each layer of carrier-trapping layer 5 is located on the side of the first oxide film 21 away from the functional layer 1, that is, one layer of carrier-trapping layer 5 is located between the first oxide film 21 and the substrate layer 3, and the other (M-1) layers of carrier-trapping layers 5 are respectively located between two adjacent first oxide films 21 in the M layers of first oxide films 21; illustratively, as Figure 3 As shown, the optical chip substrate includes N layers of first oxide film 21 and two carrier-trapping layers 5 (N≥2), wherein one carrier-trapping layer 5 is located between the first oxide layer 2 (i.e., the first oxide film 21 closest to the substrate layer 3) and the substrate layer 3, and the other carrier-trapping layer 5 is located between the second oxide layer 4 (i.e., the second oxide film 41 closest to the substrate layer 3) and the substrate layer 3.
[0079] Specifically, in some exemplary embodiments, the material of the carrier-trapping layer 5 is at least one of polycrystalline silicon and amorphous silicon.
[0080] Specifically, the single-layer thickness of the carrier-trapping layer 5 is 0.2 μm to 2 μm, that is, the thickness of each carrier-trapping layer 5 is 0.2 μm to 2 μm; it can be understood that the single-layer thickness of the carrier-trapping layer 5 can be any point value between 0.2 μm and 2 μm; illustratively, the single-layer thickness of the carrier-trapping layer 5 can be 0.2 μm, 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 2 μm, etc.; in this way, free carriers can be effectively absorbed, losses can be reduced, and the performance of the optical chip substrate can be improved.
[0081] On the other hand, Figure 4 As shown, the embodiment of the present application also provides a method for preparing an optical chip substrate, comprising:
[0082] S1, forming a first oxide layer on a first surface of a substrate layer, and forming a second oxide layer on a second surface of the substrate layer; the first surface and the second surface are opposite to each other; the first oxide layer includes at least one first oxide film, and the first oxide film is obtained by forming a first silicon film and thermally oxidizing it; the second oxide layer includes at least one second oxide film, and in the process of forming the first oxide layer, the second oxide film is obtained by forming a second silicon film and thermally oxidizing it.
[0083] S2, bonding the functional layer to the substrate layer through the first oxide layer to obtain the optical chip substrate.
[0084] In step S1, the first oxide layer 2 and the second oxide layer 4 can be collectively referred to as oxide layers, the first silicon film 22 and the second silicon film 42 can be collectively referred to as silicon films, and the first oxide film 21 and the second oxide film 41 can be collectively referred to as oxide films; this step divides the thicker oxide layer into multiple thin layers for thermal oxidation, and the preparation rate of a single thin layer is always at a faster speed, which can greatly improve the overall preparation efficiency of the oxide layer.
[0085] Among them, the method of forming the silicon thin film includes at least one of chemical vapor deposition (CVD) and physical vapor deposition (PVD); when the material of the silicon thin film is amorphous silicon, the temperature for forming the silicon thin film is 200°C to 600°C; when the material of the silicon thin film is polycrystalline silicon, the temperature for forming the silicon thin film is 600°C to 1000°C; in this way, the preparation efficiency of the silicon thin film is high and the preparation accuracy is good, which can effectively improve the structural accuracy and structural stability of the prepared silicon thin film, and is conducive to the subsequent steps such as thermal oxidation.
[0086] In some exemplary embodiments, the thermal oxidation of the silicon film can be complete oxidation or incomplete oxidation, and the thermal oxidation includes at least one of wet oxidation, chlorine-doped oxidation and water vapor oxidation, and the temperature of the thermal oxidation is 800°C to 1200°C; it can be understood that the temperature of the thermal oxidation can be any point value between 800°C and 1200°C; exemplarily, the temperature of the thermal oxidation can be 800°C, 850°C, 900°C, 950°C, 1000°C, 1100°C, 1200°C, etc.; in this way, different thermal oxidation requirements can be met, and oxide layers and optical chip substrates of various structures can be prepared to improve the performance of devices in different scenarios, with good applicability.
