Preparation method of rare earth iron-based permanent magnet material
Through rare earth alloys composed of specific elements and multiple heat treatment processes, the problem of preferential diffusion of non-rare earth elements in the heat treatment diffusion process of rare earth alloys is solved, which significantly improves the coercive force of magnets and reduces the residual magnetization drop, realizing the rare earth elements Efficient utilization and energy consumption reduction.
Patent Information
- Application Number
- CN202411317321.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-08
AI Technical Summary
During the heat treatment diffusion process of existing rare earth alloys, the preferential diffusion of non-rare earth elements leads to a sharp increase in the melting point of the diffusion source alloy components, which cannot meet the grain boundary diffusion requirements in the low temperature state of magnets. The existing technology is improving the coercive force of magnets and controlling the remaining energy. The magnetic drop level is insufficient, the cost control is poor, and it requires long-term heat treatment, which makes energy consumption high.
Rare earth alloys composed of specific elements are used as the grain boundary diffusion source. Through multiple heat treatment and annealing processes under vacuum conditions, the high concentration of non-rare earth elements in rare earth alloys preferentially diffuse into the grain boundary phase, changing the thermodynamic state of the grain boundary region, forming multiple The synergistic diffusion effect of elements, rare earth elements are distributed deep in the magnet, avoiding surface accumulation, increasing the coercive force of the magnet and reducing the remanent magnetic drop.
The coercive force of the magnet is significantly improved, and the residual magnetization drop is small, which solves the problems of large amount of rare earths, long heating time and poor diffusion effect, and achieves cost control and energy consumption reduction.
Smart Images

Figure BDA0005052580540000101
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a rare earth iron-based permanent magnetic material. Background Art
[0002] Existing grain boundary diffusion rare earth alloys are all low-melting point alloys corresponding to eutectic components, with high rare earth content and insufficient non-rare earth element content. The preferential diffusion of non-rare earth elements during heat treatment diffusion causes the melting point of the diffusion source alloy component to increase sharply, which cannot meet the kinetic requirements of grain boundary diffusion in the magnet under low temperature conditions.
[0003] CN117316616A discloses a method for reconstructing the grain boundaries of NdFeB magnets using a mixed rare earth alloy, wherein low melting point alloy powder and NdFeB powder are mechanically mixed in proportion, and then the mixed powder is heat treated, and the obtained diffused magnetic powder is sintered by discharge plasma to obtain an isotropic diffused magnet. This method is mainly used to process the basic particles in the preparation process of magnetic materials, and is not suitable for improving the performance of iron-based rare earth permanent magnets that have been prepared.
[0004] CN116072368A discloses a NdFeB magnet, wherein the distribution of rare earth elements in the main phase grains of the NdFeB magnet includes two shell structures: one is a heavy rare earth-rich yttrium-rich synchronous core-shell structure located on the surface of the NdFeB magnet; the other is a heavy rare earth-rich shell structure located inside the NdFeB magnet. According to the binary alloy phase diagram of rare earth elements and other elements, rare earth elements react with other elements at the eutectic point. The preferential diffusion of non-rare earth elements during the heat treatment diffusion process will cause the melting point of the diffusion source alloy component to rise sharply, which is not conducive to the grain boundary diffusion reaction and reduces the utilization rate of rare earth elements.
[0005] CN118507186A discloses a rare earth amorphous alloy for grain boundary diffusion of iron-based rare earth permanent magnets. Non-rare earth elements are elements that have eutectic reactions with rare earths, and there is also the problem that eutectic reactions are not conducive to grain boundary diffusion reactions.
[0006] At present, a large number of pure rare earth metals Dy, Tb or rare earth alloys containing a small amount of non-rare earth elements are used as grain boundary diffusion material sources to improve the diffusion effect of magnets by lowering the melting point. However, the existing rare earth alloys are obviously insufficient in improving the coercive force of magnets and controlling the level of residual magnetization decline. The high content of heavy rare earth in the existing diffusion source is not conducive to cost control. At the same time, the existing grain boundary diffusion technology requires long-term heat treatment and high energy consumption. Summary of the invention
[0007] In view of this, an object of the present invention is to provide a method for preparing a rare earth iron-based permanent magnetic material, which can significantly increase the coercive force of the magnet but only slightly reduce the remanence.
