Polarization beam splitting prism, polarization beam splitting plate and preparation method and application of polarization beam splitting prism and polarization beam splitting plate

By using H-Lak7 optical glass and alternate laminated film layer structure, the substrate deformation and bubble problems of existing polarized spectroscopy plates during coating are solved, and better polarized spectroscopy performance and processing efficiency are achieved.

CN118915327APending Publication Date: 2024-11-08大鼎光学薄膜(中山)有限公司 +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411106058.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing polarized spectroscopy plates are prone to introduce defects during coating, resulting in substrate deformation and bubbles, affecting optical performance.

Method used

H-Lak7 optical glass is used as the substrate, and alternately stacked Ta2O5 and SiO2 film layers are designed to reduce the thickness of the film layer, improve polarization spectroscopy performance, and reduce substrate deformation and bubble risks.

Benefits of technology

It achieves better polarization spectroscopy effect, reduces film layer thickness, improves processing efficiency, reduces appearance defects, and improves cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118915327A_ABST
    Figure CN118915327A_ABST
Patent Text Reader

Abstract

The invention discloses a polarization splitting prism, a polarization splitting plate and a preparation method and application of the polarization splitting prism and the polarization splitting plate. According to the polarization splitting prism, through the H-Lak7 base material and the adaptive beam splitting film structure design, the film layer thickness is greatly reduced, and the polarization splitting prism has better optical performance, machinability and appearance. The invention also provides a polarization beam splitter comprising the polarization splitting prism, a preparation method of the polarization beam splitter, and applications of the polarization splitting prism and the polarization beam splitter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of optical materials, and in particular to a polarization beam splitter prism, a polarization beam splitter plate, and a preparation method and application thereof. Background Art

[0002] Light has a polarization state. If the polarization vector of the light is in the plane where the incident light and the reflected light are located, it is called p-polarization. If the polarization vector is perpendicular to the plane, it is called s-polarization. When light enters the film at a non-perpendicular angle, it can be decomposed into P light and S light. The polarization splitter film is a film used to achieve P light transmission and S light cutoff. It has been widely used in laser technology, optical fiber communication technology, optoelectronic instruments and other fields.

[0003] One application method is to laminate a polarization beam splitter film on the surface of an optical substrate (such as optical glass) to form a polarization beam splitter prism, and glue multiple polarization beam splitter prisms together to form a polarization beam splitter plate. Most of the existing commercially used polarization beam splitters use high-transmittance B270 glass or BK7 glass, and their matching film systems are relatively thick, which can easily introduce defects during the coating process, and easily cause deformation of the substrate after coating, resulting in bubbles in the subsequent gluing process, affecting the optical performance.

[0004] Therefore, it is necessary to develop a polarization beam splitter with better optical performance. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a polarization beam splitter prism, which can improve the polarization beam splitting performance of an optical element (such as a polarization beam splitter plate) including the polarization beam splitter prism.

[0006] The invention also provides a polarization beam splitter.

[0007] The present invention also provides a method for preparing the polarization beam splitter.

[0008] The present invention also provides the application of the polarization beam splitter prism or the polarization beam splitter plate.

[0009] The first embodiment of the present invention relates to a polarization beam splitter prism, comprising: a first base layer, the material of which is H-Lak7 optical glass; a first beam splitter film formed on at least one side of the surface of the base layer, the film layer structure of the first beam splitter film is: from the first base layer side, it includes Ta2O5 layers and SiO2 layers alternately stacked in sequence, a total of 23 layers, and the layer thickness is 26.65-28.65nm, 283.08-287.08nm, 109.67-111.6 7nm, 218.28~222.28nm, 91.28~93.28nm, 177.06~181.06nm, 84.37~86.37nm, 204.95~208.95nm, 66.32 ~68.32nm, 127.51~131.51nm, 52.63~54.63nm, 226.66~230.66nm, 68.04~70.04nm, 107.92~111.92nm,

[0010] 50.9~52.9nm, 106.58~110.58nm, 55.85~57.85nm, 101.03~105.03nm, 50.27~ 52.27nm, 85.08~89.08nm, 52.44~54.44nm, 94.43~98.43nm, 33.18~35.18nm.

[0011] The polarization beam splitter prism according to the first aspect of the present invention has at least the following beneficial effects:

[0012] H-Lak7 is a lanthanum crown glass, the main components of which include oxides such as silicon dioxide (SiO2), aluminum oxide (Al2O3), calcium oxide (CaO), and lanthanum oxide (La2O3). Compared with the commonly used B270 or BK7 glass, H-Lak7 has a higher refractive index in the range of 1.71 to 1.72, which is conducive to achieving excellent polarization splitting effects in a wider band. Through the design of H-Lak7 substrate and adapted film system, the film thickness is greatly reduced. The total thickness of the film layer is about 2500nm, which is significantly lower than the film system (about 9000nm) adapted to the conventional B270 or BK7 substrate. The film layer is thin, the substrate is not easy to deform, and it is easier to glue, reducing appearance defects such as bubbles and splashes.