[0087] Specifically, in some exemplary embodiments, the first oxide layer 2 includes multiple layers of first oxide films 21, and the second oxide layer 4 includes multiple layers of second oxide films 41; Figure 5 As shown, the first oxide layer is formed on the first surface of the substrate layer, and the second oxide layer is formed on the second surface of the substrate layer, that is, step S1 includes:
[0088] forming the first silicon thin film on the first surface, and forming the second silicon thin film on the second surface;
[0089] thermally oxidizing the first silicon film and the second silicon film so that the first silicon film forms a first oxide film and the second silicon film forms a second oxide film;
[0090] On the substrate layer having a layer of the first oxide film and the second oxide film, the above-mentioned steps of forming the first silicon film and the second silicon film and the thermal oxidation step are repeated to form multiple layers of the first oxide film on the first surface and multiple layers of the second oxide film on the second surface, thereby obtaining the first oxide layer and the second oxide layer.
[0091] like Figure 6 As shown in the figure, with the increase of thermal oxidation time, the growth rate of the oxide thickness gradually decreases. By dividing the oxide layer into multiple thin layers and depositing silicon thin films multiple times and thermally oxidizing them, the oxidation rate can always be kept at a relatively fast stage. Compared with the traditional method of directly preparing a thicker oxide layer, the overall preparation efficiency of the first oxide layer 2 and the second oxide layer 4 is greatly improved, which is conducive to shortening the overall preparation cycle of the optical chip substrate.
[0092] Specifically, in step S1, the single-layer thickness of at least one of the first silicon film 22 and the second silicon film 42 is less than or equal to the preset single-layer thickness; in some exemplary embodiments, the single-layer thickness of the first silicon film 22 is less than or equal to the preset single-layer thickness; in other exemplary embodiments, the single-layer thickness of the second silicon film 42 is less than or equal to the preset single-layer thickness; in other exemplary embodiments, the single-layer thickness of the first silicon film 22 and the single-layer thickness of the second silicon film 42 are both less than or equal to the preset single-layer thickness.
[0093] The preset single-layer thickness is 4μm to 6μm; it can be understood that the preset single-layer thickness can be any point value between 4μm and 6μm; illustratively, the preset single-layer thickness can be 4μm, 4.2μm, 4.5μm, 5μm, 5.3μm, 5.5μm, 5.8μm, 6μm, etc.; in this way, the single-layer thickness of the silicon film is thinner, and the preparation rate of the single-layer silicon film is faster, which can maintain a high preparation rate during the preparation process of the entire oxide layer, and is less likely to have a situation where the oxidation rate gradually decreases due to the preparation thickness being too thick, thereby improving the overall preparation efficiency of the oxide layer and the optical chip substrate and shortening the preparation cycle; in some preferred embodiments, the preset single-layer thickness can be 5μm, that is, the single-layer thickness of at least one of the first silicon film 22 and the second silicon film 42 is less than or equal to 5μm.
[0094] Specifically, in some exemplary embodiments, the material of the substrate layer 3 is single crystal silicon or polycrystalline silicon, the first oxide layer 2 includes a first initial oxide film 23 and at least one layer of first oxide film 21, and the second oxide layer 4 includes a second initial oxide film 43 and at least one layer of second oxide film 41, that is, the first initial oxide film 23 and the second initial oxide film 43 are both located on the surface of the substrate layer 3, and are obtained by thermal oxidation of the material on the surface of the substrate layer 3.
[0095] like Figure 7 As shown, before forming the first oxide layer on the first surface of the substrate layer and forming the second oxide layer on the second surface of the substrate layer, that is, before step S1, the method further includes:
[0096] The substrate layer is thermally oxidized to form a first initial oxidation film and a second initial oxidation film on both side surfaces of the substrate layer.
[0097] Among them, the thickness of at least one of the first initial oxidation film 23 and the second initial oxidation film 43 is less than or equal to the preset thickness, and the first initial oxidation film 23 and the second initial oxidation film 43 can be collectively referred to as initial oxidation films; in some exemplary embodiments, the thickness of the first initial oxidation film 23 is less than or equal to the preset thickness; in other exemplary embodiments, the thickness of the second initial oxidation film 43 is less than or equal to the preset thickness; in other exemplary embodiments, the thickness of the first initial oxidation film 23 and the thickness of the second initial oxidation film 43 are both less than or equal to the preset thickness.
[0098] The preset thickness is 3μm to 5μm; it can be understood that the preset thickness can be any point value between 3μm and 5μm; illustratively, the preset thickness can be 3μm, 3.5μm, 3.8μm, 4μm, 4.2μm, 4.5μm, 5μm, etc.; in this way, the thickness of the initial oxide film is thin and the preparation rate is fast.
