Semiconductor structure etching method and semiconductor process equipment

By etching the P-type and N-type channel regions, pattern dense areas and sparse areas using specific gases and passivation gases during the etching process of Fin-FET, inhibitory by-products are generated, and the intra-trough of Fin-FET is solved. Difference in groove depth and micro-load problems in depth improve structural uniformity and performance.

CN118919410APending Publication Date: 2024-11-08BEIJING NAURA MICROELECTRONICS EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410967152.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The gap between the depth-width ratio of the trench dense area and the sparse area of ​​the Fin-FET increases, resulting in poor structural uniformity and performance, and the difference in the etching rate of the N-P channel region leads to deep microload problems.

Method used

Using an etching method of semiconductor structure, the P-type and N-type channel regions are etched by the first etching step using the first etching gas and the first passivation gas to generate and attach inhibitory by-products to reduce the Small trench depth difference; the second etching step uses the second etching gas and the second passivation gas to etch the pattern dense area and sparse area, generate and attach more by-products in the sparse area, and suppress its etching rate .

Benefits of technology

The trench depth differences in P-type and N-type channel areas and the trench depth differences in the pattern sparse and dense areas are narrowed, alleviated or eliminated the micro-load problems in N-P and I-D depths, and improved the structural uniformity and performance of Fin-FETs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919410A_ABST
    Figure CN118919410A_ABST
Patent Text Reader

Abstract

The invention discloses an etching method of a semiconductor structure and semiconductor process equipment, and the method comprises the steps: carrying out the etching of a substrate of a first channel region and a substrate of a second channel region through a first etching gas and a first passivation gas, so as to form a groove, and enabling the first passivation gas to react with the substrate of the first channel region to generate a first byproduct, the first by-product is used for being attached to the surface of the substrate of the first channel region so as to inhibit the etching rate of the substrate of the first channel region, second etching gas and second passivation gas are used for etching the substrate of the dense pattern region and the sparse pattern region so as to form a groove, the second passivation gas is used for reacting with the substrate to generate a second by-product, and the second by-product is used for generating a second by-product. The second by-product is used for being attached to the surface of the substrate, and the attachment amount of the second by-product on the surface of the substrate in the pattern sparse region is larger than that of the second by-product on the surface of the substrate in the pattern dense region, so that the etching rate of the substrate in the pattern sparse region is inhibited, and the structural uniformity and performance of semiconductor structures such as Fin-FET are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to an etching method for a semiconductor structure and semiconductor process equipment. Background Art

[0002] With the update and iteration of Fin Field-Effect Transistor (Fin-FET), the repetition period and key size of the fin of Fin-FET are continuously reduced, resulting in the continuous reduction of the trench width of the shallow trench isolation structure in the fin pattern-dense area and the continuous increase of the trench depth-to-width ratio, which leads to the continuous increase of the gap in the trench depth-to-width ratio between the fin pattern-dense area and the fin pattern-sparse area. Because the etching rate of the fin pattern-dense area is usually lower than that of the fin pattern-sparse area, the gap in the trench depth-to-width ratio between the fin pattern-dense area and the fin pattern-sparse area is continuously increasing, which in turn leads to the continuous increase of the gap in the trench depth-to-width ratio between the fin pattern-dense area and the fin pattern-sparse area, resulting in the ID (Isolation-Dense) depth micro-load problem of Fin-FET, resulting in poor structural uniformity and performance of Fin-FET.

[0003] Furthermore, in order to further improve the performance of Fin-FET, an N-type channel region with silicon (Si) material as the channel material and a P-type channel region with silicon germanium (SiGe) material as the channel material are usually formed in the substrate of Fin-FET to form N-type Fin-FET and P-type Fin-FET. However, because the etching rate of silicon germanium material is greater than the etching rate of silicon material, the gap between the depth and width of the P-type channel region and the N-type channel region will be further increased, further causing the Fin-FET to have an NP (NMOS-PMOS) deep micro-load problem, further resulting in poor structural uniformity and performance of the Fin-FET. Summary of the invention

[0004] The invention discloses an etching method for a semiconductor structure and semiconductor process equipment to improve the structural uniformity and performance of Fin-FET.

[0005] In a first aspect, the present invention discloses an etching method for a semiconductor structure, wherein the semiconductor structure comprises a substrate and a mask layer located on one side of the substrate, wherein the substrate comprises a first channel region and a second channel region, wherein the first channel region comprises a P-type channel region, and the second channel region comprises an N-type channel region, wherein the materials of the substrates of the first channel region and the second channel region are different, wherein the mask layer comprises a pattern-dense region and a pattern-sparse region, wherein the pattern density of the pattern-dense region is greater than the pattern density of the pattern-sparse region, and wherein the etching method comprises: performing a first etching step, wherein the first etching step is used to etch the substrates of the first channel region and the second channel region using a first etching gas and a first passivation gas to form a groove; wherein the first passivation gas is used to etch the substrates of the first channel region and the second channel region using a first etching gas and a first passivation gas; wherein the first passivation gas is used to etch the substrates of the first channel region and the second channel region to form a groove ... The gas is used to react with the substrate of the first channel region to generate a first by-product, and the first by-product is used to adhere to the surface of the substrate in the first channel region to suppress the etching rate of the substrate in the first channel region; a second etching step is performed, and the second etching step is used to use a second etching gas and a second passivation gas to etch the substrates in the pattern-dense region and the pattern-sparse region to form grooves; the second passivation gas is used to react with the substrate to generate a second by-product, and the second by-product is used to adhere to the surface of the substrate, and the amount of the second by-product attached to the substrate surface in the pattern-sparse region is greater than the amount of the second by-product attached to the substrate surface in the pattern-dense region to suppress the etching rate of the substrate in the pattern-sparse region.

