Insulated optical unit, preparation method thereof and application of insulated optical unit in optical fiber composite overhead ground wire

By using plastic polymer substrates and fiber reinforced materials in the insulating light units, the problem of decreasing the intensity of the insulating light units during the melting process is solved, and stable performance and long life are achieved at high temperatures.

CN118915251APending Publication Date: 2024-11-08STATE GRID HEBEI ELECTRIC POWER CO LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411058731.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing insulating light units are affected by high temperature during the melting process, resulting in a decrease in intensity, and the surface is prone to deformation, resulting in a shorter service life.

Method used

Using plastic polymer as the substrate, adding carbon fiber and metal oxide as transverse reinforcement materials, and continuous glass fiber or carbon fiber as longitudinal reinforcement materials, a new type of insulating light unit outer sleeve is designed to improve its high temperature resistance and compressive tensile resistance. Resistant shrinkage.

Benefits of technology

It significantly improves the high temperature resistance of the insulated light unit, extends the service life, avoids the intensity drop caused by high temperature, and ensures that there is no deformation under the action of high temperature for a long time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118915251A_ABST
    Figure CN118915251A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of power grid materials, and particularly discloses an insulated optical unit, a preparation method and application of the insulated optical unit in an optical fiber composite overhead ground wire. According to the novel insulating optical unit outer sleeve, the plastic polymer is used as a base material, the carbon fibers and the metal oxides are used as transverse reinforcing materials, and the continuous glass fibers or the continuous carbon fibers are used as longitudinal reinforcing materials, so that the high temperature resistance of the insulating optical unit outer sleeve at continuous high temperature is greatly improved; and under the action of long-time high-strength ice melting current, the ice melting device can be kept stable and does not deform. The problem that the service life is shortened due to the fact that the strength of the insulating optical unit affected by high temperature is reduced and the surface is prone to deformation in the existing ice melting process is effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of power grid materials, and specifically discloses an insulating optical unit, a preparation method thereof and application thereof in an optical fiber composite overhead ground wire. Background Art

[0002] The frequent occurrence of extreme cold weather has had many adverse effects on the power grid, such as a large number of trains delayed or even canceled due to icing on the contact network of high-speed rail lines, and severe damage to transmission lines due to surface icing, causing huge casualties and property losses. In the face of this problem, engineers have taken a variety of measures to deal with it.

[0003] In the face of the adverse effects of ice and snow disasters on power grids, DC ice melting is currently the main means of ice melting. DC current ice melting uses the ice-covered line as a load to apply a DC power supply, and uses a relatively low voltage to provide a short-circuit current to heat the conductor to melt the ice. For long-distance, large-capacity transmission lines of 500kV and above, the DC resistance is only 1 / 10 of the AC impedance. The power capacity required for DC ice melting is significantly lower than that for AC ice melting, which has significant advantages in the ice melting process and has been widely used in my country.

[0004] Optical fiber composite overhead ground wire (OPGW) has the functions of both lightning arrester and communication channel, and is widely used in high-voltage transmission lines. Unlike overhead wires that are energized, the current passing through the optical fiber composite overhead ground wire is very small under normal operation, and it is more likely to be covered with ice when the weather conditions are bad. The icing of overhead ground wires and optical fiber composite overhead ground wires is second only to the icing of phase lines, and has become an important factor restricting the normal operation of the line. In order to meet the requirements of DC ice melting, the optical fiber composite overhead ground wire needs to be insulated and transformed. Before the arrival of ice and snow in winter every year, the entire optical fiber composite overhead ground wire will be insulated and operated to meet the requirements of DC ice melting; after the thunderstorm season and before the arrival of winter, the optical fiber composite overhead ground wire that has undergone insulation transformation will be grounded to meet the requirements of line lightning protection and induced overvoltage.

[0005] In order to save energy and reduce consumption and facilitate the de-icing of optical fiber composite overhead ground wires, the existing technology is to isolate the grounding hardware, down conductor part and junction box of conventional optical fiber composite overhead ground wires from the pole tower through an insulating string. During the entire de-icing process of the optical fiber composite overhead ground wire, the temperature of the entire cable outer layer exceeds 100°C, and the temperature inside the optical cable exceeds 80°C. Existing insulating optical units generally use high-temperature resistant organic polymers such as polytetrafluoroethylene or ethylene-tetrafluoroethylene copolymer as outer sleeves, but there are still problems such as the strength of the insulating optical unit decreases during the de-icing process, and the surface is deformed due to high temperature, resulting in a shortened service life.