[0099] Afterwards, a silicon film is formed on the substrate layer 3 having the initial oxide film and is completely oxidized into an oxide film, thereby obtaining a first oxide layer 2 including a first initial oxide film 23 and at least one layer of a first oxide film 21, and a second oxide layer 4 including a second initial oxide film 43 and at least one layer of a second oxide film 41.
[0100] Specifically, in some exemplary embodiments, the optical chip substrate further includes at least one carrier-trapping layer 5; in some exemplary embodiments, the carrier-trapping layer 5 is a portion of the first silicon film 22 remaining after incomplete thermal oxidation of the first silicon film 22 during the thermal oxidation process, that is, the carrier-trapping layer 5 located on the first surface side of the substrate layer 3 is a part of the first oxide layer 2 that is finally formed, and the thickness of the first oxide layer 2 is the sum of the thickness of at least one first oxide film 21 and at least one carrier layer.
[0101] In some exemplary embodiments, the carrier-trapping layer 5 is a portion of the second silicon film 42 that remains after incomplete thermal oxidation of the second silicon film 42 during the thermal oxidation process, that is, the carrier-trapping layer 5 located on the second surface side of the substrate layer 3 is a part of the second oxide layer 4 that is finally formed, and the thickness of the second oxide layer 4 is the sum of the thickness of at least one layer of the second oxide film 41 and at least one layer of carriers.
[0102] In other exemplary embodiments, in the multilayer carrier-trapping layer 5, at least one layer of the carrier-trapping layer 5 is a portion of the first silicon film 22 that remains after incomplete thermal oxidation of the first silicon film 22 during the thermal oxidation process, and there is also at least one layer of the carrier-trapping layer 5 that is a portion of the second silicon film 42 that remains after incomplete thermal oxidation of the second silicon film 42 during the thermal oxidation process.
[0103] like Figure 8 As shown, in some exemplary embodiments, after the first initial oxide layer and the second initial oxide layer are formed, the first silicon film 22 and the second silicon film 42 formed subsequently undergo incomplete thermal oxidation, and the remaining portions of the first silicon film 22 and the second silicon film 42 serve as carrier-trapping layers 5, respectively. One layer of the carrier-trapping layer 5 is located between the first initial oxide layer and the first oxide film 21, and the other layer of the carrier-trapping layer 5 is located between the second initial oxide layer and the second oxide film 41. After the steps of forming the silicon film and thermally oxidizing are subsequently repeated, the silicon film remaining from the incomplete thermal oxidation also serves as a carrier-trapping layer 5, and the carrier-trapping layer 5 is located between two adjacent first oxide films 21 or between two adjacent second oxide films 41.
[0104] like Figure 9As shown, in some exemplary embodiments, in the process of forming a multilayer silicon film on both side surfaces of the substrate layer 3 and forming a multilayer oxide film after thermal oxidation, incomplete oxidation can occur during the first thermal oxidation of the silicon film on the substrate layer 3 to form a carrier-trapping layer 5, and the subsequent thermal oxidation processes are all complete oxidation. Then, the optical chip substrate includes two carrier-trapping layers 5, one carrier-trapping layer 5 is located between the first oxide film 21 and the substrate layer 3, and the other carrier-trapping layer 5 is located between the second oxide film 41 and the substrate layer 3.
[0105] like Figure 10 As shown, in some exemplary embodiments, in the process of forming multiple layers of silicon thin films on both side surfaces of the substrate layer 3 and forming multiple layers of oxide films after thermal oxidation, incomplete oxidation can occur during each thermal oxidation process of the silicon thin film to form a carrier-trapping layer 5. Then, the optical chip substrate includes multiple layers of carrier-trapping layers 5. On the first surface side of the substrate layer 3, one layer of the carrier-trapping layer 5 is located between the substrate layer 3 and the first oxide film 21, and the remaining carrier-trapping layers 5 on this side are located between the two adjacent first oxide films 21; on the first surface side of the substrate layer 3, one layer of the carrier-trapping layer 5 is located between the substrate layer 3 and the second oxide film 41, and the remaining carrier-trapping layers 5 on this side are located between the two adjacent second oxide films 41.
[0106] Specifically, in some exemplary embodiments, before bonding the functional layer to the substrate layer through the first oxide layer to obtain the optical chip substrate, that is, before step S2, the method further includes:
[0107] A planarization process is performed on at least one of a surface of the first oxide film away from the substrate layer and a surface of the second oxide film away from the substrate layer, wherein a thickness removed by the planarization process is 0.01 μm to 5 μm.