[0008] The present invention adopts the following technical solutions to achieve the above-mentioned purpose.
[0009] The present invention provides a method for preparing a rare earth iron-based permanent magnetic material, the preparation method comprising the following steps:
[0010] 1) coating a rare earth alloy on the surface of a rare earth iron-based magnet to be treated to obtain a coated rare earth iron-based magnet; wherein the atomic ratio of Tb, Al, Sn, Cu and Ti in the rare earth alloy is 24-58:12-18:9-16:35-45:10-18;
[0011] 2) heat treating the coated rare earth iron-based magnet under vacuum conditions at 600-800° C., then heat treating it at 850-960° C., and obtaining a heat-treated rare earth iron-based magnet after cooling;
[0012] 3) The rare earth iron-based magnet after heat treatment is heat treated under vacuum conditions at 450-550° C. to obtain a rare earth iron-based permanent magnet material.
[0013] According to the preparation method of the present invention, preferably, in the rare earth alloy, the atomic ratio of Tb, Al, Sn, Cu and Ti is 30-50:13-15:10-15:40-45:12-16.
[0014] According to the preparation method of the present invention, preferably, the rare earth alloy is in the form of particles, and the particle size thereof is 1 to 10 μm.
[0015] According to the preparation method of the present invention, preferably, in the rare earth iron-based magnet after coating, the thickness of the film layer formed by the rare earth alloy is 3 to 15 μm.
[0016] According to the preparation method of the present invention, preferably, the rare earth iron-based magnet to be processed is a sintered neodymium iron boron magnet.
[0017] According to the preparation method of the present invention, preferably, the main phase of the sintered NdFeB magnet is RE2Fe 14 B, where RE is a rare earth element.
[0018] According to the preparation method of the present invention, preferably, based on the total weight of the sintered NdFeB magnet, the sintered NdFeB magnet has the following composition:
[0019] Al 0.3wt%~0.5wt%, B 0.8wt%~1.0wt%, Ce 0.03wt%~0.05wt%, Co0.004wt%~0.006wt%, Cu 0.1wt%~0.2wt%, Dy 0.001wt%~0.002wt%, Ga 0.1wt%~0.3wt%, Nd 20wt%~25wt%, Pr 6wt%~8wt%, Zr 0.1wt%~0.2wt%, the balance is Fe.
[0020] According to the preparation method of the present invention, preferably, it also includes the following steps:
[0021] The rare earth iron-based blank is sandblasted to remove pollutants on the surface, and then ultrasonically cleaned in anhydrous ethanol to obtain a rare earth iron-based magnet to be processed;
[0022] The sandblasting pressure is 0.1-1.0 MPa, the angle between the spray gun and the surface normal of the rare earth iron-based blank is greater than or equal to 45°, the sandblasting trajectory is linear and the sandblasting is not repeated in the same area.
[0023] According to the preparation method of the present invention, preferably, coating the rare earth alloy on the surface of the rare earth iron-based magnet to be treated comprises the following steps:
[0024] The rare earth iron-based magnet to be processed is fixed on a fixture disk, and a rare earth alloy is used as a target material to deposit a rare earth alloy film on the surface of the rare earth iron-based magnet by magnetron co-sputtering.
[0025] According to any preparation method of the present invention, preferably, compared with the rare earth iron-based magnet to be processed, the remanence of the rare earth iron-based permanent magnet material decreases by 0.01% to 1.25%, and the coercivity increases by 95% to 99%.
[0026] The present invention uses a rare earth alloy composed of specific elements as a grain boundary diffusion source in combination with a heat treatment process to prepare a rare earth iron-based permanent magnetic material, which can significantly improve the coercive force of the magnet while reducing the magnitude of the residual magnetization drop. In addition, according to the preferred technical solution of the present invention, it can also solve the problems of large rare earth dosage, long heating time and poor diffusion effect existing in the prior art. DETAILED DESCRIPTION
[0027] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0028] The "remanent magnetism" mentioned in the present invention refers to the magnet being able to maintain a certain magnetization intensity in the original direction of the external magnetic field after the external magnetic field is removed after the magnet is magnetized to saturation, usually recorded as B r , the unit is Tesla (T) or Gauss (G).