[0013] The applicable band of the polarization beam splitter prism is 425nm-650nm, and the air incident angle is 0±8°. In the working band, when the incident angle is 0°, the average transmittance of the beam splitter film to S light is ≤0.1%, and the average transmittance to P light is ≥97%; when the incident angle is 0°±8°, the average transmittance of the beam splitter film to S light is ≤2%, and the average transmittance to P light is ≥94%, with excellent optical properties.

[0014] H-LaK7 material has good processability and a hardness FA value of 76, which is more suitable for plane processing. H-LaK7 has high UV transmittance and is suitable for light-curing bonding process. At the same time, the thin film layer of the beam splitter is more conducive to UV light transmission, achieving rapid light curing and improving processing efficiency.

[0015] In terms of cost, H-Lak7 material is slightly more expensive, but the film layer of the spectroscopic film is thinner and the production time is shorter, which basically does not increase the overall cost. At the same time, it has better performance and higher cost performance.

[0016] In some embodiments, the film layer structure of the first splitter film is as follows: from the first base layer side, it includes 23 layers of Ta2O5 layers and SiO2 layers alternately stacked in sequence, and the layer thicknesses are 27.65nm, 285.08nm, 110.67nm, 220.28nm, 92.28nm, 179.06nm, 85.37nm, 206.95nm, 67.32nm, 129.51nm,

[0017] 53.63nm, 228.66nm, 69.04nm, 109.92nm, 51.9nm, 108.58nm, 56.85nm, 103.03nm,

[0018] 51.27nm, 87.08nm, 53.44nm, 96.43nm, 34.18nm.

[0019] In some embodiments, the first base layer has a triangular prism or quadrangular prism structure. A triangular prism has two parallel and congruent triangular bottom surfaces and three quadrilateral sides connecting these bottom surfaces. A quadrangular prism has two parallel and congruent quadrilateral bottom surfaces and four quadrilateral sides connecting these bottom surfaces. The quadrilateral can be a rectangle, a parallelogram or a square.

[0020] In some embodiments, the first prismatic film is formed on at least one side surface of the triangular prism or the quadrangular prism.

[0021] In some embodiments, the first base layer is a right triangular prism, that is, it has two parallel and congruent triangular bases, and the side surfaces connecting the bases are all rectangular or square.

[0022] In some embodiments, the first substrate is a right triangular prism having two parallel and congruent right-angled triangle bottom surfaces, and the first prismatic film is formed on a side surface connecting the hypotenuses of the two right-angled triangle bottom surfaces.

[0023] In some embodiments, the right triangle base is an equilateral right triangle base.

[0024] In some embodiments, the length of the right angle side of the equilateral right triangle base is 0.5-1 mm, and the distance between the equilateral right triangle bases is 14-16 mm.

[0025] In some embodiments, the first base layer has a quadrangular prism structure and has two parallel and congruent rectangular bottom surfaces, a group of side surfaces connecting the long sides of the bottom surfaces are rectangular, and the first prismatic film is formed on one of the rectangular side surfaces.

[0026] In some embodiments, in the first base layer, a group of side surfaces connecting the short sides of the bottom surface is a parallelogram with an acute angle of 45°.

[0027] In some embodiments, in the first base layer, the bottom surface has a length of 14 to 16 mm, a width of 0.5 to 1 mm, and a distance between the bottom surfaces of 0.5 to 1 mm.

[0028] A second aspect of the present invention relates to a polarization beam splitter plate, comprising the polarization beam splitter prism described above.

[0029] In view of the characteristics of the polarization beam splitter prism described above, the polarization beam splitter plate has better optical characteristics and processability.

[0030] In some embodiments, the polarization beam splitter plate includes: a glued quadrangular prism, including a plurality of first polarization beam splitter prisms glued in sequence, the first polarization beam splitter prism having a second base layer, the second base layer having a quadrangular prism structure, a second beam splitter film formed on one side surface of the second base layer, the second beam splitter film of one of the first polarization beam splitter prisms being glued to the other side surface opposite to the second beam splitter film of the adjacent first polarization beam splitter prism, and the bottom surface on the same side of the second base layer and another group of side surfaces connected to the bottom surface are respectively located in the same plane;

[0031] A second polarizing beam splitter prism, comprising a third base layer of a right triangular prism, a third beam splitter film being formed on one side of the third base layer, and the third beam splitter film being glued to a surface of the outermost side of the glued quadrangular prism opposite to the second beam splitter film;

[0032] A third polarization beam splitter prism, comprising a fourth base layer of a right triangular prism, wherein one side surface of the fourth base layer is glued to the outermost second beam splitter film of the glued quadrangular prism;

[0033] The materials of the second base layer, the third base layer and the fourth base layer are all H-Lak7 optical glass, and the film layer structure of the second beam splitting film starting from the second base layer side and the film layer structure of the third beam splitting film starting from the third base layer side are the same as the film layer structure of the first beam splitting film starting from the first base layer side defined above; the glued quadrangular prism, the second polarization beam splitting prism and the third polarization beam splitting prism are glued to form a rectangular structure.

[0034] In some embodiments, the number of the first polarization beam splitting prisms is 16.