[0006] Based on this, developing an insulating optical unit with excellent comprehensive performance, long service life, stable optical unit strength and the ability to withstand high temperature for a long time has a significant progressive significance for the de-icing of optical fiber composite overhead ground wires. Summary of the invention

[0007] In view of the problem that the strength of the insulating optical unit is reduced due to high temperature during the existing ice melting process, and the surface is easily deformed, resulting in a shortened service life, the present invention provides an insulating optical unit, a preparation method thereof, and its application in an optical fiber composite overhead ground wire. The present invention designs a new insulating optical unit outer sleeve, which uses a plastic polymer as a base material, carbon fiber and metal oxide as lateral reinforcement materials, and continuous glass fiber or continuous carbon fiber material as a longitudinal reinforcement material, which greatly improves the high temperature resistance of the insulating optical unit outer sleeve under continuous high temperature.

[0008] To achieve this object of the invention, the present invention provides the following technical solutions:

[0009] The first aspect of the present invention provides an insulating optical unit, which comprises, from inside to outside, an optical fiber, a water-blocking grease, and an outer sleeve;

[0010] The outer sleeve comprises the following raw materials in percentage by mass: 1%-3% of a first fiber material, 1%-2% of a metal oxide, 20%-30% of a second fiber material and the remainder of a plastic polymer matrix.

[0011] Compared with the prior art, the present invention uses a plastic polymer as a substrate, a first fiber material and a metal oxide as a transverse reinforcement material, and a second fiber material as a longitudinal reinforcement material to prepare a new insulating optical unit outer sleeve. Among them, the addition of the first fiber material can significantly improve the thermal conductivity of the insulating optical unit outer sleeve, and the first fiber material can absorb part of the ultraviolet rays and extend the service life of the insulating optical unit; and the metal oxide can improve the transverse compressive resistance of the insulating optical unit outer sleeve, so that the insulating optical unit outer sleeve can maintain a high compressive resistance even if it is slightly softened under the high temperature generated by ice melting. The addition of the second fiber material can improve the axial tensile and shrinkage resistance of the insulating optical unit outer sleeve. Compared with the existing insulating optical unit outer sleeve using polytetrafluoroethylene or ethylene-tetrafluoroethylene copolymer, the insulating optical unit outer sleeve of the present invention has good compressive, tensile, shrinkage and long service life, so that the obtained insulating optical unit can withstand high temperature for a long time during ice melting, avoiding the decrease in the strength of the optical unit caused by high temperature. At the same time, the water-blocking grease can maintain the stability of the optical fiber inside the insulating optical unit, and greatly support the ice melting operation of the power grid ground wire. The insulating light unit provided by the present invention effectively solves the problem that the strength of the insulating light unit is reduced due to high temperature during the existing ice melting process, and the surface is easily deformed, resulting in a shortened service life.

[0012] Preferably, the first fiber material has a length of 3 mm to 5 mm and a diameter of 5 μm to 10 μm.

[0013] Preferably, the particle size of the metal oxide is 5 μm-75 μm.

[0014] More preferably, the metal oxide is any one or both of aluminum oxide and magnesium oxide.

[0015] Preferably, the diameter of the second fiber material is 5 μm-75 μm.

[0016] The length of the second fiber material is determined by the length of the insulating optical unit and is determined according to actual conditions.

[0017] Preferably, the polymer substrate is any one or more of polybutylene terephthalate, polycarbonate, polypropylene or polyetheretherketone.

[0018] Preferably, the first fiber material is carbon fiber.

[0019] Preferably, the second fiber material is any one or both of continuous glass fiber and continuous first fiber material.

[0020] Preferably, the water-blocking paste is any one of a low hydrogen evolution water-blocking paste and a hydrogen absorption water-blocking paste.