[0029] The "coercive force" mentioned in the present invention is the "intrinsic coercive force", which refers to the reverse magnetic field strength applied when the sum of the microscopic magnetic dipole moment vector inside the magnet is reduced to 0, usually denoted as H cj , the unit is Oersted (Oe) or Ampere / meter (A / m).
[0030] The "vacuum degree" mentioned in the present invention refers to absolute vacuum degree; the smaller the value is, the higher the vacuum degree is.
[0031] <Preparation method of rare earth iron-based permanent magnetic material>
[0032] The present invention uses a rare earth alloy with a specific element composition as a material source for the grain boundary diffusion of a rare earth iron-based magnet. When heated, the high-concentration non-rare earth elements in the rare earth alloy diffuse preferentially into the grain boundary phase. At this time, the chemical composition of the rare earth alloy diffusion source on the surface of the magnet approaches the eutectic point with a low melting point. A large amount of non-rare earth elements preferentially enter the grain boundary and alloy with it, changing the thermodynamic state parameters such as the enthalpy change and entropy change of the alloy in the grain boundary region, forming a positive effect of multi-element synergistic diffusion. The rare earth enters the deep part of the magnet and is distributed in the RE2Fe 14 The surface layer of the grains of the B main phase avoids waste caused by accumulation on the surface of the magnet, and at the same time promotes the inhomogeneous distribution of the main elements in the key phases of the magnet, which significantly improves the coercive force of the magnet while ensuring a small decrease in the remanence of the magnet.
[0033] The method for preparing the rare earth iron-based permanent magnetic material of the present invention comprises a coating step, a diffusion step and an annealing step, which are described in detail below.
[0034] Coating steps
[0035] The rare earth alloy is coated on the surface of the rare earth iron-based magnet to be treated to obtain the coated rare earth iron-based magnet.
[0036] In the rare earth alloy, the atomic ratio of Tb, Al, Sn, Cu and Ti is 24-58:12-18:9-16:35-45:10-18. According to a specific embodiment of the present invention, in the rare earth alloy, the atomic ratio of Tb, Al, Sn, Cu and Ti is 30-50:13-15:10-15:40-45:12-16; preferably, in the rare earth alloy, the atomic ratio of Tb, Al, Sn, Cu and Ti is 35-45:14-15:12-13:42-44:13-15. The present invention finds that controlling the atomic ratio within the above range can avoid the rare earth alloy from not undergoing eutectic reaction and improve the diffusion effect of rare earth elements. Therefore, controlling the above elements within the above range can reduce the amplitude of the decline in remanence and significantly improve the coercive force of the magnet.
[0037] The rare earth iron-based magnet to be processed includes various existing permanent magnets containing rare earth elements, which can be sintered magnets or bonded magnets. According to one embodiment of the present invention, the rare earth iron-based magnet to be processed is a sintered NdFeB magnet. Preferably, the main phase of the sintered NdFeB magnet is RE2Fe 14B, where RE is a rare earth element. RE must contain neodymium (Nd), and other rare earth elements may include lanthanum (La), cerium (Ce), praseodymium (Pr), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), scandium (Sc) and yttrium (Y).
[0038] According to one embodiment of the present invention, based on the total weight of the sintered NdFeB magnet, the components of the sintered NdFeB magnet are as follows:
[0039] Al 0.3wt%~0.5wt%, B 0.8wt%~1.0wt%, Ce 0.03wt%~0.05wt%, Co0.004wt%~0.006wt%, Cu 0.1wt%~0.2wt%, Dy 0.001wt%~0.002wt%, Ga 0.1wt%~0.3wt%, Nd 20wt%~25wt%, Pr 6wt%~8wt%, Zr 0.1wt%~0.2wt%, the balance is Fe.
[0040] According to another embodiment of the present invention, based on the total weight of the sintered NdFeB magnet, the components of the sintered NdFeB magnet are as follows:
[0041] Al 0.35wt%~0.45wt%, B 0.9wt%~1.0wt%, Ce 0.04wt%~0.05wt%, Co0.005wt%~0.006wt%, Cu 0.15wt%~0.18wt%, Dy0.0012wt%~0.0015wt%, Ga0.15wt%~0.2wt%, Nd 21wt%~23wt%, Pr 6.5wt%~7.5wt%, Zr 0.15wt%~0.18wt%, and the balance is Fe.