[0035] In some embodiments, the polarization beam splitter plate further includes 8 1 / 2 wavelength plates, one side bottom surface of the second base layer is the incident surface, and the other side bottom surface is the exit surface, and the 8 1 / 2 wavelength plates are respectively located on the exit surface side of the 8 first polarization beam splitter prisms in the glued quadrangular prism, and a first polarization beam splitter prism is spaced between two adjacent 1 / 2 wavelength plates. When linearly polarized light passes through the 1 / 2 wavelength plate, its phase will be delayed by half a wavelength, so that the polarization direction of the light can be adjusted to better adapt to the working angle. The material of the 1 / 2 wavelength plate can be quartz crystal or resin material, etc., with a thickness of, for example, 0.05 to 0.2 mm.

[0036] In some embodiments, the 1 / 2 wavelength plate is glued to the first polarization beam splitter prism.

[0037] In some embodiments, a first anti-reflection film is disposed on one side of the incident surface of the polarization beam splitter, and a second anti-reflection film is disposed on a surface of the polarization beam splitter opposite to the incident surface.

[0038] In some embodiments, the thickness of the first anti-reflection film and the second anti-reflection film is independently 250-300 nm. The anti-reflection film is used to reduce the reflection of light and improve the transmittance. The material of the anti-reflection film can be Ta2O5 film and SiO2 film deposited alternately in sequence, or TiO2 film and SiO2 film deposited alternately in sequence. Non-limiting examples of the total number of film layers are: 5 to 9 layers, specifically 5 layers, 6 layers, 7 layers, 8 layers or 9 layers. The thickness of each layer can be selected based on experience in the field. For example, when Ta2O5 films and SiO2 films are deposited alternately in sequence (a total of 6 layers), non-limiting examples of layer thickness are: 11.3nm, 42.31nm, 45.36nm, 8.41nm, 69.75nm, 87.72nm; if TiO2 films and SiO2 films are deposited alternately in sequence (a total of 6 layers), non-limiting examples of layer thickness are: 13.62nm, 32.69nm, 52.91nm, 10nm, 37.95nm, 89.65nm.

[0039] In some embodiments, in the first polarization beam splitter prism, the bottom surface of the second base layer is rectangular, a group of side surfaces connecting the long sides of the bottom surface are rectangular, and the second beam splitter film is formed on one of the rectangular side surfaces.

[0040] In some embodiments, in the first polarization beam splitter prism, a group of side surfaces connecting the short sides of the bottom surface is a parallelogram with an acute angle of 45°.

[0041] In some embodiments, in the first polarization beam splitter prism, the length of the bottom surface is 14-16 mm, the width is 0.5-1 mm, and the distance between the bottom surfaces is 0.5-1 mm.

[0042] In some embodiments, in the second polarization beam splitter prism, the bottom surface of the third base layer is an equilateral right triangle, and the third beam splitting film is formed on the side surface connecting the hypotenuse of the bottom surface.

[0043] In some embodiments, the length of the right angle side of the equilateral right triangle is 0.5-1 mm, and the distance between the bottom surfaces is 14-16 mm.

[0044] The third aspect of the present invention relates to a method for preparing the above-mentioned polarization beam splitter prism, comprising: alternately coating the Ta2O5 layer and the SiO2 layer on the surface of the first base layer to form the first beam splitter film to obtain the polarization beam splitter prism.

[0045] The method has high production efficiency, and the prepared polarization splitting prism has good polarization splitting effect.

[0046] In some embodiments, the method for forming the first spectroscopic film is electron beam evaporation and RF ion source assisted deposition. The RF ion source and heating method are used for coating to ensure the stability of the spectrum and the firmness of the film layer. The specific deposition process is a well-known technology, and the coating quality and film thickness can be adjusted by coating temperature, atmosphere, pressure, evaporation rate, etc.

[0047] In some implementations, before forming the first prismatic film, the first base layer is further cleaned and polished.

[0048] It can be understood that the above-mentioned method for preparing the polarization beam splitter prism can be used to prepare the polarization beam splitter prism of the above-mentioned embodiment. Therefore, for the specific structure of the prepared polarization beam splitter prism, refer to the above-mentioned embodiment of the polarization beam splitter prism.

[0049] A fourth aspect of the present invention relates to a method for preparing a polarization beam splitter, comprising the steps of:

[0050] Ta2O5 layers and SiO2 layers are alternately plated on the surface of the fifth base layer to obtain a coated base layer; multiple coated base layers are glued together in sequence, wherein the coated surface of one of the coated base layers is glued to the other surface opposite to the coated surface of an adjacent coated base layer to obtain a plywood; the plywood is cut to obtain a plurality of the polarization splitter plates; wherein the material of the fifth base layer is H-Lak7 optical glass, and the coating structure of the coated base layer from the fifth base layer side is the same as the film layer structure of the first splitter film defined above from the first base layer side.

[0051] It can be understood that in the preparation method of the above-mentioned polarization splitter plate, the fifth base layer corresponds to the first base layer of the above-mentioned polarization splitter prism, and the different positions of the fifth base layer in the plywood also correspond to the positions of the second base layer, the third base layer and the fourth base layer in the implementation method of the above-mentioned polarization splitter plate, and the only difference is the size. Therefore, the polarization splitter plate comprising the second base layer, the third base layer and the fourth base layer can be obtained by further cutting.

[0052] The method has high production efficiency, and the prepared polarization beam splitter plate has good polarization beam splitting effect.