[0021] The water-blocking ointment used in the present invention is a viscous semi-solid substance formed by dispersing a gelling agent into a base oil. The water-blocking ointment can protect the optical fiber inside the insulating optical unit to form a protective effect, not only to prevent moisture from corroding the optical fiber, but also to play a cushioning role for the optical fiber, to buffer the influence of mechanical forces such as vibration, impact or bending on the optical fiber, and to maintain the stability of the optical fiber.

[0022] Preferably, the optical fiber is a colored optical fiber, and the preparation method comprises the following steps: coating an organic-mineral composite pigment on the surface of the optical fiber, and drying at 80-130° C. in an inert atmosphere to obtain the colored optical fiber.

[0023] The present invention adopts colored optical fiber to ensure that the color of the optical fiber is clear and bright after coating, and the optical fiber surface is not damaged, so as to facilitate the identification of optical fiber types.

[0024] Preferably, the organic-mineral composite pigment is a polypropylene-mineral composite pigment.

[0025] Preferably, the coating thickness of the organic-mineral composite pigment is 3 μm-5 μm.

[0026] Preferably, the drying time is 20 min-35 min.

[0027] A second aspect of the present invention provides a method for preparing the insulating light unit, comprising the following steps:

[0028] S1. In an inert atmosphere, heating the first fiber material to 120° C.-160° C. and keeping the temperature for 1 h-3 h to obtain a pretreated first fiber material;

[0029] S2, heating the metal oxide and the second fiber material to 120° C.-160° C. respectively, and keeping the temperature for 1 h-3 h to obtain a pretreated metal oxide and a pretreated second fiber material;

[0030] S3, mixing the polymer substrate, the pretreated first fiber material, the pretreated metal oxide and the pretreated second fiber material uniformly according to the designed ratio, heating to 350° C.-400° C. to extrude into a tube, and cooling to obtain the outer sleeve of the insulating light unit;

[0031] S4. An optical fiber is arranged in the outer sleeve of the insulating optical unit, and a water-blocking grease is filled between the outer sleeve of the insulating optical unit and the optical fiber to obtain an insulating optical unit.

[0032] The third aspect of the present invention provides an optical fiber composite overhead ground wire, which comprises a central layer, a second outer layer and an outermost layer from the inside to the outside; wherein the central layer and the second outer layer both comprise the insulating optical unit.

[0033] Preferably, the central layer is composed of an insulating optical unit, an aluminum sleeve layer and a twisted aluminum clad steel wire layer from the inside to the outside.

[0034] Preferably, the secondary outer layer is formed by twisting an insulating optical unit and an aluminum-clad steel wire.

[0035] Preferably, the outermost layer is a stranded aluminum wire layer.

[0036] Further preferably, the sum of the number of insulating optical units and aluminum-clad steel wires in the sub-outer layer is 5-10.

[0037] Further preferably, the number of aluminum clad steel wires in the twisted aluminum clad steel wire layer is 6-12.

[0038] Further preferably, the number of aluminum wires in the twisted aluminum wire layer is 12-18.

[0039] A fourth aspect of the present invention provides the use of the optical fiber composite overhead tape line in power grid ice melting.

[0040] In summary, in view of the problem that the strength of the insulating optical unit is reduced due to high temperature during the existing ice melting process, and the surface is easily deformed, resulting in a shortened service life, the present invention provides an insulating optical unit, a preparation method and its application in an optical fiber composite overhead ground wire. The present invention designs a new insulating optical unit outer sleeve, which uses a plastic polymer as a base material, short carbon fiber and metal oxide as lateral reinforcement materials, and continuous glass fiber or continuous carbon fiber as a longitudinal reinforcement material, which greatly improves the performance of the insulating sleeve under continuous high temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 Schematic diagram of the cross-sectional structure of the insulating optical unit; 1 is the outer sleeve of the insulating optical unit; 2 is the optical fiber; 3 is the water-blocking grease;

[0042] Figure 2 This is a schematic diagram of the cross-sectional structure of the optical fiber composite overhead ground wire, where 1 is the insulating optical unit; 2 is the aluminum-clad steel wire; 3 is the aluminum sheath layer; and 4 is the twisted aluminum wire layer. DETAILED DESCRIPTION

