High-temperature alloy performance regulation and control method based on high-temperature oxidation

Through high-temperature oxidation orthogonal test and database construction, the problem of difficult coordination between infrared radiation performance and body performance after oxidation of high-temperature alloy is solved, and controllable regulation of high-temperature alloy performance is achieved, ensuring that the performance of oxidized parts meets the design requirements.

CN118916989APending Publication Date: 2024-11-08BEIJING HANGXING MACHINERY MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410971222.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

After high-temperature oxidation treatment, the infrared radiation performance and the body performance are difficult to coordinately control, resulting in differences in performance before and after oxidation, affecting its service performance.

Method used

The performance characterization element is designed using high-temperature oxidation orthogonal tests, and the corresponding relationship between infrared radiation performance and body performance is obtained through high-temperature oxidation experiments, a regular database is constructed, and calibration compensation is performed through intermediate parameters or repeated experiments, and appropriate high-temperature oxidation parameters are selected to achieve Performance regulation.

Benefits of technology

The coordinated control of infrared radiation performance and body performance of high-temperature alloys is achieved, and controllable regulation means are provided to ensure that the oxidized parts meet both infrared radiation performance and body performance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118916989A_ABST
    Figure CN118916989A_ABST
Patent Text Reader

Abstract

The invention discloses a high-temperature alloy performance regulation and control method based on high-temperature oxidation, and belongs to the technical field of high-temperature alloy thermal surface treatment. The method is used for solving the problems that the body performance and the infrared radiation performance of the existing high-temperature alloy before and after oxidation are different and are difficult to coordinate and control. According to the high-temperature alloy performance regulation and control method based on high-temperature oxidation, through a high-temperature oxidation orthogonal test, the corresponding relation of high-temperature oxidation parameters, infrared radiation performance and ontology performance is obtained, and construction of a rule database is completed; checking and compensating the database by using intermediate parameters or repeated experiments, continuously perfecting the database and improving the accuracy of the database; and high-temperature oxidation parameter selection is performed by combining a database with specific part design requirements, so that coordination control between the body performance and the infrared radiation performance is realized. According to the method, parameters are controllable, and a new regulation and control thought is provided for high-temperature alloy performance regulation and control based on high-temperature oxidation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of high-temperature alloy thermal surface treatment, and in particular relates to a high-temperature alloy performance control method based on high-temperature oxidation. Background Art

[0002] Superalloys, a type of metal alloy, have become the preferred material for aerospace applications due to their stable structure, excellent thermal strength, hot and cold forming, and weldability. They play a crucial role in the development of the modern aviation industry. Currently, aircraft are continuously developing towards high Mach numbers and long flight times. During high-speed reentry, aircraft encounter severe aerodynamic heating. To ensure personnel safety and equipment operation, lightweight, high-temperature resistant thermal insulation materials with varying temperature resistance levels must be applied to the aircraft surface to meet the thermal insulation requirements of different parts of the aircraft. Reusable thermal protection systems consist of a surface coating with high infrared radiation performance and an internal low thermal conductivity insulation material. The internal low thermal conductivity insulation material prevents heat transfer into the aircraft interior, while the surface coating with high infrared radiation performance dissipates heat to the external environment through radiation. Aircraft components made of superalloys are often used in relatively high ambient temperatures. Therefore, the infrared radiation performance of the surface of the superalloy components is crucial for their high-temperature serviceability.

[0003] Currently, composite coatings with high infrared radiation performance, made from metal oxides or minerals, are widely used as new heat-resistant materials on metal alloy surfaces to improve infrared radiation performance. However, the complex and expensive preparation process and the complicated spraying process hinder their widespread application. Summary of the Invention

[0004] In view of the above analysis, the present invention is based on the use of a high-temperature oxidation process to generate an oxide film on the surface of a high-temperature alloy to improve the infrared radiation performance, and provides a high-temperature alloy performance regulation method based on high-temperature oxidation, which is used to solve the problem that there are differences in the bulk performance and infrared radiation performance of the high-temperature alloy before and after oxidation, and the two properties are difficult to coordinate and control.

[0005] The purpose of the present invention is mainly achieved through the following technical solutions:

[0006] The present invention proposes a method for controlling the properties of a high-temperature alloy based on high-temperature oxidation, comprising the following steps:

[0007] S1. Design a high-temperature oxidation orthogonal test, design and process performance characterization parts, and use the performance characterization parts to complete the high-temperature oxidation experiment and conduct performance tests;

[0008] S2. Organize the performance results, obtain the corresponding relationship between high-temperature oxidation parameters, infrared radiation performance, and bulk performance, and complete the construction of the regularity database;

[0009] S3. Use intermediate parameters or repeated experiments to calibrate and compensate the database;

[0010] S4. Use the database to combine the intrinsic properties of high-temperature alloy products with the infrared radiation performance requirements to select parameters for high-temperature oxidation.

[0011] Furthermore, in S1, the processing of the performance characterization part is carried out according to the processing procedures of the parts, including additive manufacturing, solution heat treatment, machining, and welding procedures.

[0012] Furthermore, in S1, the performance characterizing part needs to be designed and processed according to the technical conditions of the part and the performance of interest to obtain the performance characterizing part.

[0013] Furthermore, in S1, the performance test includes a body performance test and an infrared radiation performance test.

[0014] Furthermore, the body properties include body mechanical properties, weld mechanical properties, and weld quality; the body mechanical properties include tensile strength, yield strength, elongation after fracture, and hardness.

[0015] Furthermore, the infrared radiation performance includes infrared emissivity, oxide layer thickness, oxide layer morphology, oxidation phase analysis, and weight gain after oxidation.

[0016] Furthermore, in S2, the high-temperature oxidation parameters include heating temperature and holding time.

[0017] Furthermore, in S3, repeated experiments are performed to correct possible abnormal result data points, and the performance results are compensated using intermediate parameters in the database.

[0018] Furthermore, in S4, based on the design requirements of the high-temperature alloy product's bulk performance and infrared radiation performance, target infrared radiation performance indicators and bulk performance indicators are proposed, and then high-temperature oxidation parameters or parameter segments that can meet the two performance indicators are selected through the database. The parts are subjected to a high-temperature oxidation process using the parameters or parameter segments to obtain finished parts.

[0019] Furthermore, the finished parts meet the requirements of infrared radiation performance and body performance at the same time.

[0020] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0021] 1) This invention improves infrared radiation performance by using an oxide film formed on the surface of a high-temperature alloy through a high-temperature oxidation process, providing a new approach to regulating the performance of high-temperature alloys through high-temperature oxidation. Through orthogonal high-temperature oxidation experiments, the present invention establishes a correlation between high-temperature oxidation parameters, infrared radiation performance, and bulk performance, and constructs a regularity database. The database is calibrated and compensated using intermediate parameters or repeated experiments, continuously improving the database and its accuracy. The database is then combined with specific part design requirements to select high-temperature oxidation parameters, achieving coordinated control between bulk performance and infrared radiation performance. This method, with controllable parameters, provides a new approach to regulating the performance of high-temperature alloys through high-temperature oxidation.