[0006] In some embodiments, after executing the second etching step, it also includes: executing a third etching step, wherein the third etching step is used to etch the substrate to form a groove; the etching selectivity ratio of the substrate to the mask layer in the third etching step is greater than the etching selectivity ratio of the substrate to the mask layer in the second etching step or the first etching step.

[0007] In some embodiments, the performing of the third etching step includes: performing a first sub-etching step, the first sub-etching step is used to use a third etching gas to etch the by-products in the groove to remove the by-products in the groove; performing a second sub-etching step, the second sub-etching step is used to use a fourth etching gas to process the inner wall of the groove to generate a passivation layer on the inner wall surface of the groove; performing a third sub-etching step, the third sub-etching step is used to use a fifth etching gas to etch the substrate so that the depth of the groove is a first preset depth.

[0008] In some embodiments, a material of the substrate of the first channel region includes a silicon germanium material, and a material of the substrate of the second channel region includes a silicon material.

[0009] In some embodiments, the first etching gas includes at least one of fluorine-containing gas, chlorine-containing gas, bromine-containing gas, and carbon fluorine gas; the first passivation gas includes hydrofluorocarbon gas; and / or, the second etching gas includes at least one of fluorine-containing gas, chlorine-containing gas, bromine-containing gas, hydrofluorocarbon gas, and carbon fluorine gas; the second passivation gas includes at least one of hydrofluorocarbon gas, sulfur-containing gas, carbon fluorine gas, and oxygen-containing gas.

[0010] In some embodiments, the fluorine-containing gas in the first etching gas includes at least SF6 or NF3, the chlorine-containing gas includes at least Cl2, the bromine-containing gas includes at least HBr, and the carbon-fluorine-containing gas includes at least C x F y The hydrofluorocarbon gas in the first passivation gas includes at least CH x F y ; The fluorine-containing gas in the second etching gas includes at least SF6 or NF3, the chlorine-containing gas includes at least Cl2, the bromine-containing gas includes at least HBr, the carbon fluorine gas includes at least CF4, and the hydrofluorocarbon gas includes at least CHF3; the hydrofluorocarbon gas in the second passivation gas includes CH2F2 or CH3F, the sulfur-containing gas includes at least COS or SO2, the carbon fluorine gas includes at least C4F6 or C4F8, and the oxygen-containing gas includes at least O2.

[0011] In some embodiments, the proportion of the first passivation gas in the process gas of the first etching step is greater than the proportion of the first etching gas; and / or the proportion of the second passivation gas in the process gas of the second etching step is greater than the proportion of the first etching gas.

[0012] In some embodiments, the lower RF power of the second etching step is greater than the lower RF power of the first etching step.

[0013] In some embodiments, the depth of the groove formed in the first etching step is less than or equal to a second preset depth, and the second preset depth is the minimum value of the thickness of the material of the substrate of the first channel region and the thickness of the material of the substrate of the second channel region.

[0014] In a second aspect, the present invention discloses a semiconductor process equipment, including a process chamber, an air intake assembly, an upper electrode assembly, a lower electrode assembly and a controller, wherein the controller includes at least one processor and at least one memory, wherein a computer program is stored in the memory, and when the computer program is executed by the processor, an etching method as described in any one of the above items is implemented.

[0015] The semiconductor structure etching method and semiconductor process equipment disclosed in the present invention, in the process of performing the first etching step, a first etching gas and a first passivation gas are used to etch the substrate, and the first passivation gas is made to react with the substrate of the first channel region such as the P-type channel region to generate a first by-product, and the first by-product is made to cover the surface of the substrate of the first channel region such as the P-type channel region, so as to suppress the etching rate of the substrate of the first channel region such as the P-type channel region, and reduce the difference between the etching rate of the substrate of the first channel region such as the P-type channel region and the etching rate of the substrate of the second channel region such as the N-type channel region, thereby reducing the difference between the groove depth of the first channel region such as the P-type channel region and the groove depth of the second channel region such as the N-type channel region, and alleviating or eliminating the NP depth micro-load problem; in the process of performing the second etching step, the second etching gas and the second passivation gas are used to etch the substrate The bottom is etched by allowing the second passivation gas to react with the substrate to generate a second by-product, and the second by-product covers the surface of the substrate, and the amount of the second by-product attached to the substrate surface in the sparsely patterned area is greater than the amount of the second by-product attached to the substrate surface in the densely patterned area, so as to suppress the etching rate of the substrate in the sparsely patterned area and reduce the difference in etching rate between the substrate in the sparsely patterned area and the densely patterned area, thereby reducing the difference in trench depth between the first channel area such as the P-type channel area and the second channel area such as the N-type channel area, while reducing the difference in trench depth between the sparsely patterned area and the densely patterned area, thereby alleviating or eliminating the NP depth micro-load problem and the ID depth micro-load problem, thereby improving the structural uniformity and performance of semiconductor structures such as Fin-FET. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the background technology, the drawings required for use in the embodiments of the present invention or the background technology will be described below.

[0017] Figure 1 A schematic diagram of the three-dimensional structure of a fin field effect transistor.

[0018] Figure 2 It is a schematic diagram of the cross-sectional structure of a substrate with a patterned mask layer.