[0053] In addition, the following method can be used to prepare a polarization beam splitter plate: after coating the surface of the fifth base layer, a polarization beam splitter prism of a target size is first made (which can be cut, polished, etc.), and multiple polarization beam splitters are glued together to obtain a polarization beam splitter plate, that is, this method is to first cut to obtain a small-sized prism, and then glue. Compared with this method, gluing into a large plate and then cutting can obtain multiple polarization beam splitters with fewer gluing times, thereby improving processing efficiency.

[0054] In some embodiments, the cleavage is multi-stage cleavage.

[0055] H-Lak7 material has good processability and is suitable for plane processing. Large-size base layers can be used and multi-pole cutting can be used to obtain the target size, further improving processing efficiency. For example, for two-stage cutting, if n intermediate plates are formed by the first stage cutting and each intermediate plate is thinned into m by the second stage cutting, n×m polarization beam splitters can be obtained.

[0056] In some embodiments, the method of depositing the Ta2O5 layer and the SiO2 layer is electron beam evaporation and RF ion source assisted deposition, refer to the method for forming the first beam splitting film mentioned above.

[0057] In some embodiments, the cutting is performed using an inner circle cutting machine and / or an outer circle cutting machine. If multi-stage cutting is performed, the outer circle cutting machine can be used for the final stage cutting, and the inner circle cutting machine can be used for other stage cutting.

[0058] In some embodiments, before plating the Ta2O5 layer and the SiO2 layer, the fifth base layer is further cleaned and polished.

[0059] In some embodiments, the method for preparing the polarization beam splitter further comprises: polishing and cleaning after the cutting.

[0060] In some embodiments, the gluing is performed in sections, that is, firstly gluing a part of the coated base layer into a sub-component, and then gluing all the sub-components into a whole. The gluing generally adopts an ultraviolet (UV) curing adhesive. The section gluing reduces the thickness of the laminated layer cured in the previous section, facilitates light penetration, and can improve the overall curing efficiency.

[0061] In some embodiments, the gluing is equally divided into three sections. For example, when a total of 18 coating base layers need to be glued, they are divided into three sections, and 6 layers in each section are glued separately into sub-blocks, and then the three sub-blocks are glued.

[0062] In some embodiments, the gluing is performed according to the thickness deviation of the coating base layer, using positive and negative deviations to offset part of the tolerance and reduce the cumulative dimensional error. Considering reasonable errors, the thickness deviation of the coating base layer can be positive or negative. When selecting the coating base layer for combined gluing, the positive and negative deviations of all the coating base layers are offset as much as possible, effectively reducing the dimensional error of the finished product.

[0063] In some embodiments, the bonding is performed using UV-curable optical adhesives. Optical adhesives are suitable for optical or optoelectronic products, and have the characteristics of high transparency, stable refractive index, high purity, good durability, and little effect on optical properties. UV-curable optical adhesives have fast curing rates and high production efficiency.

[0064] In some embodiments, the polarization splitter has an incident surface and an exit surface, and the method for preparing the polarization splitter further includes: forming a first anti-reflection film on the incident surface, attaching a 1 / 2 wavelength plate to a partial area of ​​the exit surface, and forming a second anti-reflection film on the side surface where the 1 / 2 wavelength plate is located.

[0065] In some embodiments, the first anti-reflection film and / or the second anti-reflection film are formed by electron beam evaporation and RF ion source assisted deposition.

[0066] It can be understood that the above-mentioned method for preparing the polarization beam splitter can be used to prepare the polarization beam splitter of the above-mentioned embodiment. Therefore, for the specific structure of the polarization beam splitter, refer to the above-mentioned embodiment of the polarization beam splitter. According to the structure of the polarization beam splitter, it is easy to select suitable materials for gluing and obtain the target product by cutting.

[0067] A fifth aspect of the present invention relates to a projector, comprising the above-mentioned polarization beam splitter prism or the above-mentioned polarization beam splitter plate.

[0068] In some embodiments, the projector comprises an LCOS (Liquid Crystal on Silicon) projector, or an LCD (Liquid Crystal) projector.

[0069] A sixth aspect of the present invention relates to a head-up display, comprising the above-mentioned polarization beam splitting prism or the above-mentioned polarization beam splitting plate.

[0070] In some embodiments, the heads-up display comprises a vehicle-mounted heads-up display.

[0071] A seventh aspect of the present invention relates to the use of the polarization beam splitter prism or the polarization beam splitter plate in a projector or a head-up display.

[0072] In this document, reference to numerical ranges includes the end values ​​and any subset ranges within the range. "Multiple" means two or more, and "above" includes the number itself, for example, more than two includes two.

[0073] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention.

[0074] Instruction Manual

[0075] Figure 1 FIG. 1 is a schematic top view of the polarization beam splitter of Example 1 along the incident surface.

[0076] Figure 2 It is a side view of the polarization beam splitter of Example 1.

[0077] Figure 3 This is the spectrum curve of the polarization beam splitter of Example 1.

[0078] Figure 4 This is the spectrum curve of the polarization beam splitter of comparative example 1.