[0022] 2) This invention provides a controllable means for utilizing the high-temperature alloy's inherent oxide film to enhance its inherent infrared radiation performance. After high-temperature oxidation processing in a high-temperature, oxygen-containing environment, the oxide film formed on the surface of the high-temperature alloy itself serves as an excellent interface for enhancing its inherent infrared radiation performance. However, research has found that after a certain period of high-temperature oxidation, the high-temperature alloy's bulk performance and infrared radiation performance inevitably differ compared to those before oxidation. If the alloy meets the bulk performance requirements before high-temperature oxidation, and a high-temperature oxidation experiment is conducted to enhance infrared radiation performance, while the inherent infrared radiation performance is improved after the experiment, the bulk performance also changes after high-temperature oxidation, and the alloy then fails to meet the bulk performance requirements, an undesirable situation. The present invention achieves control between bulk and infrared radiation performance. Through control, a high-temperature alloy can be prepared that meets both infrared radiation and bulk performance requirements after high-temperature oxidation, providing a controllable means for utilizing the high-temperature alloy's inherent oxide film to enhance its inherent infrared radiation performance.

[0023] Other features and advantages of the present invention will be described in the following description, and part of them will become obvious from the description, or be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the written description. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The drawings are only for purposes of illustrating particular embodiments and are not to be considered limiting of the invention.

[0025] Figure 1 The figure is a flow chart of a method for controlling the properties of high-temperature alloys based on high-temperature oxidation;

[0026] Figure 2 Schematic diagram of infrared radiation performance characterization of GH4099 high-temperature alloy parts;

[0027] Figure 3 Schematic diagram of the performance representation of the GH4099 high-temperature alloy part;

[0028] Figure 4 GH3128 high-temperature alloy shaft parts and specific surface diagram;

[0029] Figure 5 Relationship curve between oxide layer thickness of GH4099 high temperature alloy and infrared emissivity at various temperatures;

[0030] Figure 6 This is an SEM image of a high-temperature alloy with an oxide film on the surface prepared in Example 1;

[0031] Figure 7 This is the XRD pattern of the high-temperature alloy with an oxide film on the surface prepared in Example 1.

[0032] Reference numerals

[0033] 1-Infrared emissivity test piece; 2-Oxide layer thickness test piece; 3-Welding test piece; 4-Mechanical tensile test bar; 5-Hardness characterization test piece; 6-Specific surface. DETAILED DESCRIPTION

[0034] The preferred embodiments of the present invention are described in detail below. The embodiments are only used to illustrate the principles of the present invention and are not used to limit the scope of the present invention.

[0035] Currently, composite coatings with high infrared radiation performance, made from metal oxides or minerals, are widely used as new heat-resistant materials on metal alloy surfaces to improve infrared radiation performance. However, the complex and expensive preparation process and the complicated spraying process hinder their widespread application.

[0036] Based on this, the present invention proposes to use a high-temperature oxidation process to generate an oxide film on the surface of a high-temperature alloy to improve infrared radiation performance. After the high-temperature alloy is subjected to high-temperature oxidation in a certain high-temperature oxygen-containing environment, the oxide film on its surface itself is an excellent interface that improves its own infrared radiation performance.

[0037] However, research has found that after a certain period of high-temperature oxidation, the bulk properties and infrared radiation properties of high-temperature alloys will change. For general high-temperature alloy parts, while paying attention to the surface infrared radiation performance, the bulk performance is also the key to its service life. For high-temperature alloys that meet the bulk performance requirements, after high-temperature oxidation treatment to improve infrared radiation performance, although the infrared radiation performance itself is improved, the bulk performance also changes. At this time, the bulk performance of the high-temperature alloy cannot meet the requirements, which is an undesirable situation. The technical difficulty of the present invention to improve the infrared radiation performance by using the oxide oxide film generated on the surface of the high-temperature alloy through the high-temperature oxidation process is how to achieve comprehensive control of the bulk performance and infrared radiation performance of the high-temperature alloy.

[0038] Therefore, the present invention proposes a high-temperature alloy performance control method based on high-temperature oxidation, the main process and process principles are as follows Figure 1 As shown, it includes the following steps:

[0039] S1. Design a high-temperature oxidation orthogonal test, design and process performance characterization parts, use the performance characterization parts to complete the high-temperature oxidation experiment and conduct corresponding performance tests;

[0040] S2. Organize the performance results, obtain the corresponding relationship between high-temperature oxidation parameters, infrared radiation performance, and bulk performance, and complete the construction of the regularity database;

[0041] S3. Use intermediate parameters or repeated experiments to calibrate and compensate the database, continuously improving the database and increasing its accuracy;

[0042] S4. Use the database to combine the intrinsic properties of high-temperature alloy products with the infrared radiation performance requirements to select parameters for high-temperature oxidation.

[0043] Compared with the existing technology, the present invention improves the infrared radiation performance based on the oxide film generated on the surface of the high-temperature alloy by a high-temperature oxidation process, providing a new control idea for the performance control of high-temperature alloys based on high-temperature oxidation; and provides a controllable control means for the process of using the high-temperature alloy's own oxide film to improve its own infrared radiation performance.

[0044] Furthermore, in S1, when designing an orthogonal experiment, a high-temperature oxidation parameter is selected: any one of the heating temperature and the holding time is a variable and the other is a quantitative high-temperature oxidation test. For example, the heating temperature is selected as a quantitative value (750°C) and the holding time is selected as a variable (2h, 4h, 6h, 8h, 10h, 12h), and a high-temperature oxidation test is performed to obtain the infrared radiation and bulk performance results at different holding times at 750°C. Alternatively, the holding time is selected as a quantitative value (2h) and the heating temperature is selected as a variable (700°C, 750°C, 800°C, 850°C, 900°C), and a high-temperature oxidation test is performed to obtain the infrared radiation and bulk performance results at different heating temperatures for 2h.

[0045] Furthermore, in S1, the corresponding performance tests include body performance and infrared radiation performance tests.

[0046] Use body performance characterization parts to conduct corresponding performance tests on parts, including body performance, infrared radiation related performance tests, etc., to obtain performance reference data.

[0047] Furthermore, the body properties include body mechanical properties, weld mechanical properties, and weld quality; the body mechanical properties include tensile strength, yield strength, elongation after fracture, and hardness.

[0048] The high-temperature oxidation process will affect the bulk properties of the alloy. In order to obtain the bulk properties under high-temperature oxidation parameters, bulk performance testing is required.