[0019] Figure 3 for Figure 2 Schematic diagram of the cross-sectional structure of the substrate after etching.

[0020] Figure 4 The present invention discloses a flow chart of a semiconductor structure etching method.

[0021] Figure 5 It is a schematic diagram of the cross-sectional structure of a semiconductor structure after performing a first etching step according to an embodiment of the present invention.

[0022] Figure 6 It is a schematic diagram of the cross-sectional structure of a semiconductor structure after performing a second etching step according to an embodiment of the present invention.

[0023] Figure 7 This is a TEM image of the cross-sectional structure of a semiconductor structure after only the first etching step is performed according to an embodiment of the present invention.

[0024] Figure 8 This is a TEM image of the cross-sectional structure of a semiconductor structure after only the second etching step is performed according to an embodiment of the present invention.

[0025] Fig. 9 It is a schematic diagram of the cross-sectional structure of a semiconductor structure after performing a third etching step according to an embodiment of the present invention.

[0026] Fig.10 for Figure 3 TEM image of the cross-sectional structure of the semiconductor structure shown.

[0027] Fig.11 The TEM image of the cross-sectional structure of a semiconductor structure after performing a first etching step, a second etching step and a third etching step disclosed in an embodiment of the present invention.

[0028] Fig.12 A schematic diagram of the structure of a semiconductor process equipment disclosed in an embodiment of the present invention. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0030] like Figure 1 As shown, the fin field effect transistor generally includes a substrate 1, a fin 2 protruding from the substrate 1, an oxide layer 3 located on the substrate 1, a gate insulating layer (not shown in the figure) and a gate structure 4 located on the surface of the oxide layer 3 and across the fin 2, and a source or drain 5 located on both sides of the gate structure 4 and inside any fin 2. In the process of manufacturing the fin field effect transistor, a shallow trench isolation structure needs to be formed to isolate the source or drain 5 in adjacent fins 2. Before forming the shallow trench isolation structure, the substrate 1 needs to be etched to form a plurality of trenches, wherein the portion between any two trenches is the fin 2.

[0031] In a current trench etching method, such as Figure 2As shown, after a patterned mask layer 6 is formed on the surface of the substrate 1, CF4 and CHF3 are first used as the main etching gases to etch the N-type channel region 10 with silicon material as the channel material and the P-type channel region 11 with silicon germanium material as the channel material in the substrate 1, so as to etch away the natural oxide layer on the surface of the N-type channel region 10 and the P-type channel region 11 and form a shallower groove, and then O2 is used as the reaction gas to perform surface pretreatment on the side wall of the groove to generate an oxide layer on the surface of the side wall of the groove, so as to use the oxide layer to protect the side wall of the groove to prevent it from being etched in subsequent steps, and then Cl2 or Cl2 and HBr are used as the main etching gas to continue etching the groove to form a groove with a depth that meets the requirements.

[0032] However, when etching the grooves with Cl2 or Cl2 and HBr as the main etching gas, in order to make the groove depth meet the requirements, higher upper RF power and lower RF power are used to obtain high-energy ions to bombard the surface of the substrate 1. This will result in fewer ions entering the grooves with smaller openings in the dense fin pattern area, and more ions entering the grooves with larger openings in the sparse fin pattern area, resulting in the etching rate of the dense fin pattern area being lower than the etching rate of the sparse fin pattern area. Figure 3 As shown, the difference D1 between the depth and width of the trenches in the fin pattern-dense area and the fin pattern-sparse area is large, causing the Fin-FET to have an ID depth micro-load problem, resulting in poor structural uniformity and performance of the Fin-FET.

[0033] Moreover, when the silicon material and the silicon germanium material are etched using Cl2 or Cl2 and HBr as the main etching gas, the etching rate of the silicon germanium material is greater than the etching rate of the silicon material. Figure 3 As shown, the gap D2 between the depth and width of the N-type channel region 10 using silicon material as the channel material and the P-type channel region 11 using silicon germanium material as the channel material is large, which further causes the Fin-FET to have an NP depth micro-load problem, further resulting in poor structural uniformity and performance of the Fin-FET.

[0034] Although in another trench etching method, NF3 gas is used in combination with one of N2 / O2 / CO / CO2 gases in a certain ratio, or one of CF4 / CHF3 / CH2F / CH3F gases is used in combination with one of N2 / O2 / CO / CO2 gases in a certain ratio, the etching selectivity ratio of silicon germanium to silicon is adjusted in the process of etching the GAA (Gate All around) transistor. However, the etching selectivity ratio of silicon germanium to silicon is still relatively high, that is, the etching rate of silicon germanium is still greater than the etching rate of silicon, and the difference in etching rate between silicon germanium and silicon is still relatively large, which still leads to a large gap in the depth and width of the N-type channel region 10 with silicon material as the channel material and the P-type channel region 11 with silicon germanium material as the channel material, and the NP depth micro-load problem is not alleviated or eliminated. In addition, it does not disclose how to reduce the gap in the depth and width of the grooves between the densely patterned area and the sparsely patterned area, that is, it does not disclose how to alleviate or eliminate the ID depth micro-load problem.

[0035] Based on this, the present invention discloses an etching scheme, which reduces the difference between the groove depth of the P-type channel region and the groove depth of the N-type channel region while reducing the difference between the groove depth of the sparsely-patterned region and the groove depth of the densely-patterned region by executing a first etching step and a second etching step, so as to alleviate or eliminate the NP depth micro-load problem while alleviating or eliminating the ID depth micro-load problem, thereby improving the structural uniformity and performance of semiconductor structures such as Fin-FET.

