Preparation method of isotropic neodymium iron boron bonded magnetic powder

By performing high-temperature hydrogenation disproportionation reduction reaction on neodymium iron bo alloy materials, the problems of complex equipment and poor fluidity in the existing technology are solved, and efficient production of neodymium iron bo bonded magnetic powder with good fluidity is achieved, reducing production costs and Equipment investment.

CN118919282APending Publication Date: 2024-11-08BEIJING SANJILI NEW MATERIALS CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411340603.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing production methods and equipment for isotropic NdFeB bonded magnetic powder are complex, the process control is difficult, and the flowability is poor, resulting in low output and high production costs, which limits its wide application.

Method used

By placing the heat-treated neodymium iron boron alloy material with hydrogen at high temperatures, the lattice structure of the material is nano-normal magnetic characteristics, the process route is simple, the equipment is simple, and suitable for large-scale production. .

Benefits of technology

It achieves good fluidity of magnetic powder particles, reduces the pressure requirements of the magnet pressing process, is suitable for injection molding, and has little investment in equipment, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919282A_ABST
    Figure CN118919282A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of isotropic neodymium-iron-boron bonded magnetic powder, which comprises the following steps of: performing vacuum heat treatment on an alloy to eliminate an alpha-Fe phase, so that main phase grains grow to 100-150 microns; then carrying out high-temperature hydrogen absorption treatment; then carrying out dehydrogenation treatment; further carrying out hydrogenation disproportionation reduction reaction; and performing high-pressure vacuum cooling, discharging, and grinding into powder. Hydrogen is introduced into the neodymium-iron-boron alloy subjected to heat treatment under the high-temperature condition, hydrogenation disproportionation reduction reaction occurs, the lattice structure of the material is nanocrystallized, the isotropic magnetic powder is formed, and due to the fact that the powder is close to a rock shape and good in mobility, the isotropic magnetic powder is suitable for being injected into granules or magnets.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a production method of NdFeB bonded magnetic powder, belongs to the technical field of rare earth permanent magnet application, and particularly relates to a preparation method of isotropic NdFeB bonded magnetic powder. Background Art

[0002] NdFeB bonded magnetic powder is widely used in the manufacture of magnetic components for computer hardware, household appliances, automobiles and consumer electronics because of its high resistance, convenient one-piece molding, ability to make thin-walled magnetic rings, and multi-pole magnetization.

[0003] Isotropic NdFeB bonded magnetic powder has the same physical properties in all directions of space and has a wider range of applications. Usually, isotropic NdFeB bonded magnetic powder is produced by vacuum induction rapid solidification and rapid quenching method. The equipment used in this method is complex in structure and difficult to control. The product is 0.015-0.03mm thick and thin strips. The magnetic powder is dagger-shaped after being crushed into 80 mesh. The fluidity is poor and the working pressure of the molding or injection molding equipment is high. There is also a vacuum atomization powder production method for bonded NdFeB magnetic powder with good fluidity, but the equipment capacity is small, the structure is complex, the process control is complex, the output is low, and the high production cost is an important factor restricting its application. Summary of the invention

[0004] Therefore, the present invention aims to provide a method for preparing isotropic NdFeB bonded magnetic powder, which is different from rapid quenching and atomization powder making. By introducing hydrogen into the heat-treated NdFeB alloy material under high temperature heating, the alloy material and hydrogen undergo hydrogenation disproportionation reduction reaction (HDDR), so that the material lattice structure is nano-sized to form isotropic magnetic characteristics. Because the powder shape is close to rock-like and has good fluidity, it is suitable for injection molding into pellets or injection molding into magnets.

[0005] The advantages of the present invention are:

[0006] 1) The process route of the present invention is simple, the equipment is simple, and it can be produced on a large scale with low equipment investment.

[0007] 2) The magnetic powder particles produced are rock-like and have good fluidity, and the magnet pressing process requires low pressure. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Figure 1 It is a process diagram of the HDDR technology of the present invention;

[0009] Figure 2 This is an electron microscope image of the NdFeB bonded magnetic powder prepared by the present invention. DETAILED DESCRIPTION

[0010] The technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0011] Reference Figure 1 A process flow of a method for preparing isotropic NdFeB bonded magnetic powder comprises the following steps:

[0012] Step 1: Take the principal component as RExByM Z Fe 余 The rare earth alloy material is vacuum heat treated to eliminate the α-Fe phase and grow the average grain size of the main phase to 100-150μm.