[0049] Bulk mechanical property testing can determine the basic mechanical properties of materials, such as tensile strength, yield strength, elastic modulus, hardness, etc.; it can evaluate the response of materials under different load conditions, ensure that the materials can withstand the expected stress and strain in actual applications, and provide data support for material selection and design.

[0050] Weld mechanical property evaluation can assess the mechanical properties of welded joints, including their response under tension, compression, bending and impact loads; ensure that the mechanical properties of welds meet design requirements and avoid structural failure due to welding quality problems; detect defects that may occur during the welding process, such as cracks, pores, lack of fusion, etc., and use test results to guide improvements in welding processes.

[0051] The quality of weld joints can evaluate the macro and micro structures of welds, including the shape, size and internal organization of welds, and check whether welds have defects such as cracks, inclusions, holes, etc. These defects may affect the load-bearing capacity and durability of welds.

[0052] Furthermore, the performance test of the body is closely related to the performance characterization component. The shape and size of the performance characterization component directly affect the stress distribution and deformation pattern during the test, which is crucial to the accuracy, representativeness, and reliability of the test results. The performance characterization component of the appropriate shape and size can be selected according to the specific test requirements.

[0053] Furthermore, the infrared radiation performance includes infrared emissivity, oxide layer thickness, oxide layer morphology, oxidation phase analysis, and weight gain after oxidation.

[0054] The high-temperature oxidation process will affect the infrared radiation performance of the alloy. In order to obtain the infrared radiation performance under high-temperature oxidation parameters, infrared radiation performance testing is required.

[0055] Infrared emissivity testing can test the ability of a material to emit infrared radiation under thermal radiation conditions, which helps to evaluate the material's heat dissipation, corrosion resistance, and wear resistance. The oxide layer thickness test determines whether the protective layer on the material surface meets the requirements to judge the material's corrosion resistance and wear resistance. The oxide layer morphology observation evaluates its quality and performance by observing the surface morphology of the oxide layer. The oxide layer phase analysis determines the phase composition of the oxide layer to understand its stability and reactivity under different conditions. The weight gain test before and after oxidation evaluates the protective ability of the coating or material to the substrate at high temperatures by measuring the change in mass of the sample before and after oxidation.

[0056] Furthermore, infrared radiation performance testing is closely related to performance characterization components. Objects of different shapes and sizes may have varying distributions and intensities of infrared radiation emitted from their surfaces. Infrared testing requires a rigorous testing environment. If the shape and size of the performance characterization component differ significantly from the actual product, the test results may not truly reflect the product's performance. Therefore, selecting the appropriate performance characterization component is crucial for ensuring accurate test results.

[0057] Furthermore, in S1, the performance representative parts need to be designed and processed according to the technical conditions of the parts and the performance of interest to obtain the performance representative parts.

[0058] It should be noted that infrared radiation and bulk performance testing typically requires the use of performance characterization components. These components primarily serve to provide a benchmark or reference for testing and analysis, ensuring the accuracy and reliability of measurement results. During performance testing, these components simulate the material's behavior in real applications under controlled laboratory conditions, enabling more accurate assessment of material performance, predicting its actual performance, and ensuring product quality and reliability.

[0059] Specifically, to ensure consistency and comparability of test results, the shape of the performance characterization component must be designed. This is because different test types and test methods require different shapes for the performance characterization component, and the shape design of the performance characterization component is not universal. The specific shape of the performance characterization component is designed based on the test requirements.

[0060] When conducting infrared emissivity tests, the shape of the characterizing piece is disc-shaped. The diameter of the disc is manufactured according to the requirements of the infrared test instrument and is generally 10mm to 50mm. The disc shape helps ensure the consistency and comparability of the test results. It is also highly symmetrical, with small directional errors. The surface can provide uniform infrared radiation and reception, which helps reduce the impact of local hot spots or cold spots on the test results. The diameter is easy to measure and standardize, which helps to accurately control the test parameters and improve the accuracy, repeatability and comparability of the infrared emissivity test. For example, Figure 2 The shape of the mid-infrared emissivity test piece.

[0061] When testing the oxide layer thickness and oxide layer morphology, both can be tested using SEM to characterize the shape of the part. Figure 2The shape of the medium oxide thickness test piece is a square test piece. The side length is generally about 10mm and the thickness is 1-3mm. It meets many standards and specifications for oxide thickness testing, which helps to ensure the consistency and comparability of test results. The surface is relatively uniform, which helps to obtain more consistent results in oxide thickness testing. The cutting and grinding processes are simple and easy to implement. The test piece size is easy to measure and can be precisely controlled to ensure the accuracy of the test results. It helps to improve the accuracy, repeatability and comparability of oxide thickness testing. It is a standard shape widely used in oxide thickness assessment.

[0062] When performing oxidation phase analysis, XRD phase analysis can be used, and the shape of the characterization part can be as follows Figure 2 The shape of the mid-infrared emissivity test piece is disc-shaped, or it can be Figure 2 The shape of the medium oxide layer thickness test piece is a square test piece.

[0063] When conducting the weight gain test after oxidation, the weight gain after oxidation is measured using an analytical balance to characterize the shape of the part. Figure 2 The shape of the mid-infrared emissivity test piece is disc-shaped.

[0064] When testing the weld quality, use SEM to observe the weld after welding and oxidation to see if there are cracks. If there are no cracks, it means the quality is qualified. Figure 3 Welding of representative parts of the welding test piece shape ( Figure 3 The welding test piece is a rectangular test piece, and the side length is made according to the standard sample and processing allowance, generally 100×200mm; the rectangular test piece complies with multiple welding standards and specifications, such as AWS and ISO, which helps to ensure the consistency and comparability of test results; it can more accurately represent the actual shape and size of the weld, because the weld is usually long in the actual welding process; it is relatively easy to cut out from the welded part, especially when destructive testing is required; the shape of the rectangular test piece helps to improve the accuracy, repeatability and comparability of weld joint quality testing, and is a standard shape widely used in welding quality assessment). Figure 3 The representative parts of the shape of the welding test piece are welded to form a square weld quality test piece generally with a size of 200×200 mm, and then the weld of the weld quality test piece is observed by SEM.

[0065] When conducting weld mechanical property tests, in order to evaluate the mechanical properties of the weld joint, a portion of the 200×200mm square weld quality test specimen can be cut to form a long strip including the weld, which serves as a representative piece for the weld mechanical property test.

[0066] When conducting the mechanical property test of the body, the shape of the representative piece is cylindrical, and the specific size is made according to the standard sample and processing allowance, which is generally During the test, the mechanical properties of the body such as tensile strength, yield strength, elongation after fracture, etc. can be obtained at the same time. The cylindrical shape has been adopted by many international standards. Since stress concentration usually occurs at the sharp corners or irregular shapes of the specimen, the stress distribution of the cylindrical geometry is relatively uniform, which can reduce the stress concentration phenomenon and help to more accurately evaluate the mechanical properties of the material; during the stretching process, the cylinder is easier to be fixed by the clamp, the diameter and length are easy to measure, and the deformation of the specimen is easier to predict and control, which helps to accurately control the size of the specimen, thereby ensuring the accuracy of the test results. For example, the characterization parts of the body mechanical properties test are such as Figure 3 The shape of the tensile test bar in medium mechanics.