[0079] Reference numerals:

[0080] A first polarization beam splitter prism 110; a second beam splitter film 111; a second polarization beam splitter prism 120; a third beam splitter film 121;

[0081] A third polarization beam splitter prism 130 ; a half-wavelength plate 140 ; ​​a first anti-reflection film 150 ; and a second anti-reflection film 160 . DETAILED DESCRIPTION

[0082] Embodiments of the present invention are described in detail below. The embodiments are exemplary and are only used to explain the present invention, but are not to be construed as limiting the present invention.

[0083] In the following examples and comparative examples, the relevant raw materials are described as follows:

[0084] Glue: UT20, a UV curing optical adhesive, was purchased from Sekisui Fuleku Kaisha, Japan.

[0085] M2 membrane: The coating material is Merck M2 coating material.

[0086] The coating process of the second and third beam splitting films is electron beam evaporation and RF ion source assisted deposition. The process parameters are as follows: the working temperature is 200 °C, the working gas is oxygen, the gas flow rate is 65 sccm; the starting pressure is 8.0×10 -4 Pa; the Ta2O5 material and SiO2 material are melted by the heat energy of the electron beam, and the two materials are evaporated alternately, the Ta2O5 evaporation rate is 0.25nm / second; the SiO2 evaporation rate is 0.8nm / second.

[0087] The coating process of the first antireflection film and the second antireflection film is electron beam evaporation and RF ion source assisted deposition. The process parameters are as follows: the working temperature is 60 ° C, the working gas is oxygen, the gas flow rate is 85 sccm; the starting pressure is 8.0×10 -4 Pa; the thermal energy of the electron beam is used to melt the Ta2O5 material and the SiO2 material, and the two materials are evaporated alternately, the evaporation rate of Ta2O5 is 0.25nm / second; the evaporation rate of SiO2 is 0.8nm / second. The deposition thicknesses are: 11.3nm, 42.31nm, 45.36nm, 8.41nm, 69.75nm, 87.72nm.

[0088] 1 / 2 wavelength plate: thickness 0.156 mm, model WA-280T, resin material, purchased from Nippon Kayaku.

[0089] Unless otherwise specified, the raw materials or equipment involved are conventional raw materials or equipment that can be purchased commercially.

[0090] Example 1

[0091] This embodiment prepares a polarizing beam splitter, the structure of which is as follows Figure 1-2 As shown. The polarized beam splitter plate of this embodiment includes 16 first polarized beam splitter prisms 110 glued in sequence. The first polarized beam splitter prism has a second base layer made of H-Lak7 material and a quadrangular prism structure. The upper and lower bottom surfaces of the second base layer are rectangular (length 15.3±0.15mm, width 0.92±0.02mm), and the distance between the bottom surfaces is 0.92±0.02mm. A set of side surfaces connecting the long sides of the bottom surface is a rectangle, and another set of side surfaces connecting the short sides of the bottom surface is a parallelogram with an acute angle of 45°.

[0092] A second prismatic film 111 is deposited on a rectangular side of the second base layer. The second prismatic film 111 includes 23 layers of Ta2O5 layers and SiO2 layers alternately stacked in sequence from the second base layer side. The film thickness from the second base layer side is as shown in Table 1, wherein the thickness error of the Ta2O5 layer is controlled within ±1nm, and the thickness error of the SiO2 layer is controlled within ±2nm:

[0093] Table 1: Structure of the spectroscopic film of Example 1

[0094]

[0095]

[0096] The second beam splitter film 111 of one first polarization beam splitter prism 110 is glued to another rectangular side surface opposite to the second beam splitter film 111 of another first polarization beam splitter prism 110, so that the bottom surface on the same side and the parallelogram side surface on the same side of the second base layer are located in the same plane, forming a glued quadrangular prism.

[0097] The second polarization beam splitter prism 120 has a third base layer of H-Lak7 material and a straight triangular prism structure. The two bottom surfaces of the third base layer are equilateral right triangles, the length of the right angle side is 0.92±0.02mm, and the distance between the bottom surfaces is 15.3±0.15mm. A third beam splitter film 121 is provided on the side surface of the hypotenuse connecting the two bottom surfaces. The film layer structure and film thickness of the third beam splitter film 121 from the third base layer side are the same as the second beam splitter film 111 (Table 1). The third beam splitter film 121 is glued to the outermost rectangular side of the glued quadrangular prism without the second beam splitter film 111.

[0098] The third polarization beam splitter prism 130 has a fourth base layer of H-Lak7 material and a straight triangular prism structure. The two bottom surfaces of the fourth base layer are equilateral right triangles, the length of the right angle side is 0.92±0.02mm, and the distance between the bottom surfaces is 15.3±0.15mm. The side surface of the hypotenuse connecting the two bottom surfaces is glued to the outermost second beam splitter film 111 of the glued quadrangular prism. The glued quadrangular prism, the second polarization beam splitter prism 120 and the third polarization beam splitter prism 130 are glued to form a rectangular parallelepiped structure.