[0013] In RExByM Z Fe 余 In rare earth alloy materials, RE represents rare earth elements, including one or more metal elements selected from Nd, Pr, Y, La, Ce, Dy (neodymium, praseodymium, yttrium, lanthanum, cerium, dysprosium), B represents boron element, M represents one or more metal elements selected from Zr, Ti, Nb, Al, Ga (zirconium, titanium, niobium, aluminum, gallium), and Fe represents iron element.

[0014] The above elements are contained in the following weight percentages: x: 25-30wt%, y: 0.95-1.1wt%, z: 0-5wt%, and the balance is Fe. The present invention mainly processes this type of material.

[0015] Furthermore, before vacuum heat treatment, the furnace must be vented first. The vacuum furnace is vented at room temperature for about 60 minutes before vacuuming. The vacuuming process is accompanied by rapid temperature rise in the furnace at a rate of about 15°C / min. When the temperature rises to between 1100-1140°C, it is kept warm and the vacuum degree is maintained at <1Pa.

[0016] In this step, vacuum heat treatment is the key. The temperature of vacuum heat treatment is as high as 1100-1140℃ and the insulation time is 10-20Hr.

[0017] The purpose of vacuum heat treatment is to eliminate the α-Fe phase and control the grain size of the main phase. In the process evaluation, the α-Fe phase area is less than 0.5% and the average grain size of the main phase grows to between 100-150μm, which is considered qualified. Among them, the average grain size of the main phase is 100-150μm, which is an important feature and a condition that must be met in order to obtain bonded magnetic powder with good fluidity in the method of the present invention.

[0018] The original alloy material is a metal material with a lattice structure, and its physical properties are anisotropic. The first step is just the alloy heat treatment, which mainly eliminates the α-Fe phase and makes the grains grow. In the subsequent HDDR process, the grains are nanosized and transformed to isotropy.

[0019] Step 2: The crystallized alloy is crushed into magnetic powders less than 0.5 mm and placed in a vacuum hydrogenation furnace for high-temperature hydrogen absorption treatment.

[0020] The alloy magnetic powder after crystallization treatment absorbs hydrogen at high temperature, and a high-temperature disproportionation physical and chemical reaction will occur, as follows:

[0021] Nd2Fe14B+H2→NdHx+Fe2B+α-Fe

[0022] In this step, the alloy after vacuum heat treatment is placed in a vacuum hydrogenation furnace for high-temperature hydrogen absorption. The hydrogen absorption temperature must be maintained at 650-800°C, and the hydrogen pressure is 0.068-0.098MPa. Z Fe 余 The alloy absorbs hydrogen at high temperature to undergo a disproportionation reaction. Under a hydrogen pressure of 0.068-0.098MPa, the lattice structure changes to form nanocrystals. The hydrogen absorption time depends on the reaction situation, and the reaction is generally completed in about 180 minutes.

[0023] Step 3: Place the alloy magnetic powder after high-temperature hydrogen absorption treatment in a vacuum hydrogenation furnace for dehydrogenation treatment.

[0024] This step is also a physical and chemical reaction. Part of the hydrogen in NdHx is extracted, and the organizational structure becomes unstable.

[0025] In this step, the dehydrogenation treatment temperature should be between 800°C and 820°C, the hydrogen pressure should be between 1 and 5 KPa, and the maintenance time should be about 30 minutes.

[0026] Step 4: Hydrodisproportionation reduction reaction.

[0027] In this step, the structure of (NdHx+Fe2B+α-Fe) containing a small amount of hydrogen is extremely unstable. Continuing dehydrogenation will cause reduction and recombination. The reaction is as follows:

[0028] NdHx+Fe2B+α-Fe→Nd2Fe14B+H2

[0029] After reduction and recombination, the grains form isotropic nanocrystalline Nd2Fe14B.

[0030] This stage belongs to the vacuum reorganization stage. In this step, the disproportionation reduction temperature in the vacuum hydrogenation furnace should be 800-850℃, which is an important feature. The hydrogenation disproportionation reduction reaction time is about 60 minutes.

[0031] Step 5: High pressure vacuum cooling and taking out of the oven.

[0032] This step is to cool the vacuum hydrogenation furnace to room temperature (less than 30°C) and blow argon into the vacuum hydrogenation furnace at the same time. The argon pressure must reach 0.068-0.098MPa. After cooling, the crystalline powder is taken out and the vacuum furnace is depressurized.

[0033] Step 6: Grind the magnetic powder balls to the required mesh size to obtain the finished product.