[0108] That is, in the process of forming a silicon film and thermally oxidizing it at least once, after the last formation of the first oxide film 21 and the last formation of the second oxide film 41, the surface of the outermost oxide film away from the substrate layer 3 is planarized; for polycrystalline / amorphous materials, the thermal oxidation process of converting the silicon film into an oxide film will cause the surface roughness of the oxide film to increase. After multiple film formations are superimposed, the outermost surface roughness of the oxide layer away from the substrate layer 3 is larger. The planarization treatment can greatly reduce the surface roughness of the outermost oxide layer, improve the surface quality of the first oxide layer 2 and the second oxide layer 4, and is also beneficial to the subsequent bonding steps and the surface quality of the final optical chip substrate.
[0109] It can be understood that the removal thickness of the planarization treatment can be any point value between 0.01μm and 5μm; for example, the removal thickness of the planarization treatment can be 0.01μm, 0.1μm, 0.5μm, 1μm, 2μm, 5μm, etc.; in this way, the surface roughness of the first oxide layer 2 and the second oxide layer 4 can be effectively reduced, and the surface quality can be improved, which is beneficial to improving the bonding accuracy and bonding reliability of the subsequent bonding steps, and improving the surface quality, structural accuracy and structural stability of the optical chip substrate after bonding, which is beneficial to improving the device performance of the semiconductor device having the optical chip substrate.
[0110] Specifically, in some exemplary embodiments, before performing the planarization process, the method further includes:
[0111] Chamfering is performed on at least one of the surface of the first oxide film away from the substrate layer and the surface of the second oxide film away from the substrate layer so that a T-shaped chamfer is formed on at least one of the surface of the first oxide film away from the substrate layer and the surface of the second oxide film away from the substrate layer, wherein the depth of the T-shaped chamfer is 2 μm to 50 μm, and the width of the T-shaped chamfer is 0.5 mm to 3 mm.
[0112] That is, after the silicon film is formed and thermally oxidized at least once, the surface of the outermost oxide film in the formed oxide layer away from the substrate layer 3 is chamfered. The chamfering treatment is used to remove edge defects, improve the uniformity of polishing, and further improve the surface quality of the first oxide layer 2 and the second oxide layer 4, which is beneficial to improving the reliability of the subsequent bonding step and the surface quality of the final optical chip substrate.
[0113] In some exemplary embodiments, the outermost surface of the first oxide film 21 away from the substrate layer 3 has a T-shaped chamfer; in other exemplary embodiments, the outermost surface of the second oxide film 41 away from the substrate layer 3 has a T-shaped chamfer; in other exemplary embodiments, the outermost surface of the first oxide film 21 away from the substrate layer 3 and the outermost surface of the second oxide film 41 away from the substrate layer 3 both have a T-shaped chamfer.
[0114] It can be understood that the depth of the T-chamfer can be any value between 2μm and 50μm, and the width of the T-chamfer can be any value between 0.5mm and 3mm; for example, the depth of the T-chamfer can be 2μm, 5μm, 10μm, 15μm, 20μm, 25μm, 50μm, etc., and the width of the T-chamfer can be 0.5mm, 1mm, 1.5mm, 2mm, 2.5mm, 3mm, etc.; in this way, the polishing uniformity of the surface of the first oxide layer 2 and the surface of the second oxide layer 4 is good and the surface quality is high.
[0115] Then, in step S2, as Figure 4 As shown, in some exemplary embodiments, the functional layer 1 can be obtained by annealing and planarizing the functional wafer 11 after bonding.
[0116] like Figure 11 As shown, in other exemplary embodiments, the functional layer 1 can also be prepared by ion implantation into the functional wafer 11, and fine annealing and flattening after bonding; exemplarily, ion implantation is performed on the functional wafer 11 to form a defect layer 12 in the functional wafer 11, and after the substrate layer 3 and the functional layer 1 are bonded to form a bonding structure through the first oxide layer 2, the bonding structure is annealed to remove the defect layer 12, and the functional wafer 11 is separated to form the functional layer 1, thereby obtaining an optical chip substrate having the functional layer 1; wherein, during the ion implantation process, the thickness of the defect layer 12 formed in the functional wafer 11 and the depth of the defect layer 12 can be controlled by controlling the implantation energy and implantation dose of the implanted ions, thereby preliminarily controlling the thickness range of the formed functional layer 1, so as to control the thickness of the functional layer 1 formed after subsequent bonding and removal of the defect layer 12, with high accuracy and good reliability.