[0042] The present invention has found that the magnet with such a composition is particularly suitable for using the above rare earth alloy to improve its coercive force, and the remanence is slightly reduced.
[0043] The rare earth alloy is coated on the surface of the rare earth iron-based magnet to be treated to obtain a coated rare earth iron-based magnet. The coating method can be selected from at least one of co-sputtering, thermal spraying, evaporation, ion plating and screen printing. Preferably, the coating method is co-sputtering, thermal spraying, and ion plating. More preferably, the coating method is magnetron co-sputtering. This is more conducive to using the above rare earth alloy to improve the coercive force of the magnet, and the residual magnetism is reduced very little.
[0044] According to a specific embodiment of the present invention, the magnetron co-sputtering method is as follows:
[0045] The rare earth iron-based magnet to be processed is fixed on a fixture plate, and a rare earth alloy is used as a target material to deposit a rare earth alloy film on the surface of the rare earth iron-based magnet by magnetron co-sputtering. The rare earth alloy can be obtained by vacuum melting and air flow milling. No further details are given here.
[0046] According to a specific embodiment of the present invention, the rare earth alloy is in the form of particles with a particle size of 1 to 10 μm, preferably 2 to 8 μm, and more preferably 3 to 6 μm. Controlling the particle size within the above range is conducive to the volatilization of the rare earth alloy, and does not cause eutectic reaction, thereby improving the diffusion effect of the rare earth element.
[0047] According to a specific embodiment of the present invention, in the coated rare earth iron-based magnet, the thickness of the film formed by the rare earth alloy is 3-15 μm, preferably 5-12 μm, and more preferably 6-10 μm, which can reduce the amount of rare earth elements used and ensure a greater increase in coercivity.
[0048] In order to obtain the rare earth iron-based magnet to be processed, a sandblasting process can be used. The specific steps are as follows:
[0049] The rare earth iron-based blank is sandblasted to remove pollutants on the surface, and then ultrasonically cleaned in anhydrous ethanol to obtain a rare earth iron-based magnet to be treated.
[0050] The sandblasting pressure is 0.1-1.0 MPa, preferably 0.2-0.8 MPa, and more preferably 0.3-0.5 MPa; the angle between the spray gun and the surface normal of the rare earth iron-based blank is greater than or equal to 45°, preferably greater than or equal to 60°, the sandblasting trajectory is linear and the sandblasting is not repeated in the same area.
[0051] The present invention finds that the above process can ensure that the surface of the rare earth iron-based magnet to be treated is suitable for coating the rare earth alloy by magnetron co-sputtering, thereby improving the coercive force of the magnet and reducing the drop in residual magnetism.
[0052] Diffusion Steps
[0053] The coated rare earth iron-based magnet is subjected to a primary heat treatment at 600-800° C. under vacuum conditions, and then subjected to a secondary heat treatment at 850-960° C., and then cooled to obtain a heat-treated rare earth iron-based magnet.
[0054] The two heat treatments are both carried out in a vacuum furnace. The coated rare earth iron-based magnet is placed in a vacuum furnace and evacuated. The vacuum degree of the vacuum condition can be 10 to 60 Pa, preferably 15 to 50 Pa, and more preferably 20 to 45 Pa.
[0055] Start heating when the vacuum degree is 10-60 Pa. Heat up from room temperature (25°C, the same below) to the temperature of the first heat treatment at a heating rate of 2-8°C / min, preferably 3-7°C / min, and more preferably 5-6°C / min. The temperature of the first heat treatment can be 600-800°C, preferably 650-750°C, and more preferably 660-720°C. The time of the first heat treatment is 0.5-3 hours, preferably 0.8-2.5 hours, and more preferably 1-2 hours. Continue heating, at a heating rate of 2-8°C / min, preferably 3-7°C / min, and more preferably 5-6°C / min to the temperature of the second heat treatment. The temperature of the second heat treatment can be 850-960°C, preferably 900-950°C, and more preferably 880-930°C. The time of the second heat treatment can be 2-6 hours, preferably 2.5-5.5 hours, and more preferably 3-5 hours. Then cool to room temperature. By adopting such heat treatment conditions, the diffusion depth of the rare earth elements into the magnet can be controlled, thereby improving the coercive force of the magnet while avoiding the reduction of the residual magnetism.