[0034] Figure 2 This is an electron microscope image of NdFeB bonded magnetic powder obtained under an embodiment. In this embodiment, first, an alloy material containing 25wt% RE, 1wt% B, 3wt% M and the remainder Fe is subjected to vacuum heat treatment, the heating temperature is 1100°C, the holding time is 20Hr, the α-Fe phase tissue area is detected to be less than 0.5%, and the average grain size of the main phase is between 100-150μm, which meets the requirements; then the alloy material is mechanically crushed to less than 0.5mm, and placed in a vacuum hydrogenation furnace for high-temperature hydrogen absorption treatment, the hydrogen absorption temperature is maintained at 780°C, and the hydrogen pressure is 0.08MPa; after hydrogen absorption for about 1 hour, dehydrogenation is carried out, the dehydrogenation temperature is 800°C, the hydrogen pressure is 5KPa, and the dehydrogenation is completed after about 30min; then a vacuum disproportionation reduction reaction is further carried out to reorganize its organization, the disproportionation reduction temperature is 820°C, and the disproportionation reduction pressure is 5KPa; after the disproportionation reduction reaction time is about 60min, the furnace is vacuum cooled to take out the magnetic powder, and ball-milled to less than 40 mesh to become a finished product.

[0035] The following is a table of properties of two alloy magnetic powders obtained under the guidance of the process of the present invention. The table shows that the remanence (Br, unit KG), intrinsic coercive force (Hcj, unit KOe), and maximum magnetic energy product ((BH)max, unit GsKoe) of the two alloys are all very high.

[0036] alloy Br, KG Hcj,KOe (BH)max,GsKoe A 7.54 13.1 11.63 B 7.95 10.6 12.16

Claims

1. A method for preparing isotropic NdFeB bonded magnetic powder, It is characterized in that The steps include: Step 1: Take the main component as RExByMZFe 余 The alloy is vacuum heat treated to eliminate the α-Fe phase and grow the average grain size of the main phase to 100-150μm; Step 2: crush the alloy treated in step 1 into magnetic powders less than 0.5 mm, and place them in a vacuum hydrogenation furnace for high-temperature hydrogen absorption treatment; Step 3: placing the alloy magnetic powder treated in step 2 in a vacuum hydrogenation furnace for dehydrogenation treatment; Step 4: subjecting the alloy magnetic powder treated in step 3 to a hydrogenation and disproportionation reduction reaction in a vacuum hydrogenation furnace; Step 5: The alloy magnetic powder processed in step 4 is cooled under high pressure and vacuum and then taken out of the furnace; Step 6: Grind the alloy magnetic powder processed in step 5 to a size below the required mesh size to obtain the finished product.

2. The method for preparing isotropic NdFeB bonded magnetic powder according to claim 1, It is characterized in that In step 1, the vacuuming process is accompanied by heating in the furnace, which is heated to 1100-1140°C and maintained; In step 2, the hydrogen absorption temperature is 650-800°C and the hydrogen pressure is 0.068-0.098MPa; In step 3, the dehydrogenation temperature is 800°C-820°C and the hydrogen pressure is 1-5KPa; In step 4, the disproportionation reduction temperature is 800-850°C.

3. The method for preparing isotropic NdFeB bonded magnetic powder according to claim 1, It is characterized in that BYZ 余 In the alloy material, RE represents one or more metal elements selected from Nd, Pr, Y, La, Ce, and Dy, with a content of x: 25-30wt%, B represents boron element, with a content of y: 0.95-1.1wt%, M represents one or more metal elements selected from Zr, Ti, Nb, Al, and Ga, with a content of z: 0-5wt%, and the balance is Fe.

4. The method for preparing isotropic NdFeB bonded magnetic powder according to claim 1 or 2, It is characterized in that In the first step, before vacuum heat treatment, the furnace is vented and then vacuumed. The heating rate in the furnace is 15°C / min, the insulation time is 10-20Hr, and the vacuum degree is maintained at <1Pa.

5. The method for preparing isotropic NdFeB bonded magnetic powder according to claim 1, It is characterized in that In step 5, the vacuum hydrogenation furnace is cooled to room temperature, and argon gas is blown into the vacuum hydrogenation furnace at the same time, with the argon gas pressure being 0.068-0.098 MPa.

Citation Information

Cited By

  • A method for optimizing the metallographic structure of NdFeB magnets

    CN119764044A

  • A method for optimizing the metallographic structure of NdFeB magnets

    CN119764044B