[0117] Specifically, after bonding the functional layer to the substrate layer through the first oxide layer and before obtaining the optical chip substrate, the method further includes:
[0118] The bonding structure formed by bonding the functional layer to the substrate layer through the first oxide layer is annealed.
[0119] During the annealing process, the temperature is 50°C to 250°C, and the annealing atmosphere is at least one of nitrogen, argon and vacuum environment, so as to effectively peel off the functional wafer 11 and transfer the functional layer 1 to the substrate layer 3, thereby improving the preparation yield and performance stability of the functional layer 1; afterward, the annealed bonding structure is ground and flattened to thin the functional wafer 11 to obtain the optical chip substrate.
[0120] Specifically, in other optional embodiments, after bonding and before obtaining the optical chip substrate; further, after the annealing step and before grinding and planarization, the functional layer 1 in the bonding structure can also be post-annealed, and after post-annealing, grinding and planarization, the optical chip substrate is obtained; wherein, during the post-annealing process, the post-annealing temperature is 200°C to 1200°C, and the post-annealing atmosphere is at least one of nitrogen, oxygen, argon and vacuum environment; in this way, through post-annealing, grinding and planarization, the surface roughness of the functional layer 1 is reduced, and surface scratches and damage are reduced, which is beneficial to improving the surface morphology and structural accuracy of the prepared optical chip substrate, and improving the performance of the optical chip substrate.
[0121] The present application also provides a semiconductor device comprising the optical chip substrate as described above, or comprising an optical chip substrate manufactured by the method for manufacturing the optical chip substrate as described above, and the device has good performance.
[0122] Specifically, in some exemplary embodiments, the semiconductor device includes at least one of an optical device and an electro-optical device.
[0123] like Figure 12-13 FIG. 1 is a schematic diagram of an oxide layer with a thickness of 15 μm prepared by the above-mentioned method for preparing an optical chip substrate in a specific embodiment of the present application and a surface morphology diagram thereof during the preparation process; FIG. Figure 12 As shown, it can be seen that the thickness of the oxide layer provided in the embodiment of the present application is relatively uniform, indicating that the thermal stress during the preparation process is relatively balanced, so that the morphology of the overall oxide layer is close to the desired morphology, the morphology accuracy is high, and the structural stability is good; Figure 13 As shown in FIG, after thermal oxidation but before planarization, the surface of the oxide layer is relatively rough, wherein Ra (arithmetic mean of the absolute value of the roughness profile ordinate) is 0.274 nm, and Rq (root mean square average of the roughness profile ordinate) is 0.345 nm; Figure 14 As shown in the figure, after the planarization treatment, the Ra of the nutrient layer surface is 0.150nm and the Rq is 0.189nm. It can be seen that the oxide layer formed after the planarization treatment has a lower surface roughness, which is beneficial to improving the morphology accuracy, surface quality and structural stability of the oxide layer and the optical chip substrate.
[0124] It should be noted that the various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same and similar parts between the various embodiments can be referenced to each other.
[0125] The above description has fully disclosed the specific embodiments of this application. It should be noted that any changes made by those skilled in the art to the specific embodiments of this application do not depart from the scope of the claims of this application. Accordingly, the scope of the claims of this application is not limited to the above specific embodiments.
Claims
1. An optical chip substrate, characterized in that: It comprises a functional layer, a first oxide layer, a substrate layer and a second oxide layer, wherein the substrate layer comprises a first surface and a second surface which are opposite to each other, the first oxide layer is located between the functional layer and the first surface, and the second oxide layer is located on the second surface; The first oxide layer includes at least one first oxide film, and the first oxide film is obtained by forming a first silicon film and thermally oxidizing it; The second oxide layer includes at least one second oxide film. In the process of forming the first oxide layer, the second oxide film is obtained by forming a second silicon film and then thermally oxidizing it.
2. The optical chip substrate according to claim 1, characterized in that: The first oxide film and the second oxide film are arranged in one-to-one correspondence. During the preparation process, the first oxide film and the second oxide film at corresponding positions are formed synchronously.