[0067] When conducting a hardness characterization test block test, the characterization piece is in the shape of a cube, and the side length is made according to the standard specimen and processing allowance, generally 5mm to 20mm. The cube shape meets the standards of most hardness tests, such as Rockwell hardness and Brinell hardness tests, which helps to ensure the consistency and comparability of test results. The cube shape helps to reduce stress concentration, and its six faces are flat, which can reduce measurement errors caused by irregular shapes and help stabilize the specimen during the test. In addition, this shape is easy to process, and it is also easy to position and align the test instrument during the test, which can reduce operational errors. For example, the characterization piece for the hardness characterization test block test is such as Figure 3 Medium hardness characterizes the shape of the test piece.

[0068] Furthermore, in S1, the types of performance characterization parts, such as test bars for body mechanical properties (yield strength, tensile strength, elongation after fracture), test blocks for body mechanical properties (hardness), and wafers for infrared emissivity performance characterization, should be as complete as possible to pass a high-temperature oxidation process test once and test more performance results to improve the applicability of constructing the database.

[0069] In one possible implementation, additively manufactured GH4099 furnace test bars are used to characterize the mechanical tensile properties of parts at room temperature and 900°C; additively manufactured GH4099 furnace test blocks are used to characterize the room temperature hardness; additively manufactured GH4099 furnace test pieces of different sizes are used to characterize the room temperature hardness; infrared emissivity test pieces and oxide layer thickness test pieces of corresponding sizes and shapes are used to characterize the infrared radiation performance of high-temperature alloys; the number of the above characterization parts can be determined according to design requirements, and the design schematics of different performance characterization parts are shown as follows. Figure 2 、 Figure 3 shown.

[0070] Furthermore, in S1, the performance characterization parts are also processed according to the normal processing steps for the parts. The furnace-mounted performance characterization parts are formed during the laser selective additive manufacturing process. During the heat treatment process, all performance characterization parts are solution treated in the same furnace as the parts. During the part welding process, the mechanical performance characterization test pieces are connected according to the part's welding process parameters. During the machining process, the surface condition of the part is ensured to be consistent with the performance characterization parts.

[0071] Furthermore, in S1, the processing of the performance characterization part is carried out according to the processing procedures of the parts, including additive manufacturing, solution heat treatment, machining, and welding procedures.

[0072] Specifically, in S1, conventional additive manufacturing technology can be used for additive manufacturing. The material of the target part is selected for additive manufacturing. The integral part requiring high-temperature oxidation is a welded assembly made of high-temperature alloy additive manufacturing. The furnace performance characterization part and the part are manufactured together during the laser selective additive forming process.

[0073] Specifically, in S1, the purpose of solution heat treatment is to improve the microstructure and macroscopic properties of the material, enhancing the performance of the additively manufactured part to meet product application requirements. During solution heat treatment, the part and the performance characterization part must be processed in the same furnace to ensure that the preparation conditions of the characterization part and the part are consistent.

[0074] Specifically, in S1, machining refers to machining allowance. Factors such as material deposition and thermal effects during additive manufacturing result in insufficient dimensional accuracy of parts and high surface roughness of additive manufacturing. Machining can improve surface quality, reduce surface defects, and ensure that parts meet design requirements. At this time, the parts and performance characterization parts need to be processed together during machining to ensure that the surface state of the parts is consistent with the performance characterization parts. In addition, after the high-temperature oxidation process, the performance characterization parts will also be processed for subsequent performance testing, which generally refers to mechanical processing, such as processing the test rod into a certain test size, cutting the welding test piece into the size required for the test, etc.

[0075] Specifically, in S1, the welding process completes the connection of the welded mechanical properties characterization test pieces according to the welding process parameters of the parts. If the high-temperature oxidation process is placed before welding, the parts and performance characterization parts, especially those related to infrared radiation performance characterization, need to be surface treated before welding, such as grinding and polishing, sandblasting, or solution cleaning and wiping, to make the surface easier to weld.

[0076] Specifically, in S1, the high-temperature oxidation process can be performed after or before welding, depending on the product requirements. If the entire product surface requires an oxide film, the high-temperature oxidation process can be placed after welding; if a partial surface requires an oxide film, the high-temperature oxidation process can be placed before welding.

[0077] Furthermore, in S1, during the high-temperature oxidation process, oxidation parameters, including heating temperature, holding time, and oxygen environment, need to be controlled. The heating temperature and holding time can be set based on design requirements and processing needs. Oxygen environments primarily include conventional air and oxygen-enriched environments. Generally, to achieve the same oxide layer thickness and infrared radiation performance, the processing time of high-temperature alloys in conventional air is longer than in oxygen-enriched environments. Therefore, the oxygen environment can also be appropriately selected based on the holding time setting.

[0078] It should be noted that in the specific operation, the performance results under the experimental parameters (oxidation parameters) are obtained by first matching the different parameters in the database and using the performance characterization parts to carry out the experiment. Then, the corresponding parts are selected according to the desired performance, and then the parts are tested under the same oxidation parameters to achieve the purpose of regulating the oxidation parameters during the high-temperature oxidation process.

[0079] In one possible embodiment, the aging heat treatment system of GH4099 high-temperature alloy is used to perform high-temperature oxidation treatment on the parts and all performance-characterizing parts in an air environment, with a heating temperature of 850°C, a holding time of 8 hours, and an oxygen environment of conventional air.

[0080] Specifically, the high-temperature oxidation experiment also requires an aging heat treatment process, the main purpose of which is to improve the performance of the alloy and stabilize the microstructure and geometric dimensions. When the product quality requirements are not high, the aging heat treatment process can be omitted; when the product quality requirements are high, the aging heat treatment process is required. In this case, the high-temperature oxidation process can be combined with the aging heat treatment process. During the aging heat treatment, the alloy is exposed to air. Due to the high temperature, the alloy surface reacts with oxygen to form oxides, completing the high-temperature oxidation process and simplifying the process. In this process, all performance characterization parts are processed together with the parts.

[0081] Furthermore, in S1, the surface of the parts and performance characterization parts after the processing step has an oxide film; the oxide film is an oxide film formed by the high-temperature alloy itself, and has a thickness of 5μm to 50μm.

[0082] Specifically, in S2, grinding and polishing is to use a grinding wheel or a grinding head for rough grinding to remove surface unevenness and roughness to make the surface smoother, and use a mechanical polishing machine or manual operation to perform fine polishing on parts and other performance characterizing parts, especially infrared radiation performance characterizing parts, to remove the surface oxide layer, rust and other contaminants of parts and performance characterizing parts, ensure that the metal surface is brighter, and increase its appearance texture.