[0056] Annealing step
[0057] The rare earth iron-based magnet after heat treatment is heat treated at 450-550° C. under vacuum conditions to obtain a rare earth iron-based permanent magnetic material.
[0058] Continue to evacuate the vacuum furnace. The vacuum degree of the vacuum condition can be 1-30Pa, preferably 5-20Pa, and more preferably 10-15Pa. Heat up from room temperature to annealing temperature at a heating rate of 2-8°C / minute, preferably 3-7°C / minute, and more preferably 5-6°C / minute. The annealing temperature can be 450-580°C, preferably 480-560°C, and more preferably 490-550°C. The annealing time can be 0.5-3 hours, preferably 1-3 hours, and more preferably 1.5-2.5 hours. Then, cool quickly to room temperature to obtain a rare earth iron-based permanent magnet material. Using such annealing conditions can ensure that the rare earth elements are evenly diffused inside the magnet, improve the coercive force of the magnet, and reduce the decline in remanence.
[0059] The heat treatment and annealing process of the present invention cooperates with the rare earth alloy of specific element composition, so as to ensure that the coercive force of the prepared permanent magnet material is greatly improved while the residual magnetism decreases slightly.
[0060] According to a specific embodiment of the present invention, compared with the rare earth iron-based magnet to be treated, the remanence of the rare earth iron-based permanent magnet material can decrease by 0.01% to 1.25%, preferably by 0.01% to 1%, and more preferably by 0.01% to 0.5%, and the coercive force can increase by 95% to 99%, preferably by 98% to 99%.
[0061] <Ingredients>
[0062] The sintered NdFeB magnets used in the following examples are N50 magnets, and the components are as follows (wt%) based on the total weight of the sintered NdFeB magnets:
[0063] Al 0.4472, B 0.9500, Ce 0.0485, Co 0.0056, Cu 0.1500, Dy 0.0012, Ga 0.1927, Nd 22.8000, Pr 7.2000, Zr 0.17580, the balance is Fe.
[0064] <Test method>
[0065] The magnetic properties of rare earth iron-based permanent magnet materials were measured using a BH magnetometer at room temperature.
[0066] The calculation of the reduction range of the residual magnetism is as follows: (the residual magnetism of the rare earth iron-based magnet to be treated-the residual magnetism of the prepared rare earth iron-based permanent magnet material) / the residual magnetism of the rare earth iron-based magnet to be treated×100%.
[0067] The increase in coercive force is calculated as follows: (coercive force of the prepared rare earth iron-based permanent magnetic material-coercive force of the rare earth iron-based magnet to be treated) / coercive force of the rare earth iron-based magnet to be treated×100%.
[0068] Example 1
[0069] The surface contaminant layer and processing oil of the rare earth iron-based magnet (sintered NdFeB magnet in this embodiment) are removed by sandblasting, and then ultrasonically cleaned in anhydrous ethanol to obtain the rare earth iron-based magnet to be processed. The sandblasting pressure is 0.4MPa, the angle between the spray gun and the surface normal of the rare earth iron-based magnet is greater than 60°, the sandblasting trajectory is linear, and the sandblasting is not repeated in the same area.
[0070] The rare earth iron-based magnet to be treated is fixed on a fixture disk, and a rare earth alloy is used as a target material. A rare earth alloy film with a thickness of 8 μm is deposited on the surface of the rare earth iron-based magnet by magnetron co-sputtering to obtain a coated rare earth iron-based magnet. In the rare earth alloy, the atomic ratio of Tb, Al, Sn, Cu and Ti is 35:15:12:43:14. A rare earth alloy with a D50 of 4.8 μm is obtained by vacuum melting and air flow milling as a target material. After testing, it is a non-eutectic rare earth alloy.
[0071] Place the coated rare earth iron-based magnet in a vacuum furnace and evacuate. Start heating when the vacuum reaches 45 Pa, and heat from room temperature to 700°C at a heating rate of 5°C / min, and heat treat at 700°C for 1 hour. Continue heating from 700°C to 925°C at a heating rate of 6°C / min, and heat treat at 925°C for 3 hours. Then cool to room temperature.
[0072] Continue to evacuate. When the vacuum degree reaches 10 Pa, start heating, raise the temperature from room temperature to 544°C at a heating rate of 5°C / min, and heat treat at 544°C for 1.5 hours. Then, quickly cool to room temperature to obtain rare earth iron-based permanent magnet material.