[0043] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] Example 1

[0045] This embodiment provides an insulating light unit, which specifically includes the following contents:

[0046] The insulating optical unit includes colored optical fiber, low hydrogen evolution water-blocking paste and outer sleeve from the inside to the outside, wherein the outer sleeve includes the following raw material components by mass percentage: 2% carbon fiber, 2% metal oxide, 25% continuous carbon fiber and 71% polybutylene terephthalate substrate. The specific preparation method is as follows:

[0047] S1. In an inert atmosphere, heat a carbon fiber with a length of 4 mm and a diameter of 10 μm to 150° C. and keep the temperature for 2 hours to obtain a pretreated first fiber material;

[0048] S2, heating the aluminum oxide particles with a particle size of 50 μm and the continuous carbon fibers with a diameter of 25 μm to 140° C. respectively, and keeping the temperature for 2 hours to obtain a pretreated metal oxide and a pretreated second fiber material;

[0049] S3, mixing the polybutylene terephthalate substrate, the pretreated short-segment first fiber material, the pretreated metal oxide and the pretreated second fiber material evenly according to the designed ratio, heating to 380° C. for extrusion, and cooling into a tube to obtain the outer sleeve of the insulating light unit;

[0050] S4. A colored optical fiber is arranged in the outer sleeve of the insulating optical unit, and a low hydrogen evolution water-blocking grease is filled between the outer sleeve of the insulating optical unit and the optical fiber to obtain an insulating optical unit.

[0051] The method for preparing the colored optical fiber comprises the following steps: coating the surface of the optical fiber with a polypropylene-blue vitriol composite pigment having a thickness of 3 μm, and drying the pigment at 120° C. for 30 minutes under an inert atmosphere to obtain the colored optical fiber.

[0052] Example 2

[0053] This embodiment provides an insulating light unit, which specifically includes the following contents:

[0054] The insulating optical unit includes colored optical fiber, low hydrogen evolution water blocking grease and outer sleeve from the inside to the outside, wherein the outer sleeve includes the following raw material components by mass percentage: 2% carbon fiber, 2% metal oxide, 25% continuous glass fiber and 71% polycarbonate substrate. The specific preparation method is as follows:

[0055] S1. In an inert atmosphere, heat a carbon fiber with a length of 3.5 mm and a diameter of 8 μm to 140° C. and keep the temperature for 1.5 h to obtain a pretreated first fiber material;

[0056] S2, heating the magnesium oxide particles with a particle size of 35 μm and the continuous glass fiber with a diameter of 45 μm to 150° C. respectively, and keeping the temperature for 1.5 hours to obtain a pretreated metal oxide and a pretreated second fiber material;

[0057] S3, mixing the polycarbonate substrate, the pretreated first fiber material, the pretreated metal oxide and the pretreated second fiber material uniformly according to the designed ratio, heating to 360° C. for extrusion, and cooling into a tube to obtain the outer sleeve of the insulating light unit;

[0058] S4. A colored optical fiber is arranged in the outer sleeve of the insulating optical unit, and a low hydrogen evolution water-blocking grease is filled between the outer sleeve of the insulating optical unit and the optical fiber to obtain an insulating optical unit.

[0059] The method for preparing the colored optical fiber comprises the following steps: coating the surface of the optical fiber with a polypropylene-iron red composite pigment having a thickness of 5 μm, and drying the pigment at 110° C. for 30 minutes under an inert atmosphere to obtain the colored optical fiber.

[0060] Example 3

[0061] This embodiment provides an insulating light unit, which specifically includes the following contents:

[0062] The insulating optical unit includes colored optical fiber, OPGW optical cable special hydrogen absorption and water blocking paste and outer sleeve from the inside to the outside, wherein the outer sleeve includes the following raw material components by mass percentage: 3% carbon fiber, 1% metal oxide, 24.5% continuous glass fiber and 71.5% polycarbonate substrate. The specific preparation method is as follows:

[0063] S1. In an inert atmosphere, heat a carbon fiber with a length of 5 mm and a diameter of 8 μm to 160° C. and keep the temperature for 1 hour to obtain a pretreated first fiber material;