[0036] As an optional implementation of the disclosure of the present invention, an embodiment of the present invention discloses a method for etching a semiconductor structure. Figure 2 As shown, the semiconductor structure includes a substrate 1 and a mask layer 6 located on one side of the substrate 1 .

[0037] The substrate 1 includes a first channel region and a second channel region. The first channel region includes a P-type channel region 11, which can at least be used to make a P-type Fin-FET; the second channel region includes an N-type channel region 10, which can at least be used to make an N-type Fin-FET. In addition, the materials of the substrate 1 of the first channel region and the second channel region are different, or in other words, the channel materials of the first channel region and the second channel region are different. For example, the material of the substrate 1 of the P-type channel region 11 is silicon germanium, and the material of the substrate 1 of the N-type channel region 10 is silicon. It is understandable that the substrate 1 can be formed by etching a silicon substrate to form a groove and filling the groove with silicon germanium material. Figure 2 The substrate 1 is shown.

[0038] The mask layer 6 includes a pattern-dense area 60 and a pattern-sparse area 61, wherein the pattern density of the pattern-dense area 60 is greater than the pattern density of the pattern-sparse area 61. The pattern-dense area 60 corresponds to the fin pattern-dense area, and the pattern-sparse area 61 corresponds to the fin pattern-sparse area. In the process of etching the substrate 1 with the mask layer 6 as a mask to form grooves and fins, the pattern-dense area 60 will transfer the pattern to the substrate 1 to form the fin pattern-dense area, and the pattern-sparse area 61 will transfer the pattern to the substrate 1 to form the fin pattern-sparse area.

[0039] In some embodiments, the mask layer 6 includes two stacked film layers, the upper film layer includes silicon oxide, and the lower film layer includes silicon nitride. The mask layer 6 can be made by using the self-aligned quadruple patterning (SAQP) technology to make the critical dimension and opening width of the mask layer 6 smaller, so that the repetition period and critical dimension of the fin of the fin field effect transistor are smaller. Of course, the present invention is not limited to this. In other embodiments, the mask layer 6 can also include a single layer or more film layers, and the mask layer 6 can also be made of other materials or processes, which will not be repeated here.

[0040] like Figure 4 As shown, Figure 4 A flowchart of an etching method for a semiconductor structure disclosed in an embodiment of the present invention, the etching method is at least used for Figure 2 The semiconductor structure shown is etched, and the etching method includes:

[0041] S101: Execute a first etching step, which is used to etch the substrate of the first channel region and the second channel region using a first etching gas and a first passivation gas to form a groove; the first passivation gas is used to react with the substrate of the first channel region to generate a first by-product, and the first by-product is used to adhere to the surface of the substrate of the first channel region to suppress the etching rate of the substrate of the first channel region.

[0042] In the process of performing the first etching step, the first etching gas and the first passivation gas may be used to Figure 2 The substrate 1 of the semiconductor structure shown in FIG. 1 is etched to remove the natural oxide layer on the substrate 1 to form a semiconductor structure as shown in FIG. Figure 5 The trench 100 is shown having a first depth H1.

[0043] Although the etching rate of the first etching gas on the substrate 1 of the first channel region, such as the P-type channel region 11, is greater than the etching rate on the substrate 1 of the second channel region, such as the N-type channel region 10, the first passivation gas can react with the substrate 1 of the first channel region, such as the P-type channel region 11, to generate a first by-product, and the first by-product can be attached to the surface of the substrate 1 of the first channel region, such as the P-type channel region 11. Therefore, the etching rate of the substrate 1 of the first channel region, such as the P-type channel region 11, can be suppressed, thereby reducing the difference in etching rate between the substrate 1 of the first channel region, such as the P-type channel region 11, and the substrate 1 of the second channel region, such as the N-type channel region 10, thereby reducing the difference in depth between the trench 100 of the first channel region, such as the P-type channel region 11, and the trench 100 of the second channel region, such as the N-type channel region 10, thereby alleviating or eliminating the NP depth micro-load problem, thereby improving the structural uniformity and performance of semiconductor structures such as Fin-FET.

[0044] S102: Execute a second etching step, which is used to use a second etching gas and a second passivation gas to etch the substrate in the pattern-dense area and the pattern-sparse area to form a groove; the second passivation gas is used to react with the substrate to generate a second by-product, and the second by-product is used to adhere to the surface of the substrate, and the amount of the second by-product attached to the substrate surface in the pattern-sparse area is greater than the amount of the second by-product attached to the substrate surface in the pattern-dense area, so as to suppress the etching rate of the substrate in the pattern-sparse area.

[0045] In the process of performing the second etching step, a second etching gas and a second passivation gas may be used to Figure 5 The substrate 1 shown in FIG. 1 is etched so that the depth of the groove 100 is the second depth. In the case where the first etching step is performed first and the second etching step is performed later, the following is formed: Figure 6 The trench 100 is shown having a second depth H2 that is greater than the first depth H1.