[0083] Specifically, in S2, sandblasting involves using compressed air to spray dry, oil-free, and non-large quartz sand onto the metal surfaces of parts and other performance-relevant components. This removes surface stains and impurities while increasing the roughness of the metal surface for subsequent high-temperature treatment. The diameter of the quartz sand and the air pressure of the sandblaster can be appropriately selected based on the material and thickness of the part. After sandblasting, the workpiece should evenly and completely reveal the natural metal color, and the surface color should be uniform.

[0084] Specifically, in S2, solution cleaning and wiping is to use a dust-free cloth dipped in anhydrous ethanol solution or acetone solution to wipe the surface of the parts after sandblasting, ensuring that the surfaces of the cleaned parts and other performance-characterizing parts should not be touched with bare hands.

[0085] Furthermore, in S2, the high-temperature oxidation parameters include heating temperature, holding time, and oxygen environment.

[0086] Specifically, when conducting orthogonal tests, in order to ensure product performance, orthogonal tests of heating temperature and holding time are carried out to obtain the test results of bulk mechanics and infrared radiation performance.

[0087] In one possible implementation, to establish a database of correspondences between high-temperature oxidation parameters and performance, and to ensure mechanical properties, orthogonal tests were conducted on GH4099 parts at heating temperatures of 700°C, 750°C, 800°C, 850°C, and 900°C, with holding times of 2h, 4h, 6h, 8h, 10h, and 12h. Results were obtained for infrared emissivity, oxide layer thickness, bulk mechanical properties (tensile strength, yield strength, and elongation), hardness, and weld mechanical properties (tensile strength, yield strength, and elongation). Some of the results are shown in Tables 3 and 4. Table 3 shows the orthogonal test results for heating at 750°C and holding times of 2h, 4h, 6h, 8h, 10h, and 12h; Table 4 shows the orthogonal test results for heating at 850°C and holding times of 2h, 4h, 6h, 8h, 10h, and 12h.

[0088] Furthermore, in S2, the construction of the correspondence and regularity database of high-temperature oxidation parameters, infrared radiation performance, and bulk performance is composed of data points of the test results.

[0089] Furthermore, in S3, repeated experiments are performed to correct possible abnormal result data points, and the performance results are compensated using intermediate parameters in the database.

[0090] Specifically, the database is calibrated and compensated using intermediate parameters or repeated experiments to continuously improve the database and increase its accuracy. For example, according to the results in the regular database, the performance obtained under 850℃ for 8h can meet the performance requirements of the parts, while the performance obtained under 850℃ for 6h cannot meet the performance requirements of the parts. In order to explore the optimal process window, the database was calibrated using 850℃ for 7h. The specific performance results are shown in Table 5, which shows the test results of infrared emissivity performance, bulk mechanical properties (yield strength, tensile strength, elongation after fracture, hardness), and weld mechanical properties obtained from the test with a heating temperature of 850℃ and a holding time of 7h. In addition, in this step, the abnormal points in the database can also be repeatedly tested.

[0091] Furthermore, in S4, based on the design requirements for the high-temperature alloy product's bulk and infrared radiation performance, target infrared radiation performance indicators and bulk performance indicators are proposed. A database is then used to identify high-temperature oxidation parameters or parameter ranges that meet both performance indicators, and the high-temperature oxidation process is performed using these parameters or parameter ranges. Using the database data and design requirements, it is determined whether the bulk and infrared radiation performance of the high-temperature alloy are balanced. If both the bulk and infrared radiation performance are met, or vice versa, if both the infrared and bulk performance are met, then a balance has been achieved, effectively regulating the balance between the two.

[0092] It should be noted that the chemical composition and microstructure of high-temperature alloys determine their bulk properties. Modifying bulk properties to control infrared radiation performance will affect the basic properties of the alloy. High-temperature alloys require high-temperature oxidation to optimize their properties. Simultaneously controlling bulk and infrared radiation performance during high-temperature oxidation requires precise control of temperature, time, and atmosphere, which is difficult in practice. Infrared radiation performance can be controlled by varying the thickness, morphology, and phase of the surface oxide layer. However, these techniques may adversely affect the bulk properties of the alloy, such as reducing its tensile strength and elongation.

[0093] Furthermore, this control method first proposes target infrared radiation performance indicators and bulk performance indicators based on the design requirements of the high-temperature alloy product's infrared radiation performance and bulk performance. Then, a database is used to find high-temperature oxidation parameters that can meet both performance indicators, and oxidation experiments are conducted using these parameters. When only one performance indicator can be met, the more important indicator is met first. In some cases, improving one aspect of the alloy's performance may sacrifice another. For example, increasing the alloy's infrared radiation capability may require using a specific thickness of oxide layer and high-temperature oxidation treatment parameters, which may reduce the alloy's mechanical properties.

[0094] The following is a detailed description of a high-temperature alloy performance evaluation and control method based on high-temperature oxidation according to the present invention.

[0095] Example 1

[0096] This example provides a method for controlling the properties of GH4099 high-temperature alloy based on high-temperature oxidation.

[0097] GH4099 superalloy is one of the most widely used high-temperature alloys in aerospace applications. It is a highly alloyed nickel-based aging alloy. The addition of Cr, Co, W, and Mo provides solid solution strengthening, while Al and Ti form an age-strengthening phase. B, Ce, and Mg strengthen grain boundaries. GH4099 superalloy can be used for extended periods below 900°C, with short-term maximum operating temperatures reaching 1000°C. The primary heat treatment methods for GH4099 superalloy are solution treatment and aging treatment, which can be performed in both vacuum and air atmospheres.

[0098] In this embodiment, the integral part requiring high temperature oxidation is a welded assembly manufactured using additive manufacturing of GH4099 high temperature alloy. The overall performance of the part that requires attention is mainly divided into two parts: bulk performance and infrared radiation performance.

[0099] The main body properties and requirements include: main body mechanical properties: hardness (room temperature, HV ≥ 400), weld mechanical properties (room temperature), main body mechanical properties: yield strength, tensile strength, elongation after fracture (room temperature, 900 ° C). The specific design requirements are shown in Table 1.

[0100] Table 1 GH4099 alloy body properties and requirements

[0101]

[0102] Infrared radiation performance includes: infrared emissivity after high temperature oxidation (room temperature ≥ 0.75, 1000 ℃ ≥ 0.8) and oxide layer thickness ≥ 15 μm. According to the technical solution provided by the present invention, the specific steps in this embodiment are as follows:

[0103] Step 1: Design a high-temperature oxidation orthogonal test, design and process performance characterization parts, use the performance characterization parts to complete the high-temperature oxidation experiment and conduct corresponding performance tests.