3. The optical chip substrate according to claim 1, characterized in that: The optical chip substrate satisfies at least one of the following characteristics: The thickness of at least one of the first oxide layer and the second oxide layer is 2 μm to 50 μm; The thickness of the second oxide layer is greater than that of the first oxide layer, and the thickness difference between the second oxide layer and the first oxide layer is 0.01 μm to 5 μm.
4. The optical chip substrate according to claim 1, characterized in that: The optical chip substrate further comprises at least one carrier trapping layer, and the carrier trapping layer satisfies at least one of the following characteristics: The carrier trapping layer is located between the substrate layer and the first oxide layer; The carrier trapping layer is located between the substrate layer and the second oxide layer; The carrier trapping layer is located between two adjacent first oxide films; The carrier trapping layer is located between two adjacent second oxide films; The single layer thickness of the carrier trapping layer is 0.2 μm to 2 μm.
5. The optical chip substrate according to any one of claims 1 to 4, characterized in that: The optical chip substrate satisfies at least one of the following characteristics: The material of the functional layer includes at least one of single crystal lithium niobate, single crystal lithium tantalate, silicon carbide, silicon, germanium, indium phosphide, barium titanate, strontium titanate and calcium fluoride; The material of at least one of the first silicon thin film and the second silicon thin film is at least one of polycrystalline silicon and amorphous silicon; The material of at least one of the first oxide film and the second oxide film is silicon oxide; The material of the carrier trapping layer is at least one of polycrystalline silicon and amorphous silicon; The material of the substrate layer includes at least one of single crystal silicon, polycrystalline silicon, silicon on insulator, sapphire, silicon carbide, silicon carbide on insulator, aluminum nitride and diamond.
6. A method for preparing an optical chip substrate, characterized in that: include: A first oxide layer is formed on a first surface of a substrate layer, and a second oxide layer is formed on a second surface of the substrate layer; the first surface and the second surface are opposite to each other; the first oxide layer includes at least one first oxide film, which is obtained by forming a first silicon film and then thermally oxidizing it; the second oxide layer includes at least one second oxide film, which is obtained by forming a second silicon film and then thermally oxidizing it during the process of forming the first oxide layer; The functional layer is bonded to the substrate layer through the first oxide layer to obtain the optical chip substrate.
7. The optical chip substrate according to claim 6, characterized in that: A single layer thickness of at least one of the first silicon thin film and the second silicon thin film is less than or equal to a preset single layer thickness, and the preset single layer thickness is 4 μm to 6 μm.
8. The method for preparing an optical chip according to claim 6, characterized in that: The first oxide layer includes multiple layers of first oxide films, and the second oxide layer includes multiple layers of second oxide films; the forming of the first oxide layer on the first surface of the substrate layer and the forming of the second oxide layer on the second surface of the substrate layer includes: forming the first silicon thin film on the first surface, and forming the second silicon thin film on the second surface; thermally oxidizing the first silicon film and the second silicon film so that the first silicon film forms a first oxide film and the second silicon film forms a second oxide film; On the substrate layer having a layer of the first oxide film and the second oxide film, the steps of forming the first silicon film and the second silicon film and the thermal oxidation step are repeated so that multiple layers of the first oxide film are formed on the first surface and multiple layers of the second oxide film are formed on the second surface, thereby obtaining the first oxide layer and the second oxide layer.
9. The method for preparing an optical chip substrate according to claim 6, characterized in that: The material of the substrate layer is single crystal silicon or polycrystalline silicon, the first oxide layer includes a first initial oxide film and at least one layer of the first oxide film, and the second oxide layer includes a second initial oxide film and at least one layer of the second oxide film; Before forming the first oxide layer on the first surface of the substrate layer and forming the second oxide layer on the second surface of the substrate layer, the method further includes: The substrate layer is thermally oxidized to form a first initial oxide film and a second initial oxide film on both side surfaces of the substrate layer respectively; the thickness of at least one of the first initial oxide film and the second initial oxide film is less than or equal to a preset thickness, and the preset thickness is 3μm to 5μm.
10. The method for preparing an optical chip substrate according to claim 6, characterized in that: The optical chip substrate further comprises at least one carrier trapping layer; The carrier trapping layer is a portion of the first silicon film remaining after incomplete thermal oxidation of the first silicon film during thermal oxidation; and / or The carrier trapping layer is a portion of the second silicon film remaining after incomplete thermal oxidation of the second silicon film during the thermal oxidation process.