[0046] Although the etching rate of the second etching gas on the substrate 1 in the sparse pattern area 61 is greater than the etching rate on the substrate 1 in the dense pattern area 60, the second passivation gas can react with the substrate 1 to generate a second by-product, and the second by-product can be attached to the surface of the substrate 1, and the amount of the second by-product attached to the surface of the substrate 1 in the sparse pattern area 61 is greater than the amount of the second by-product attached to the surface of the substrate 1 in the dense pattern area 30. Therefore, the etching rate of the substrate 1 in the sparse pattern area 61 can be suppressed, and the etching rate of the substrate 1 in the sparse pattern area 61 can be reduced. The difference in etching rate of the substrate 1 in the pattern-dense area 60 can be reduced while the difference in depth of the groove 100 in the first channel area such as the P-type channel area 11 and the second channel area such as the N-type channel area 10 can be reduced. At the same time, the difference in depth of the groove 100 in the pattern-sparse area 61 and the depth of the groove 100 in the pattern-dense area 60 can be reduced, thereby alleviating or eliminating the NP depth micro-load problem while alleviating or eliminating the ID depth micro-load problem, thereby improving the structural uniformity and performance of semiconductor structures such as Fin-FET.

[0047] It should be noted that, although the difference in etching rate between the substrate 1 in the sparsely patterned area 61 and the substrate 1 in the densely patterned area 60 in the first etching step will also affect the difference in depth between the trench 100 in the first channel area, such as the P-type channel area 11, and the trench 100 in the second channel area, such as the N-type channel area 10, Figure 5 As shown, the difference between the etching rate of the substrate 1 in the sparsely patterned area 61 and the etching rate of the substrate 1 in the densely patterned area 60 is still relatively large; however, because the difference between the etching rate of the substrate 1 in the sparsely patterned area 61 and the etching rate of the substrate 1 in the densely patterned area 60 will be reduced in the second etching step, the influence of the difference between the etching rate of the substrate 1 in the sparsely patterned area 61 and the etching rate of the substrate 1 in the densely patterned area 60 may be ignored in the first etching step.

[0048] It should also be noted that, in some embodiments, the first etching step can stop at the material of the substrate 1 of the first channel region, such as the P-type channel region 11, or the bottom of the channel material. Because the material of the substrate 1 at the bottom of the first channel region, such as the P-type channel region 11, is the same as the material of the substrate 1 at the bottom of the second channel region, such as the N-type channel region 10, it is not necessary to consider the impact of the different materials of the substrate 1 or the channel material on the etching rate, and the second etching step can be used to reduce the difference in the depth of the groove 100 in the sparsely patterned region 61 and the depth of the groove 100 in the densely patterned region 60.

[0049] That is, in some embodiments, the depth of the groove formed in the first etching step is less than or equal to the second preset depth, and the second preset depth is the minimum value of the thickness of the material of the substrate of the first channel region and the thickness of the material of the substrate of the second channel region. Figure 5 As shown, the depth of the trench formed in the first etching step is less than or equal to the thickness D of the material of the substrate of the P-type channel region 11 .

[0050] Of course, the present invention is not limited to this. In other embodiments, the etching stop position or etching stop time of the first etching step can be determined according to the difference between the depth of the groove 100 of the first channel region, such as the P-type channel region 11, and the depth of the groove 100 of the second channel region, such as the N-type channel region 10, so as to minimize the difference. Among them, the first etching step can be stopped at any position of the material of the substrate 1 or the channel material of the first channel region, such as the P-type channel region 11. In addition, the etching stop position or etching stop time of the second etching step can be determined according to the actual etching requirements.

[0051] In some embodiments of the present invention, the material of the substrate 1 of the first channel region, such as the P-type channel region 11, includes a silicon germanium material, and the material of the substrate 1 of the second channel region, such as the N-type channel region 10, includes a silicon material. Of course, the present invention is not limited thereto, and in other embodiments, the first channel region, such as the P-type channel region 11, and the second channel region, such as the N-type channel region 10, may also be other different materials, which will not be described in detail herein.

[0052] In some embodiments of the present invention, the first etching gas includes at least one of a fluorine-containing gas, a chlorine-containing gas, a bromine-containing gas, and a fluorine-containing gas, wherein the fluorine-containing gas includes at least SF6 or NF3, the chlorine-containing gas includes at least Cl2, the bromine-containing gas includes at least HBr, and the fluorine-containing gas includes at least C x F y The first passivation gas includes a hydrofluorocarbon gas. The hydrofluorocarbon gas includes at least CH x F y .

[0053] In some embodiments, during the first etching step, the substrate 1 may be etched using a process gas including an inert gas, a first etching gas, and a first passivation gas, wherein the inert gas includes at least one of N2, Ar, and He. In some embodiments, the total flow rate of the mixed gas is 300 sccm to 600 sccm. In some embodiments, the proportion of the first passivation gas is greater than or equal to the proportion of the first etching gas. In some embodiments, the proportion of the first etching gas is 5% to 15%, and the proportion of the first passivation gas is 5% to 30%.

[0054] In some embodiments, during the first etching step, the pressure of the process chamber is 5mT to 40mT, so as to desorb the byproducts in the etching process in time and obtain better morphology and uniformity. In some embodiments, during the first etching step, the upper RF power fed into the process chamber by the upper RF power supply is 300W to 1000W, and the lower RF power fed into the process chamber by the lower RF power supply is 50W to 400W, so as to improve the etching selectivity of the depth direction and the width direction of the groove 100. Among them, the upper RF power supply works in the continuous wave mode, and the frequency of the continuous wave output is 13.56MHz; the lower RF power supply works in the pulse wave mode, and the frequency of the pulse wave output is 13.56MHz, and the duty cycle is 5% to 60%. In some embodiments, during the first etching step, the temperature of the electrostatic chuck is 30℃ to 60℃.