[0104] When designing performance characterization parts, first determine the experimental objectives, experimental parameters, material type, experimental temperature range, oxidation time, etc., and then design the performance characterization parts. Designing performance characterization parts involves calculating the geometry, size, material, number of performance characterization parts required for orthogonal testing, and performance type. Processing performance characterization parts refers to the processing steps before the high-temperature oxidation process, such as additive manufacturing, heat treatment, grinding, and welding of welded coupons.

[0105] It should be noted that the database is constructed using the performance test results of representative parts after high-temperature oxidation experiments. To establish an accurate database, the accuracy of the performance test results of the representative parts must be guaranteed. Therefore, the processing steps of the representative parts must be consistent with the processing steps of the parts to ensure that the representative parts represent the performance of the final parts.

[0106] After processing the performance characterization parts, they must undergo high-temperature oxidation tests, which is called a high-temperature oxidation process. After the high-temperature oxidation process, the performance characterization parts will also be processed for subsequent performance testing, which generally refers to mechanical processing, such as processing the test rods into certain test sizes, cutting the welding test pieces into the required test sizes, etc.

[0107] In this implementation, the material state of the parts before high-temperature oxidation is in a solid solution state. According to the properties of the material and general rules, it is difficult to meet the precipitation of the strengthening phase in the GH4099 material at a lower temperature, thus failing to achieve the purpose of strengthening the material. At the same time, the production of the oxide film on the surface of the material at a lower temperature is also very difficult. The solid solution temperature of GH4099 is around 1100°C, and the temperature of high-temperature oxidation should be lower than the solid solution temperature. Therefore, in order to meet the mechanical properties of the parts, the high-temperature oxidation temperature parameters of the selected orthogonal test can be set at 750°C-950°C. The designed orthogonal experiment is shown in Table 2. Under one process parameter, multiple types of specimens were processed, and different types of specimens obtained different properties, and all performance results under the process parameters were obtained.

[0108] Table 2 High temperature oxidation orthogonal test

[0109]

[0110] In this embodiment, because the parts are formed by additive manufacturing, the GH4099 furnace test bars manufactured by additive manufacturing are used to characterize the mechanical tensile properties of the parts at room temperature and 900°C; the GH4099 furnace test blocks manufactured by additive manufacturing are used to characterize the hardness at room temperature; the GH4099 furnace test pieces of different sizes manufactured by additive manufacturing are used to characterize the hardness at room temperature; infrared emissivity test pieces and oxide layer thickness test pieces of corresponding sizes and shapes manufactured by additive manufacturing are also used to characterize the infrared emissivity performance of high-temperature alloys; the test plates manufactured by additive manufacturing are welded by a specific welding method, and the strength of the welded joints is tested; the number of the above characterization parts can be determined according to design requirements. The design schematic diagram of different performance characterization parts is shown as follows. Figure 2 、 Figure 3 As shown, the test pieces, test rods, and test blocks are just different in shape and all are performance characterizing parts.

[0111] Step 2: Organize the performance results, obtain the corresponding relationship between high-temperature oxidation parameters, infrared emissivity performance, and body performance, and complete the construction of the regularity database.

[0112] Based on the overall test results, the corresponding relationships between high-temperature oxidation parameters, infrared emissivity performance, and bulk performance were analyzed and a regularity database was constructed. For ease of illustration, only some of the results are shown in Tables 3 and 4. Table 3 shows the test results of infrared emissivity performance, mechanical properties, hardness, and room-temperature mechanical properties of the weld obtained from an orthogonal test with a heating temperature of 750°C and holding times of 2h, 4h, 6h, 8h, 10h, and 12h. Table 4 shows the test results of infrared emissivity performance, mechanical properties, hardness, and room-temperature mechanical properties of the weld obtained from an orthogonal test with a heating temperature of 850°C and holding times of 2h, 4h, 6h, 8h, 10h, and 12h.

[0113] Table 3 Orthogonal test results with heating temperature of 750℃ and holding time of 2h, 4h, 6h, 8h, 10h and 12h

[0114]

[0115] Table 4 Orthogonal test results with heating temperature of 850℃ and holding time of 2h, 4h, 6h, 8h, 10h and 12h

[0116]

[0117] Use intermediate parameters or repeated experiments to calibrate and compensate the database, continuously improve the database and enhance its accuracy.

[0118] Based on the results in the regularity database, the performance achieved at 850°C for 8 hours meets the part performance requirements. To explore the optimal process window, the database was calibrated using 850°C for 7 hours. Specific performance results are shown in Table 5, which shows the infrared emissivity, mechanical properties, hardness, and room-temperature mechanical properties of the weld obtained from the test with a heating temperature of 850°C and a holding time of 7 hours. Furthermore, this step can also be used to repeat the test for outliers in the database.

[0119] Table 5 Test results of heating temperature 850℃ and holding time 7h

[0120]

[0121] The database is used to select parameters for high-temperature oxidation in combination with specific part design requirements.

[0122] From the database results and the compensation group experimental results, it was found that the process parameters of 850℃8h met the design requirements of the parts.

[0123] The database is used to conduct low-cost evaluation and characterization of infrared emissivity performance under specific high-temperature oxidation parameters.

[0124] From the database rules, for GH4099 with the same forming method and processing path, there is a certain relationship between the infrared emissivity results and the change of oxide layer thickness, such as Figure 5 The following graph shows the relationship between the oxide layer thickness and infrared emissivity at various temperatures for GH4099 superalloy. As can be seen from the graph, as the oxide layer thickness increases, the infrared emissivity also increases, forming a parabolic curve. Because infrared emissivity testing is expensive, the oxide layer thickness in this database can be used to indirectly represent the infrared emissivity results.

[0125] The performance characterization parts under the high temperature oxidation parameters of 850℃ for 8h were subjected to oxidation layer morphology analysis and oxidation phase analysis tests. The test results are as follows: Figure 6 and Figure 7 As shown, Figure 6 This is an SEM image of a high-temperature alloy with an oxide film on the surface prepared in Example 1; Figure 7 This is the XRD pattern of the high-temperature alloy with an oxide film on the surface prepared in Example 1.

[0126] from Figure 6 It can be seen that the thickness of the oxide film is evenly distributed over the entire surface, with no obvious thickness difference. The oxide film exhibits consistent uniformity, indicating that the oxide film prepared under the high-temperature oxidation parameters is very successful.

[0127] from Figure 7It can be seen that the oxide film is mainly composed of Cr2Ni3 with high purity. In addition, it also contains a small amount of Cr2O3 and CoCr2O4. The oxide film has a low impurity content and meets certain performance requirements.

[0128] Step 3: Process the part according to the normal processing steps, completing the furnace performance characterization parts during the laser selective additive manufacturing process (the performance characterization parts and the part are formed together using the same forming process). During the heat treatment process, all performance characterization parts are solution treated in the same furnace as the part. During the part welding process, the mechanical performance characterization test pieces are connected according to the part's welding process parameters. During the machining process, ensure that the surface condition of the part is consistent with the performance characterization parts.