[0099] Through the design of substrate and splitter film, the film thickness is greatly reduced. The total thickness of the splitter film on one side is about 2500nm, which is significantly lower than the film system (about 9000nm) adapted to the conventional B270 or BK7 substrate. The film layer is thin, the substrate is not easy to deform, and it is easier to glue, reducing appearance defects such as bubbles and splashes. More importantly, better optical performance is obtained, the applicable band is 425nm-650nm, and the air incidence angle is 0±8°, which is better than the conventional technical indicators in the industry: 450-650nm, air incidence 0°±5°. The characteristics of all dichroic films meet the following requirements: AOI = 0°, λ = 425nm-650nm, Ts,ave ≤ 0.1%, Tp,ave ≥ 97%; AOI = 0° ± 8°, λ = 430nm-650nm, Ts,ave ≤ 2%, Tp,ave ≥ 94%; AOI represents the air incident angle, λ represents the incident wavelength, Ts,ave represents the average transmittance of S light, and Tp,ave represents the average transmittance of P light.

[0100] Average transmittance test method: Use a spectrophotometer (model PHOTON RT, manufacturer Essent Optics), set the test mode of the spectrophotometer to transmittance T%, select P light and S light, set the wavelength range to 380-780nm, the transmittance range to 0-100%, and perform instrument baseline calibration; after the calibration is completed, insert the polarization beam splitter, the polarization beam splitter and the light receiver are in a vertical state, and select to start the test; after the test is completed, export the test data.

[0101] H-LaK7 material has good processability and a hardness FA value of 76, which is more suitable for plane processing. H-LaK7 has high UV transmittance and is suitable for light-curing bonding process. At the same time, the thin film layer of the splitter film is more conducive to UV light transmission, achieving rapid light curing and improving processing efficiency. In terms of cost, because the film layer of the splitter film is thinner, it offsets the cost pressure of H-Lak7 and basically does not increase the overall cost. At the same time, the performance is better and it has a higher cost performance.

[0102] In one embodiment, a 1 / 2 wavelength plate 140 (as an exit surface, and the other side is an incident surface) is covered on the bottom surface on the same side of any of the outermost first, third, fifth, seventh, ninth, eleventh, thirteenth, and fifteenth first polarization beam splitting prisms 110 to delay the phase of the passing polarized light by half a wavelength to adjust the polarization direction of the light to better adapt to the working angle. The material of the 1 / 2 wavelength plate 140 can be quartz crystal, and the fixing method can be gluing. The characteristics of the 1 / 2 wavelength plate meet the following requirements: AOI = 0° ± 10°, reflectivity Rave ≤ 0.5% @ 425nm-650nm, delay: λ / 2 @ 425nm-650nm, delay error: λ / 500.

[0103] A first anti-reflection film 150 is deposited on the incident side of the polarization beam splitter, and a second anti-reflection film 160 is deposited on the exit side of the polarization beam splitter. The first anti-reflection film 150 and the second anti-reflection film 160 are used to reduce light reflection and improve light transmittance. The material, thickness of each layer and deposition process are as described above. All anti-reflection film characteristics meet the following requirements: AOI = 0° ± 8°, λ = 425nm-650nmm, Rave ≤ 0.5%.

[0104] Example 2

[0105] This embodiment provides a method for preparing the polarization beam splitter of embodiment 1, comprising the steps of:

[0106] S1. Provide a rectangular fifth base layer.

[0107] S2. After the fifth base layer is cleaned and polished, the Ta2O5 layer and SiO2 layer in Table 1 are alternately plated on one side of the surface to obtain a coated substrate. The coating method is electron beam evaporation and RF ion source assisted deposition, and the process is as described above. In terms of operation, the cleaned baffle, bottom plate, cover plate, etc. will be replaced before each furnace plating to facilitate the control of the coating appearance.

[0108] S3. Use glue to bond the coated substrates in sequence. The coated surface or the opposite side of the coated substrate is the bonding surface. All coated surfaces are oriented in the same direction so that the bonding interface contains only one layer of coating. A total of 6 layers of coated substrates are bonded in a single bonding to obtain a sub-block. During bonding, the thickness deviation of the coating base layer is detected, and positive and negative deviations are used for bonding to offset the overall deviation as much as possible (for example, in a 6-layer board, 3 sheets with a thickness tolerance of -0.01mm and 3 sheets with a thickness tolerance of +0.01mm are combined, and one positive and one negative are selected for bonding to offset the cumulative error). During bonding, constant pressure control is performed to improve the consistency of bonding thickness.

[0109] S4, perform the first UV curing on the sub-block of step S3, and then glue the three sub-blocks according to the same rule (the coating surface or the opposite side is the bonding surface, all the coating surfaces are oriented in the same direction, so that the bonding interface contains only one coating layer), perform UV curing, and obtain an 18-layer plywood.

[0110] S5. Cut the plywood of step S4 (the cutting direction is not parallel to the bonding interface direction, for example, perpendicular or intersecting, to ensure that the total number of layers is still 18 layers, corresponding to the second base layer, the third base layer and the fourth base layer) to obtain a plurality of polarizing beam splitters with the structure shown in Example 1.

[0111] Specifically, in order to prepare the polarized beam splitter of Example 1, the size of the plywood is controlled to be appropriately larger than the polarized beam splitter (this can be achieved by adjusting the size of the fifth substrate and / or the stacking direction) so that multiple polarized beam splitters of the same structure can be obtained by cutting. When stacking is required at a certain angle (for example, 45°), an auxiliary reference block can be used for positioning. When cutting is required at a certain angle (for example, 45°), a 45° cutting jig can be used to fix the tool spacing, and the size can be detected after cutting to improve the stability of the cutting quality. Cutting can be performed using an inner circle cutting machine or an outer circle cutting machine. Specifically, an outer circle cutting machine can be used for final cutting, and an inner circle cutting machine can be used for other graded cutting.