[0055] It should be noted that, because Ge is more likely to react with the first etching gas such as Cl2 / HBr to form volatile GeCl4 / GeBr4 byproducts than Si, the first etching gas has a higher etching rate for SiGe in the first channel region such as the P-type channel region 11 than for Si in the second channel region such as the N-type channel region 10. x F y After ignition, gaseous *CH x F y Free radicals, and the Ge-F chemical bond has a smaller chemical bond strength than the Si-F chemical bond, that is, *CH x F y Free radicals are more likely to combine with Ge to form Ge*CH x F y The first byproducts will be attached to the surface of SiGe in the first channel region, such as the P-type channel region 11, to form a passivation layer, so the etching rate of the first etching gas on the first channel region, such as the P-type channel region 11, can be suppressed. In addition, since the formation of Ge-H chemical bonds will induce Si to be enriched on the surface of SiGe in the first channel region, such as the P-type channel region 11, the etching rate of the first etching gas on the first channel region, such as the P-type channel region 11, can also be suppressed.

[0056] In some embodiments, after performing the first etching step, Figure 7 As shown, the depths of the Si trench and the SiGe trench are almost the same, indicating that the etching selectivity ratio of Si / SiGe is almost equal to 1, indicating that the first etching step can achieve the same rate etching of Si and SiGe. It should be noted that by adjusting the gas ratio of the first etching gas to the first passivation gas, the ratio of the etching rate of SiGe in the first channel region, such as the P-type channel region 11, to the etching rate of Si in the second channel region, such as the N-type channel region 10, can be adjusted.

[0057] In some embodiments, if only the first etching step is performed or the first etching step is performed first and then the second etching step, the etching rate of SiGe in the first channel region such as the P-type channel region 11 in the first etching step can be equal to the etching rate of Si in the second channel region such as the N-type channel region 10, so that the etching depth of SiGe in the first channel region such as the P-type channel region 11 in the first etching step is equal to the etching depth of Si in the second channel region such as the N-type channel region 10.

[0058] In other embodiments, if the second etching step is performed before the first etching step, because the etching depth of SiGe in the first channel region such as the P-type channel region 11 will be greater than the etching depth of Si in the second channel region such as the N-type channel region 10 during the execution of the second etching step, when the first etching step is performed, the etching rate of SiGe in the first channel region such as the P-type channel region 11 can be made lower than the etching rate of Si in the second channel region such as the N-type channel region 10, so as to ultimately achieve that the etching depth of SiGe in the first channel region such as the P-type channel region 11 is equal to the etching depth of Si in the second channel region such as the N-type channel region 10.

[0059] It should be noted that the embodiment of the present invention does not limit the execution order of the first etching step and the second etching step. However, if the second etching step is performed before the first etching step, it is necessary to ensure that after the second etching step or when the first etching step is performed, there are still different channel materials such as silicon material and silicon germanium material in the substrate 1.

[0060] In some embodiments of the present invention, the second etching gas includes at least one of fluorine-containing gas, chlorine-containing gas, bromine-containing gas, hydrofluorocarbon gas, and carbon fluorine gas, wherein the fluorine-containing gas includes at least SF6 or NF3, the chlorine-containing gas includes at least Cl2, the bromine-containing gas includes at least HBr, the carbon fluorine gas includes at least CF4, and the hydrofluorocarbon gas includes at least CHF3. The second passivation gas includes at least one of hydrofluorocarbon gas, sulfur-containing gas, carbon fluorine gas, and oxygen-containing gas, wherein the hydrofluorocarbon gas includes CH2F2 or CH3F, the sulfur-containing gas includes at least COS or SO2, the carbon fluorine gas includes at least C4F6 or C4F8, and the oxygen-containing gas includes at least O2.

[0061] In some embodiments, during the second etching step, the substrate 1 may be etched using a process gas including an inert gas, a second etching gas, and a second passivation gas, wherein the inert gas includes at least one of N2, Ar, and He. In some embodiments, the total flow rate of the mixed gas is 300 sccm to 600 sccm. In some embodiments, the proportion of the second passivation gas is greater than or equal to the proportion of the second etching gas. In some embodiments, the proportion of the second etching gas is 5% to 15%, and the proportion of the second passivation gas is 10% to 35%.

[0062] In some embodiments, during the second etching step, the pressure of the process chamber is 5mT to 40mT, so as to desorb the byproducts in the etching process in time and obtain better morphology and uniformity. In some embodiments, during the second etching step, the upper RF power fed into the process chamber by the upper RF power supply is 300W to 1000W, and the lower RF power fed into the process chamber by the lower RF power supply is 300W to 800W, so as to improve the etching selectivity of the depth direction and the width direction of the groove 100. In some embodiments, the lower RF power of the second etching step is greater than the lower RF power of the first etching step, so as to assist in reducing the difference between the depth of the groove 100 in the sparse pattern area 61 and the depth of the groove 100 in the dense pattern area 60.

[0063] Although the groove width of the sparsely-patterned area 61 is greater than that of the densely-patterned area 60, the amount of second etching gas entering the groove of the sparsely-patterned area 61 is greater than that of the densely-patterned area 60, so that the etching rate of the second etching gas on the substrate 1 in the sparsely-patterned area 61 is greater than that on the substrate 1 in the densely-patterned area 60. However, because the second passivating gas can react with Si and SiGe to generate heavier second by-products that are easy to deposit, and when the groove width of the sparsely-patterned area 61 is greater than that of the densely-patterned area 60, the amount of the second by-products attached to the surface of the substrate 1 in the sparsely-patterned area 61 will be greater than the amount of the second by-products attached to the surface of the substrate 1 in the densely-patterned area 30. Therefore, the etching rate of the second etching gas on the substrate 1 in the sparsely-patterned area 61 can be suppressed.