[0129] Step 4: Surface treatment of parts and performance characterization parts, especially infrared radiation related performance characterization parts. The specific treatment steps include: (1) grinding and polishing, using a grinding wheel or a grinding head for rough grinding to remove surface unevenness and roughness, making the surface smoother, and using a polishing machine or manual fine polishing to ensure that the metal surface is brighter and increase its appearance texture; (2) sand blasting, using compressed air to spray quartz sand particles onto the metal surface to remove surface stains and impurities, and at the same time increase the roughness of the metal surface for subsequent high-temperature treatment. After sand blasting, the surface color of parts and infrared radiation related performance characterization parts should be uniform; (3) solution cleaning and wiping, using a dust-free cloth dipped in alcohol solution to wipe the surface of the parts after sand blasting to ensure cleanliness.

[0130] Step 5: Use the GH4099 aging heat treatment system to perform high-temperature oxidation treatment on the parts and all performance-characterized parts in an air environment. The heating temperature is 850°C, the heat holding time is 8 hours, and the oxygen environment is a normal air environment.

[0131] Step 6: After high-temperature oxidation, use performance characterization parts to conduct corresponding performance tests on the parts to obtain performance reference data.

[0132] Step 7: In this embodiment, an orthogonal test under certain parameters is designed, and the above steps are repeated to obtain the correspondence and regularity set between high-temperature oxidation parameters and bulk properties and infrared radiation properties; for the GH4099 parts in this embodiment, in order to ensure the mechanical properties, orthogonal tests were carried out with heating temperatures of 700°C, 750°C, 800°C, 850°C, and 900°C and holding times of 2h, 4h, 6h, 8h, 10h, and 12h, and the performance test results of bulk mechanical properties (yield strength, tensile strength, elongation after fracture, hardness), weld mechanical properties, and infrared radiation properties (oxide layer thickness, infrared emissivity) were obtained.

[0133] Step 8: Using the obtained experimental parameters and performance result set, the corresponding high-temperature oxidation parameters in the set can be selected according to the design requirements of the body performance and infrared radiation performance of different GH4099 parts.

[0134] According to the infrared radiation performance requirements: infrared emissivity after high-temperature oxidation (room temperature ≥0.75), the data in Table 3 were screened, and it was found that the room temperature infrared emissivity results in Table 3 did not meet the requirement of ≥0.75, so Table 3 was excluded; then the data in Table 4 were screened, and it was found that only test group numbers 3-3, 4-3, 5-3, and 6-3 in Table 4 met the requirements, so 1-3 and 2-3 were excluded.

[0135] According to the infrared radiation performance requirements: infrared emissivity after high-temperature oxidation (1000°C ≥ 0.8), data were screened in the test groups 3-3, 4-3, 5-3, and 6-3 in Table 4, and it was found that these test groups all met the requirements.

[0136] According to the infrared radiation performance requirement: the oxide layer thickness is ≥ 15 μm, the data in the test groups 3-3, 4-3, 5-3, and 6-3 in Table 4 were screened, and it was found that only the test groups 4-3, 5-3, and 6-3 met the requirements, so 3-3 was excluded.

[0137] In turn, according to the specific design requirements of the main performance requirements: room temperature hardness (HV ≥ 400), room temperature weld mechanical properties, room temperature and 900 ° C high temperature mechanical tensile properties (yield strength, tensile strength, elongation after fracture), screening was carried out in test groups 4-3, 5-3, and 6-3, and it was found that all met the requirements.

[0138] Test group numbers 4-3, 5-3, and 6-3 all meet the experimental requirements, that is, 850℃8h, 850℃10h, and 850℃12h all meet the requirements. The most energy-saving 850℃8h is selected as the optimal condition, that is, the performance obtained under 850℃8h insulation can meet the part performance requirements.

[0139] To explore the optimal process window, although experiment 3-3 (850℃ 6h) was previously excluded, it was not yet determined whether 850℃ 7h was better than 850℃ 8h. Therefore, the database was calibrated using 850℃ 7h. The specific performance results are shown in Table 5.

[0140] According to the infrared radiation performance requirements: infrared emissivity after high-temperature oxidation (room temperature ≥0.75, 1000℃ ≥0.8), oxide layer thickness ≥15μm, the data in Table 5 were screened and it was found that Table 5 met the requirements.

[0141] According to the requirements of the main performance: room temperature hardness (HV ≥ 400), and the specific design requirements of the room temperature weld mechanical properties and room temperature and 900 ° C high temperature mechanical tensile properties (yield strength, tensile strength, elongation after fracture) in Table 1, the data in Table 5 were screened and it was found that the room temperature weld mechanical properties (yield strength / MPa) required to be ≥ 650, while the value in Table 5 was 620, which did not meet the requirements. Therefore, the condition of 850 ° C 7h was excluded, and the condition of 850 ° C 8h was the optimal condition.

[0142] Step 9: After testing, all the properties obtained when the heating temperature is 850° C., the holding time is 8 hours, and the oxygen environment is an ordinary air environment meet the design requirements of the parts in this embodiment, and the curing process is applicable.

[0143] Example 2

[0144] This example provides a method for controlling the properties of the GH3128 superalloy based on high-temperature oxidation. GH3128 is a high-performance nickel-based alloy with excellent plasticity, long-term creep strength, oxidation resistance, and good stamping and welding properties. Through solid solution strengthening with tungsten and molybdenum elements and grain boundary strengthening with boron and zirconium elements, GH3128's overall performance leads the pack among similar nickel-based solid solution alloys. This alloy is particularly suitable for manufacturing high-temperature components such as combustion chamber flame tubes, afterburner casings, and regulating plates. Capable of withstanding temperatures of 950°C and long-term operation, it is widely used in the aerospace engine field.

[0145] In this embodiment, the integral part that needs high-temperature oxidation is a GH3128 high-temperature alloy shaft-shaped part. There are requirements for the performance of the part itself, and at the same time, the performance that needs to be paid attention to on a specific surface of the part is the infrared radiation performance. The main body performance includes: the mechanical tensile properties of the part at room temperature and 900°C (tensile strength, elongation). The specific requirements are: after the part is oxidized at high temperature, the infrared emissivity should be ≥0.75, and the tensile strength of the part at room temperature should be ≥800MPa, the elongation should be ≥25%, the tensile strength at 900°C should be ≥210MPa, the elongation should be ≥50%, and the infrared radiation performance includes: infrared emissivity after high-temperature oxidation. The general shape of the part and the specific surface that needs to pay attention to the infrared radiation performance are as follows Figure 4 As shown in , according to the technical solution provided by the present invention, the specific steps in this embodiment are as follows:

[0146] Step 1: Based on the technical conditions and performance of the part, the process design and process preparation of the part and the performance characterization parts are carried out. In this embodiment, GH3128 furnace test bars are used to characterize the mechanical tensile properties of the part at room temperature and 900°C. Infrared emissivity test pieces and oxide layer thickness test pieces of corresponding sizes and shapes are used to characterize the infrared radiation performance of the high-temperature alloy. At the same time, before the part is officially put into production and processing, the process method provided by the present invention is used to complete the relationship between different holding times and the infrared emissivity of the GH3128 high-temperature alloy under 900°C heating conditions. A brief list of the collection is as follows:

[0147] Table 6 Relationship between holding time at 900℃ and infrared emissivity of GH3128 superalloy

[0148] Heating temperature / ℃ Holding time / h Oxygen environment Infrared emissivity <![CDATA[Oxidation weight gain / mg·cm -2 > 900 10h Regular air 0.55 0.25 900 20h Regular air 0.75 0.31 900 30h Regular air 0.79 0.34 900 40h Regular air 0.81 0.39

[0149] Table 7 Relationship between holding time at 900℃ and bulk properties of GH3128 superalloy

[0150]

[0151] Step 2: The overall part processing steps primarily include additive manufacturing, solution heat treatment, preliminary machining, high-temperature oxidation, and final machining. In this example, only one surface of the shaft-shaped part requires high-temperature oxidation, so the high-temperature oxidation surface must be processed during the preliminary machining process. After oxidation, final machining is performed on all areas except the surface where the heat-insulating oxide film is to be retained, in order to remove the oxide layer from the remaining areas of the high-temperature alloy part.

[0152] Step 3: Process the parts according to other normal processing procedures. During the processing, ensure that the surface of the parts that need to be high-temperature oxidized is consistent with the surface state of the infrared performance characterization parts.

[0153] Step 4: Surface treatment of parts and performance characterization parts, especially infrared radiation related performance characterization parts. The specific treatment steps include: (1) grinding and polishing, using a grinding wheel or a grinding head for rough grinding to remove surface unevenness and roughness, making the surface smoother, and using a polishing machine or manual fine polishing to ensure that the metal surface is brighter and increase its appearance texture; (2) sand blasting, using compressed air to spray quartz sand particles onto the surface of the shaft part that needs high-temperature oxidation to remove surface stains and impurities, and at the same time increase the roughness of the metal surface for subsequent high-temperature treatment. After sand blasting, the surface color of the parts and infrared radiation related performance characterization parts should be uniform; (3) solution cleaning and wiping, using a dust-free cloth dipped in alcohol solution to wipe the surface of the sandblasted parts to ensure cleanliness.

[0154] Step 5: Based on the relationship between the holding time at 900°C and the infrared emissivity and bulk properties of the GH3128 high-temperature alloy, the experimental parameters for high-temperature oxidation of the parts are determined as follows: heating temperature 900°C, holding time 20h, and oxygen environment as conventional air environment.

[0155] According to the infrared radiation performance requirements: infrared emissivity after high-temperature oxidation (room temperature ≥ 0.75), screening was performed in Table 6, and the conditions of infrared emissivity of 0.55 and 900°C for 10h were excluded.

[0156] According to the requirements of the main performance: the tensile strength of the part at room temperature ≥ 800MPa, elongation ≥ 25%, the tensile strength at 900℃ ≥ 210MPa, elongation ≥ 50%, the data in Table 7 are screened and found to meet the requirements, that is, the heating temperature of 900℃ and the holding time of 20h to 40h meet the requirements. At this time, the most energy-saving 900℃ 20h is selected as the best condition, that is, the performance obtained under the holding time of 900℃ 20h can meet the performance requirements of the part. At this time, combined with Table 6, it can be seen that the oxidation weight gain / mg·cm -2 Should be ≥0.31 mg·cm -2 .

[0157] Step 6: As can be seen from Table 6, as the infrared emissivity increases, the oxidation weight gain also gradually increases. For this GH3128 part, the high-temperature oxidation process is used to cure it. Since the infrared emissivity test cost is 1,500 yuan per time, in order to reduce the test cost and ensure product quality, in the subsequent production process, the weight gain before and after oxidation is used as a means of evaluating the infrared radiation performance of the part. That is, the weight gain of the infrared emissivity test piece after high-temperature oxidation is measured using an analytical balance to calculate the oxidation weight gain, and according to the design requirements, the oxidation weight gain should be ≥0.31 mg·cm -2 .

[0158] The above description is only a preferred specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with this technical field within the technical scope disclosed by the present invention should be covered by the scope of protection of the present invention.

Claims

1. A method for controlling the properties of a high-temperature alloy based on high-temperature oxidation, characterized in that: The following steps are involved: S1. Design high-temperature oxidation orthogonal test, design and process performance characterization parts, use performance characterization parts to complete high-temperature oxidation experiment and conduct performance test; S2. Arrange the performance results, obtain the corresponding relationship between high temperature oxidation parameters, infrared radiation performance, and bulk performance, and complete the construction of the regularity database; S3. Use intermediate parameters or repeated experiments to calibrate and compensate the database; S4. Use the database to combine the high-temperature alloy product's intrinsic properties and infrared radiation performance requirements to select high-temperature oxidation parameters.

2. The performance control method according to claim 1, characterized in that: In S1, the processing of the performance characterization part is carried out according to the processing procedures of the parts, including additive manufacturing, solution heat treatment, machining, and welding procedures.

3. The performance control method according to claim 1, characterized in that: In S1, the performance characterizing part needs to be designed and processed according to the technical conditions of the part and the performance of interest to obtain the performance characterizing part.

4. The performance control method according to claim 1, characterized in that: In S1, the performance test includes a body performance test and an infrared radiation performance test.

5. The performance control method according to claim 4, characterized in that: The main body properties include main body mechanical properties, weld mechanical properties, and weld quality; the main body mechanical properties include tensile strength, yield strength, elongation after fracture, and hardness.

6. The performance control method according to claim 4, characterized in that: The infrared radiation performance includes infrared emissivity, oxide layer thickness, oxide layer morphology, oxidation phase analysis, and weight gain after oxidation.

7. The performance control method according to claim 1, characterized in that: In S2, the high temperature oxidation parameters include heating temperature and holding time.

8. The performance control method according to claim 1, characterized in that: In S3, repeated experiments are performed to correct possible abnormal result data points, and the performance results are compensated using intermediate parameters in the database.

9. The performance control method according to claim 1, characterized in that: In S4, according to the design requirements of the main performance and infrared radiation performance of the high-temperature alloy product, the target infrared radiation performance index and the main performance index are proposed, and then the high-temperature oxidation parameters or parameter segments that can meet the two performance indicators are selected through the database. The parts are subjected to a high-temperature oxidation process using the parameters or parameter segments to obtain the finished parts.

10. The performance control method according to claim 9, characterized in that: The finished parts meet the requirements of infrared radiation performance and body performance at the same time.