[0112] H-Lak7 material has good processability and is suitable for plane processing. It can be glued with large-sized substrates and then cut and subdivided into target sizes to improve processing efficiency. After cutting, it can be cleaned and polished to reduce surface contaminants and defects.

[0113] In one embodiment, the steps are further included:

[0114] S6: With one bottom surface of the polarization beam splitter as the incident surface and the other bottom surface as the exit surface, Ta2O5 film and SiO2 film of corresponding thickness are alternately plated on one side of the incident surface of the polarization beam splitter, which is the same as the first anti-reflection film 150 in Example 1.

[0115] S7: Using glue to bond a plurality of half-wavelength plates 140 to one side of the output surface of the polarization beam splitter;

[0116] S8: Alternately deposit Ta2O5 films and SiO2 films of corresponding thicknesses on one side of the output surface of the polarization beam splitter, similar to the second anti-reflection film 160 in Example 1.

[0117] It can be understood that in steps S6 to S8 , the number and position of the half-wavelength plates 140 , and the positions of the first anti-reflection film 150 and the second anti-reflection film 160 are determined with reference to Example 1.

[0118] Comparative Example 1

[0119] The structure of the existing polarization beam splitter is similar to that of Example 1, except that the second base layer, the third base layer, and the fourth base layer are made of B270 glass, the film structure and thickness of the second beam splitter film from the second base layer side, and the film structure and thickness of the third beam splitter film from the third base layer side are shown in Table 2 (wherein the thickness error of the M2 layer is controlled within ±1 nm, and the thickness error of the SiO2 layer is controlled within ±2 nm), the coating process is electron beam evaporation and RF ion source assisted deposition, and the process parameters are as follows: the working temperature is 250°C, the working gas is oxygen, and the gas flow rate is 85 sccm; the starting pressure is 8.0×10 -4Pa; the coating material is melted by the heat energy of the electron beam, causing the two materials to evaporate alternately, with an M2 evaporation rate of 0.3nm / sec; and an SiO2 evaporation rate of 0.8nm / sec.

[0120] Table 2: Structure of the spectroscopic film of Comparative Example 1

[0121]

[0122]

[0123] The parameters of the beam splitter film of comparative example 1 are as follows: AOl = 0°, λ = 425nm-650nm, Ts,ave ≤ 2%, Tp,ave ≥ 96%; AOl = 0° ± 8°, λ = 430nm-650nm, Ts,ave ≤ 3%, Tp,ave ≥ 94%. The spectral curves of the polarization beam splitter plates of embodiment 1 and comparative example 1 are shown in FIG. Figure 3 and Figure 4 .

[0124] It can be seen that the polarization separation effect of the spectroscopic film of comparative example 1 is obviously inferior to that of embodiment 1, and the coating design curve fluctuates greatly, resulting in the theoretical design values ​​of the P light and S light transmittance of 0°±5° failing to meet the requirements. However, the spectroscopic film of embodiment 1 has high ultraviolet light transmittance, a smoother coating design curve, and the theoretical design values ​​of the P light and S light of 0°±5° can meet the requirements, and the applicable band is wider.

[0125] In addition, the embodiment 1 has a thin spectroscopic film (about 2500nm), good finish, easy gluing, and reduced appearance risk. The spectroscopic film of comparative example 1 is about 9000nm thick, with a thick film layer and high stress, which easily generates bubbles during gluing and easily produces pitting on the appearance. The B270 material is easy to deliquesce and is prone to the risk of debonding. It is inferior to the embodiment 1 in terms of optical performance, appearance, and use strength.

[0126] In view of the performance advantages of the polarization beam splitter of this embodiment, it can better meet the use requirements of optoelectronic products such as projectors or head-up displays, and can be applied to products such as LCOS projectors, LCD projectors or vehicle-mounted head-up displays.

[0127] The present invention has been described in detail above in conjunction with the embodiments, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A polarization beam splitter prism, It is characterized in that include: The first base layer is made of H-Lak7 optical glass; A first spectral film is formed on at least one side of the first substrate, wherein the film layer structure of the first spectral film is as follows: Ta is alternately stacked in sequence from the first substrate side; 2 O 5 Layer and SiO 2 There are 23 layers in total, and the thicknesses are 26.65-28.65nm, 283.08-287.08nm, 109.67-111.67nm, 218.28-222.28nm, 91.28-93.28nm, 177.06-181.06nm, 84.37-86.37nm, 204.95-208.95nm, 66.32-68.32nm, 127.51-131.51nm, 52.63-54 .63nm, 226.66~230.66nm, 68.04~70.04nm, 107.92~111.92nm, 50.9~52.9nm, 106.58~110.58nm, 55.85~57.8 5nm, 101.03~105.03nm, 50.27~52.27nm, 85.08~89.08nm, 52.44~54.44nm, 94.43~98.43nm, 33.18~35.18nm.