[0064] S2, heating the aluminum oxide particles with a particle size of 15 μm and the continuous glass fiber with a diameter of 60 μm to 140° C. respectively, and keeping the temperature for 2 hours to obtain a pretreated metal oxide and a pretreated second fiber material;

[0065] S3, mixing the polycarbonate substrate, the pretreated first fiber material, the pretreated metal oxide and the pretreated second fiber material uniformly according to the designed ratio, heating to 390° C. for extrusion, and cooling into a tube to obtain the outer sleeve of the insulating light unit;

[0066] S4. A colored optical fiber is arranged in the outer sleeve of the insulating optical unit, and a hydrogen-absorbing and water-blocking paste specially used for OPGW optical cables is filled between the outer sleeve of the insulating optical unit and the optical fiber to obtain an insulating optical unit.

[0067] The method for preparing the colored optical fiber comprises the following steps: coating the surface of the optical fiber with a polypropylene-iron red composite pigment having a thickness of 3 μm, and drying the mixture at 100° C. for 25 minutes in an inert atmosphere to obtain the colored optical fiber.

[0068] Example 4

[0069] This embodiment provides an insulating light unit, which specifically includes the following contents:

[0070] The insulating optical unit includes colored optical fiber, OPGW optical cable special hydrogen absorption and water blocking grease and outer sleeve from the inside to the outside, wherein the outer sleeve includes the following raw material components in percentage by weight: 1% of the first fiber material, 1.5% of the metal oxide, 28.5% of the continuous carbon fiber and 69% of the polyetheretherketone substrate. The specific preparation method is as follows:

[0071] S1. In an inert atmosphere, heat a carbon fiber with a length of 4 mm and a diameter of 10 μm to 150° C. and keep the temperature for 2 hours to obtain a pretreated first fiber material;

[0072] S2, heating the aluminum oxide particles with a particle size of 50 μm and the continuous carbon fibers with a diameter of 25 μm to 140° C. respectively, and keeping the temperature for 2 hours to obtain a pretreated metal oxide and a pretreated second fiber material;

[0073] S3, mixing the polycarbonate substrate, the pretreated first fiber material, the pretreated metal oxide and the pretreated second fiber material uniformly according to the designed ratio, heating to 400° C. for extrusion, and cooling into a tube to obtain the outer sleeve of the insulating light unit;

[0074] S4. A colored optical fiber is arranged in the outer sleeve of the insulating optical unit, and a hydrogen-absorbing and water-blocking paste specially used for OPGW optical cables is filled between the outer sleeve of the insulating optical unit and the optical fiber to obtain an insulating optical unit.

[0075] The method for preparing the colored optical fiber comprises the following steps: coating the surface of the optical fiber with a polypropylene-copper green composite pigment having a thickness of 4 μm, and drying the pigment at 100° C. for 30 minutes under an inert atmosphere to obtain the colored optical fiber.

[0076] Example 5

[0077] This embodiment provides an insulating light unit, which specifically includes the following contents:

[0078] The insulating optical unit includes colored optical fiber, OPGW optical cable special hydrogen absorption and water blocking grease and outer sleeve from the inside to the outside, wherein the outer sleeve includes the following raw material components by mass percentage: 3% carbon fiber, 2% metal oxide, 30% continuous carbon fiber and 65% polypropylene substrate. The specific preparation method is as follows:

[0079] S1. In an inert atmosphere, heating a first fiber material having a length of 4 mm and a diameter of 6 μm to 155° C. and keeping the temperature for 1.5 h to obtain a pretreated first fiber material;

[0080] S2, heating the magnesium oxide particles with a particle size of 50 μm and the continuous carbon fibers with a diameter of 25 μm to 125° C. respectively, and keeping the temperature for 3 hours to obtain a pretreated metal oxide and a pretreated second fiber material;

[0081] S3, mixing the polycarbonate substrate, the pretreated short-segment first fiber material, the pretreated metal oxide and the pretreated second fiber material evenly according to the designed ratio, heating to 400° C. for extrusion, and cooling into a tube to obtain the outer sleeve of the insulating light unit;

[0082] S4. A colored optical fiber is arranged in the outer sleeve of the insulating optical unit, and a hydrogen-absorbing and water-blocking paste specially used for OPGW optical cables is filled between the outer sleeve of the insulating optical unit and the optical fiber to obtain an insulating optical unit.