[0064] In some embodiments, only after the second etching step is performed, Figure 8 As shown, the depth of the groove 100 in the pattern-dense area 60 of the first channel region such as the P-type channel region 11 and the second channel region such as the N-type channel region 10 is deeper than the depth of the groove 100 in the pattern-sparse area 61, indicating that the second etching step can make the etching rate of the substrate 1 in the pattern-dense area 60 greater than the etching rate of the substrate 1 in the pattern-sparse area 61. It should be noted that by adjusting the gas ratio of the second etching gas to the second passivation gas, the ratio of the etching rate of the substrate 1 in the pattern-dense area 60 to the pattern-sparse area 61 can be adjusted.

[0065] In some embodiments, if only the second etching step is performed or the second etching step is performed first and then the first etching step, the etching rate of the substrate 1 in the graphic dense area 60 in the second etching step can be made equal to the etching rate of the substrate 1 in the graphic sparse area 61, so that the etching depth of the substrate 1 in the graphic dense area 60 is equal to the etching depth of the substrate 1 in the graphic sparse area 61.

[0066] In other embodiments, if the first etching step is performed before the second etching step, because the etching depth of the substrate 1 in the graphic dense area 60 will be less than the etching depth of the substrate 1 in the graphic sparse area 61 during the execution of the first etching step, when the second etching step is performed, the etching rate of the substrate 1 in the graphic dense area 60 can be made greater than the etching rate of the substrate 1 in the graphic sparse area 61, so as to ultimately achieve the etching depth of the substrate 1 in the graphic dense area 60 being equal to the etching depth of the substrate 1 in the graphic sparse area 61.

[0067] Based on any of the above embodiments, in some embodiments of the present invention, after performing the second etching step, a third etching step may be performed, and the third etching step is used to etch the substrate 1 to form a groove. In the case where the first etching step, the second etching step and the third etching step are performed in sequence, Fig. 9 As shown, the third depth H3 is greater than the second depth H2. The etching selectivity ratio of the substrate to the mask layer in the third etching step is greater than the etching selectivity ratio of the substrate to the mask layer in the second etching step or the first etching step. Based on this, by performing the third etching step, not only can the groove 100 be formed into a more vertical morphology, but also the depth of the groove 100 can reach the target depth faster.

[0068] In some embodiments, executing the third etching step includes executing a first sub-etching step, a second sub-etching step, and a third sub-etching step in sequence, wherein the first sub-etching step is used to use a third etching gas to etch the by-products in the groove 100 to remove the by-products in the groove 100; the second sub-etching step is used to use a fourth etching gas to process the inner wall of the groove 100 to generate a passivation layer on the inner wall surface of the groove 100 to protect the inner wall of the groove 100 from being etched, so that the groove 100 forms a more vertical morphology while ensuring that the size of the fins between the grooves 100 meets the requirements; the third sub-etching step is used to use a fifth etching gas to etch the substrate 1 so that the depth of the groove 100 is a first preset depth such as a third depth H3.

[0069] In some embodiments, the main parameters of the process recipe of the first sub-etching step are as follows: the pressure of the process chamber is 5mT to 60mT, the upper RF power is 200W to 800W, the lower RF power is 50W to 200W, the electrostatic chuck temperature is 30°C to 60°C, and the third etching gas includes a hydrofluorocarbon gas, which includes at least one of CH2F2, CH3F and CHF3. In some embodiments, the proportion of CH3F can be 10% to 20%, and the proportion of CHF3 can be 10% to 20%. In some embodiments, the process gas of the first sub-etching step can also include an inert gas, which can include a mixed gas of Ar and He. In some embodiments, the total flow rate of the process gas of the first sub-etching step is 300sccm to 600sccm.

[0070] The main parameters of the process recipe of the second sub-etching step are as follows: the pressure of the process chamber is 5mT to 100mT, the upper RF power is 600W to 1500W, the lower RF power is 0W, the electrostatic chuck temperature is 30°C to 60°C, and the fourth etching gas includes an oxygen-containing gas, and the oxygen-containing gas includes O2. In some embodiments, the process gas of the second sub-etching step may also include an inert gas, and the inert gas may include a mixed gas of Ar and He. In some embodiments, the proportion of O2 is 40% to 80%, and the proportion of inert gas is 20% to 60%. In some embodiments, the total flow rate of the process gas of the second sub-etching step is 300sccm to 500sccm.

[0071] The main parameters of the process recipe of the third sub-etching step are as follows: the pressure of the process chamber is 10mT~80mT, the upper RF power is 250W~800W, the lower RF power is 300W~1400W, the electrostatic chuck temperature is 30℃~60℃, and the fifth etching gas includes at least one of a chlorine-containing gas and a bromine-containing gas, the chlorine-containing gas includes Cl2, and the bromine-containing gas includes HBr. In some embodiments, the proportion of Cl2 is 50%~80%, and the proportion of HBr is 10%~30%. In some embodiments, the process gas of the third sub-etching step may also include an inert gas, which may include a mixed gas of Ar and He. In some embodiments, the total flow rate of the process gas of the second sub-etching step is 600sccm~1000sccm.