2. The polarization beam splitter according to claim 1, It is characterized in that The first base layer has a triangular prism or quadrangular prism structure; and / or the film layer structure of the first prismatic film is: starting from the first base layer side, it includes Ta 2 O 5 Layer and SiO 2 There are 23 layers in total, and the layer thicknesses are 27.65nm, 285.08nm, 110.67nm, 220.28nm, 92.28nm, 179.06nm, 85.37nm, 206.95nm, 67.32nm, 129.51nm, 53.63nm, 228.66nm, 69.04nm, 109.92nm, 51.9nm, 108.58nm, 56.85nm, 103.03nm, 51.27nm, 87.08nm, 53.44nm, 96.43nm, and 34.18nm from the first base layer side.

3. A polarization beam splitter, It is characterized in that Comprising the polarization beam splitter prism as claimed in claim 1 or 2.

4. The polarization beam splitter according to claim 3, It is characterized in that The polarization beam splitter comprises: A glued quadrangular prism, comprising a plurality of first polarization beam splitting prisms glued in sequence, wherein the first polarization beam splitting prism has a second base layer, the second base layer has a quadrangular prism structure, a second beam splitting film is formed on one side surface of the second base layer, the second beam splitting film of one of the first polarization beam splitting prisms is glued to the other side surface opposite to the second beam splitting film of the adjacent first polarization beam splitting prism, and the bottom surface on the same side of the second base layer and another group of side surfaces connected to the bottom surface are respectively located in the same plane; A second polarizing beam splitter prism, comprising a third base layer of a right triangular prism, a third beam splitter film being formed on one side of the third base layer, and the third beam splitter film being glued to a surface of the outermost side of the glued quadrangular prism opposite to the second beam splitter film; A third polarization beam splitter prism, comprising a fourth base layer of a right triangular prism, wherein one side surface of the fourth base layer is glued to the outermost second beam splitter film of the glued quadrangular prism; The materials of the second base layer, the third base layer and the fourth base layer are all H-Lak7 optical glass, and the film layer structure of the second prismatic film from the second base layer side and the film layer structure of the third prismatic film from the third base layer side are the same as the film layer structure of the first prismatic film from the first base layer side defined in claim 1; The glued quadrangular prism, the second polarization beam splitting prism and the third polarization beam splitting prism are glued together to form a rectangular parallelepiped structure.

5. The polarization beam splitter according to claim 4, It is characterized in that The number of the first polarization beam splitting prisms is 16; And / or, in the first polarization beam splitter prism, the bottom surface of the second base layer is a rectangle, a group of side surfaces connecting the long sides of the bottom surface are rectangles, the second beam splitter film is formed on one of the rectangular side surfaces, and a group of side surfaces connecting the short sides of the bottom surface are parallelograms with an acute angle of 45°; And / or, in the first polarization beam splitter prism, the length of the bottom surface is 14-16 mm, the width is 0.5-1 mm, and the distance between the bottom surfaces is 0.5-1 mm; And / or, in the second polarization splitter prism, the bottom surface of the third base layer is an equilateral right triangle, and the third splitter film is formed on the side surface connecting the hypotenuse of the bottom surface. Optionally, the right angle side length of the equilateral right triangle is 0.5 to 1 mm, and the distance between the bottom surfaces is 14 to 16 mm.

6. The polarization beam splitter according to claim 4, It is characterized in that The polarization beam splitter plate also includes 8 1 / 2 wavelength plates, one side bottom surface of the second base layer is the incident surface, and the other side bottom surface is the exit surface, the 8 1 / 2 wavelength plates are respectively located on one side of the exit surface of the 8 first polarization beam splitter prisms in the glued quadrangular prism, and a first polarization beam splitter prism is spaced between two adjacent 1 / 2 wavelength plates.

7. The polarization beam splitter according to claim 6, It is characterized in that A first anti-reflection film is disposed on one side of the incident surface of the polarization beam splitter, and a second anti-reflection film is disposed on a surface of the polarization beam splitter opposite to the incident surface; Optionally, the thickness of the first anti-reflection film and the second anti-reflection film are independently 250-300 nm.

8. A method for preparing a polarization beam splitter. It is characterized in that Includes steps: Ta is alternately plated on the surface of the fifth base layer 2 O 5 Layer and SiO 2 layer to obtain a coating base layer; gluing a plurality of coated base layers in sequence, wherein the coated surface of one of the coated base layers is glued to the other surface opposite to the coated surface of an adjacent coated base layer, to obtain a plywood; and cutting the plywood to obtain a plurality of the polarization beam splitters; The material of the fifth base layer is H-Lak7 optical glass, and the coating structure of the coating base layer starting from the fifth base layer side is the same as the film layer structure of the first beam splitting film defined in claim 1 starting from the first base layer side.

9. The method for preparing the polarization beam splitter according to claim 8, It is characterized in that The polarization beam splitter has an incident surface and an exit surface, and the method for preparing the polarization beam splitter further includes: forming a first anti-reflection film on the incident surface, attaching a 1 / 2 wavelength plate to a part of the exit surface, and forming a second anti-reflection film on a side surface where the 1 / 2 wavelength plate is located; And / or, the cutting is multi-stage cutting; And / or, the Ta plating 2 O 5 Layer and SiO 2 The layer methods are electron beam evaporation and RF ion source assisted deposition; And / or, the gluing is segmented gluing.