[0083] The method for preparing the colored optical fiber comprises the following steps: coating the surface of the optical fiber with a polypropylene-cinnabar composite pigment having a thickness of 4 μm, and drying the pigment at 90° C. for 35 minutes under an inert atmosphere to obtain the colored optical fiber.

[0084] Comparative Example 1

[0085] This comparative example provides an insulating light unit, which is different from Example 1 in that the outer sleeve of the insulating light unit is made of polytetrafluoroethylene plastic, and other materials remain unchanged, specifically including the following contents:

[0086] A colored optical fiber is arranged in a polytetrafluoroethylene plastic tube, and a low hydrogen evolution water-blocking paste is filled between the outer sleeve of the insulating optical unit and the optical fiber to obtain an insulating optical unit.

[0087] The method for preparing the colored optical fiber comprises the following steps: coating the surface of the optical fiber with a polypropylene-blue vitriol composite pigment having a thickness of 3 μm, and drying the pigment at 120° C. for 30 minutes under an inert atmosphere to obtain the colored optical fiber.

[0088] Comparative Example 2

[0089] This comparative example provides an insulating light unit, which is different from Example 1 in that the outer sleeve of the insulating light unit is made of ethylene-tetrafluoroethylene copolymer plastic, and other materials remain unchanged, specifically including the following contents:

[0090] A colored optical fiber is arranged in an ethylene-tetrafluoroethylene copolymer plastic tube, and a low hydrogen evolution water-blocking paste is filled between the outer sleeve of the insulating optical unit and the optical fiber to obtain an insulating optical unit.

[0091] The method for preparing the colored optical fiber comprises the following steps: coating the surface of the optical fiber with a polypropylene-blue vitriol composite pigment having a thickness of 3 μm, and drying the pigment at 120° C. for 30 minutes under an inert atmosphere to obtain the colored optical fiber.

[0092] Comparative Example 3

[0093] This comparative example provides an insulating light unit, which is different from Example 1 in that the outer sleeve of the insulating light unit is made of polybutylene terephthalate plastic, and other materials remain unchanged, specifically including the following contents:

[0094] A colored optical fiber is arranged in a polybutylene terephthalate plastic tube, and a low hydrogen evolution water-blocking paste is filled between the outer sleeve of the insulating optical unit and the optical fiber to obtain an insulating optical unit.

[0095] The method for preparing the colored optical fiber comprises the following steps: coating the surface of the optical fiber with a polypropylene-blue vitriol composite pigment having a thickness of 3 μm, and drying the pigment at 120° C. for 30 minutes under an inert atmosphere to obtain the colored optical fiber.

[0096] In order to further reflect the technical effect of applying the insulating optical unit provided by the present invention to the optical fiber composite overhead ground wire, the present invention uses the insulating optical units obtained in Examples 1-4 and Comparative Examples 1-3 to prepare the optical fiber composite overhead ground wire according to the operation of the test example, which specifically includes the following contents:

[0097] Test example

[0098] The optical fiber composite overhead ground wire includes a central layer, a second outer layer and an outermost layer from the inside to the outside, and specifically includes the following contents:

[0099] Step 1: Select an insulating optical unit as the central layer reinforcement, and set an aluminum sleeve layer on the outside of it, and then use a stranding machine to strand 10 aluminum-clad steel wires outside the aluminum sleeve layer to form the central layer;

[0100] Step 2: Using a twisting machine, twist one insulating optical unit and five aluminum-clad steel wires outside the center layer obtained in step 1 to obtain a secondary outer layer;

[0101] Step 3: Use a twisting machine to twist 12 aluminum wires in the secondary outer layer to obtain an optical fiber composite overhead ground wire.

[0102] In order to further reflect the technical effect of the present invention, the present invention uses the insulating optical units obtained in Examples 1-5 and Comparative Examples 1-3 to prepare optical fiber composite overhead ground wires according to the test examples, and conducts relevant performance tests on them. The obtained optical fiber composite overhead ground wire is short-circuited for 30 minutes under an ice melting current of 2000-3000A, and the deformation of the outer sleeve of the insulating optical unit is observed. The results are shown in Table 1.