[0073] The performance test results of the rare earth iron-based permanent magnet material are shown in Table 1. r The decrease was 1.24%, and the coercivity H cj The improvement is 96.5%. The performance of permanent magnet material is improved from the original N52 grade to the N52SH grade.
[0074] Comparative Examples 1 to 4
[0075] Except for using other rare earth alloy targets, the rest is the same as Example 1. The composition of other rare earth alloys and the performance test results of the obtained rare earth iron-based permanent magnet materials are shown in Table 1.
[0076] Table 1. Test results of rare earth iron-based permanent magnet materials performance
[0077]
[0078] It can be seen from Table 1 that the rare earth iron-based permanent magnetic material prepared by the present invention is significantly better than the comparative example in terms of both the reduction range of remanence and the increase range of coercive force.
[0079] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.
Claims
1. A method for preparing a rare earth iron-based permanent magnetic material, comprising the following steps: 1) coating a rare earth alloy on the surface of a rare earth iron-based magnet to be treated to obtain a coated rare earth iron-based magnet; wherein the atomic ratio of Tb, Al, Sn, Cu and Ti in the rare earth alloy is 24-58:12-18:9-16:35-45:10-18; 2) heat treating the coated rare earth iron-based magnet under vacuum conditions at 600-800° C., then heat treating it at 850-960° C., and obtaining a heat-treated rare earth iron-based magnet after cooling; 3) The rare earth iron-based magnet after heat treatment is heat treated under vacuum conditions at 450-550° C. to obtain a rare earth iron-based permanent magnet material.
2. The preparation method according to claim 1, characterized in that: In the rare earth alloy, the atomic ratio of Tb, Al, Sn, Cu and Ti is 30-50:13-15:10-15:40-45:12-16.
3. The preparation method according to claim 1, characterized in that: The rare earth alloy is in the form of particles, and the particle size thereof is 1 to 10 μm.
4. The preparation method according to claim 1, characterized in that: In the coated rare earth iron-based magnet, the thickness of the film layer formed by the rare earth alloy is 3 to 15 μm.
5. The preparation method according to claim 1, characterized in that: The rare earth iron-based magnet to be processed is a sintered neodymium iron boron magnet.
6. The preparation method according to claim 5, characterized in that: The main phase of sintered NdFeB magnet is RE2Fe 14 B, where RE is a rare earth element.
7. The preparation method according to claim 6, characterized in that: Based on the total weight of the sintered NdFeB magnet, the composition of the sintered NdFeB magnet is as follows: Al 0.3wt%~0.5wt%, B 0.8wt%~1.0wt%, Ce 0.03wt%~0.05wt%, Co 0.004wt%~0.006wt%, Cu 0.1wt%~0.2wt%, Dy 0.001wt%~0.002wt%, Ga 0.1wt%~0.3wt%, Nd 20wt%~25wt%, Pr 6wt%~8wt%, Zr 0.1wt%~0.2wt%, and the balance is Fe.
8. The preparation method according to claim 1, characterized in that: The following steps are also included: The rare earth iron-based blank is sandblasted to remove pollutants on the surface, and then ultrasonically cleaned in anhydrous ethanol to obtain a rare earth iron-based magnet to be processed; The sandblasting pressure is 0.1-1.0 MPa, the angle between the spray gun and the surface normal of the rare earth iron-based blank is greater than or equal to 45°, the sandblasting trajectory is linear and the sandblasting is not repeated in the same area.
9. The preparation method according to claim 1, characterized in that: The process of coating the rare earth alloy on the surface of the rare earth iron-based magnet to be treated comprises the following steps: The rare earth iron-based magnet to be processed is fixed on a fixture disk, and a rare earth alloy is used as a target material to deposit a rare earth alloy film on the surface of the rare earth iron-based magnet by magnetron co-sputtering.
10. The preparation method according to any one of claims 1 to 9, characterized in that: Compared with the rare earth iron-based magnet to be processed, the residual magnetism of the rare earth iron-based permanent magnet material decreases by 0.01% to 1.25%, and the coercive force increases by 95% to 99%.
Citation Information
Cited By
Diffusion heat treatment method suitable for cerium-containing neodymium iron boron magnet
CN121394158A