[0103] Table 1 Deformation results of the outer sleeve of the insulating optical unit

[0104]

[0105]

[0106] It can be seen from Table 1 that the outer sleeve of the insulating light unit provided in Examples 1-5 of the present invention has excellent high temperature resistance and the outer sleeve of the insulating light unit will not be deformed even under the action of a long-term high ice-melting current.

[0107] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. An insulating light unit, characterized in that: From inside to outside, it includes optical fiber, water-blocking grease and outer sleeve; The outer sleeve comprises the following raw materials in percentage by mass: 1%-3% of a first fiber material, 1%-2% of a metal oxide, 20%-30% of a second fiber material and the remainder of a plastic polymer matrix.

2. The insulating light unit according to claim 1, characterized in that: The first fiber material has a length of 3 mm to 5 mm and a diameter of 5 μm to 10 μm; and / or The particle size of the metal oxide is 5 μm-75 μm; and / or The diameter of the second fiber material is 5 μm-75 μm.

3. The insulating light unit according to claim 1, wherein: The plastic polymer substrate is any one or more of polybutylene terephthalate, polycarbonate, polypropylene or polyetheretherketone; and / or The first fiber material is carbon fiber; and / or The second fiber material is any one or both of continuous glass fiber and continuous carbon fiber; and / or The water-blocking ointment is any one of a low hydrogen evolution water-blocking ointment and a hydrogen absorption water-blocking ointment.

4. The insulating light unit according to claim 1, wherein: The optical fiber is a colored optical fiber, and the preparation method comprises the following steps: coating an organic-mineral composite pigment on the surface of the optical fiber, and drying it at 80-130° C. in an inert atmosphere to obtain the colored optical fiber.

5. The insulating light unit according to claim 4, characterized in that: The organic-mineral composite pigment is a polypropylene-mineral composite pigment; and / or The coating thickness of the organic-mineral composite pigment is 3 μm-5 μm; and / or The drying time is 20 min-35 min.

6. A method for preparing an insulating optical unit according to any one of claims 1 to 5, characterized in that: The steps include: S1. In an inert atmosphere, heating the first fiber material to 120° C.-160° C. and keeping the temperature for 1 h-3 h to obtain a pretreated first fiber material; S2, heating the metal oxide and the second fiber material to 120° C.-160° C. respectively, and keeping the temperature for 1 h-3 h to obtain a pretreated metal oxide and a pretreated second fiber material; S3, mixing the polymer substrate, the pretreated first fiber material, the pretreated metal oxide and the pretreated second fiber material uniformly according to the designed ratio, heating to 350° C.-400° C. to extrude into a tube, and cooling to obtain the outer sleeve of the insulating light unit; S4. An optical fiber is arranged in the outer sleeve of the insulating optical unit, and a water-blocking grease is filled between the outer sleeve of the insulating optical unit and the optical fiber to obtain an insulating optical unit.

7. An optical fiber composite overhead ground wire, characterized in that: From the inside to the outside, it includes a central layer, a sub-outer layer and an outermost layer in sequence; wherein the central layer and the sub-outer layer both include the insulating light unit described in any one of claims 1-5.

8. The optical fiber composite overhead ground wire according to claim 7, characterized in that: The central layer includes the insulating optical unit, the aluminum sleeve layer and the twisted aluminum clad steel wire layer in sequence from the inside to the outside; and / or The secondary outer layer is formed by twisting the insulating optical unit and the aluminum clad steel wire; and / or The outermost layer is a stranded aluminum wire layer.

9. The optical fiber composite overhead ground wire according to claim 8, characterized in that: The sum of the number of insulating optical units and aluminum-clad steel wires in the sub-outer layer is 5-10; and / or The number of aluminum clad steel wires in the twisted aluminum clad steel wire layer is 6-12; and / or The number of aluminum wires in the twisted aluminum wire layer is 12-18.

10. Use of the optical fiber composite overhead tape line according to any one of claims 7 to 9 in power grid ice melting.