[0072] It should be noted that, although the etching rate of the substrate 1 of the first channel region such as the P-type channel region 11 in the third sub-etching step is greater than the etching rate of the substrate 1 of the second channel region such as the N-type channel region 10, the etching rate of the substrate 1 of the first channel region such as the P-type channel region 11 in the first etching step can be made lower than the etching rate of the substrate of the second channel region such as the N-type channel region 10, so that the depth of the trench 100 of the P-type channel region 11 is equal to the depth of the trench 100 of the N-type channel region 10.

[0073] Although the etching rate of the substrate 1 in the graphic dense area 60 in the third sub-etching step is lower than the etching rate of the substrate 1 in the graphic sparse area 61, the etching rate of the substrate 1 in the graphic dense area 60 in the second etching step can be made higher than the etching rate of the substrate 1 in the graphic sparse area 61 to make the depth of the groove 100 in the graphic dense area 60 equal to the depth of the groove 100 in the graphic sparse area 61.

[0074] That is, in some embodiments, in the third etching step, the etching rate of the substrate in the first channel region is greater than the etching rate of the substrate in the second channel region, and the etching rate of the substrate in the pattern-dense region is less than the etching rate of the substrate in the pattern-sparse region; and / or, in the first etching step, the etching rate of the substrate in the first channel region is less than the etching rate of the substrate in the second channel region; and / or, in the second etching step, the etching rate of the substrate in the pattern-dense region is greater than the etching rate of the substrate in the pattern-sparse region.

[0075] Of course, the present invention is not limited to this. In other embodiments, in the first etching step, the etching rate of the substrate in the first channel region may also be equal to the etching rate of the substrate in the second channel region; in the second etching step, the etching rate of the substrate in the pattern-dense region may also be equal to the etching rate of the substrate in the pattern-sparse region.

[0076] It can be understood that, in the case where the first etching step makes the etching depth of the substrate 1 of the first channel region, such as the P-type channel region 11, equal to the etching depth of the substrate 1 of the second channel region, such as the N-type channel region 10, and / or the second etching step makes the etching depth of the substrate 1 of the pattern-dense region 60 equal to the etching depth of the substrate 1 of the pattern-sparse region 61, although the etching rate of the substrate 1 of the first channel region, such as the P-type channel region 11, is greater than the etching rate of the substrate 1 of the second channel region, such as the N-type channel region 10, and the etching rate of the substrate 1 of the pattern-dense region 60 is greater than the etching rate of the substrate 1 of the second channel region, such as the N-type channel region 10, 0 is less than the etching rate of the substrate 1 in the sparsely patterned area 61; however, because the etching depth of the substrate 1 in the third sub-etching step is thinner, the influence of the third sub-etching step on the difference of the groove 100 is smaller, and the difference in the depth of the groove 100 in the first channel area such as the P-type channel area 11 and the second channel area such as the N-type channel area 10 can still be reduced while reducing the difference in the depth of the groove 100 in the sparsely patterned area 61 and the depth of the groove 100 in the densely patterned area 60.

[0077] It should be noted that the execution order of the first etching step, the second etching step and the third etching step is not limited in the embodiment of the present invention. The first etching step, the second etching step and the third etching step can be performed in sequence, or the second etching step, the first etching step and the third etching step can be performed in sequence, or the first etching step, the third etching step and the second etching step can be performed in sequence. However, it is necessary to ensure that when the first etching step is performed, there are still different channel materials such as silicon material and silicon germanium material in the substrate 1. In addition, in the embodiment of the present invention, the number of executions of the first etching step, the second etching step and the third etching step is not limited. For example, the third etching step can be performed multiple times so that the etching depth of the groove 100 reaches the target depth. Of course, when the third etching step is performed multiple times, the proportion of the fifth etching gas can be adjusted to achieve a higher etching selectivity while also making the morphology of the groove 100 more vertical.

[0078] like Fig.10 and Fig.11 As shown, Fig.10 for Figure 3 TEM image of the structure shown, Fig.11 for Fig. 9 TEM image of the structure shown, and Fig.10 compared to, Fig.11 The morphology of the groove 100 is more vertical, the difference between the depth of the groove 100 in the first channel region such as the P-type channel region 11 and the depth of the groove 100 in the second channel region such as the N-type channel region 10 is smaller, and the difference between the depth of the groove 100 in the sparsely patterned region 61 and the depth of the groove 100 in the densely patterned region 60 is also smaller.

[0079] As another optional implementation of the content disclosed in the present invention, the embodiment of the present invention further discloses a semiconductor process equipment, such as Fig.12 As shown, the semiconductor process equipment includes a process chamber 10, an air intake assembly, an exhaust assembly, an upper electrode assembly, a lower electrode assembly, and a control device, etc. The control device includes at least one memory and at least one processor, the memory stores a computer program, and the processor executes the computer program to implement the etching method disclosed in any of the above embodiments.

[0080] The gas inlet assembly is used to introduce gas into the process chamber 10, and the gas includes process gases such as etching gas and passivation gas. The control device is used to control the opening or closing of the electronic valve of the gas inlet assembly to control the gas inlet assembly to start or stop introducing gas into the process chamber 10. The exhaust assembly is used to extract the gas in the process chamber 10, and the gas includes byproduct gas generated after the etching reaction. The control device can also be used to control the opening or closing of the electronic valve of the exhaust assembly to control the exhaust assembly to start or stop extracting the gas in the process chamber 10. In addition, the control device can also be used to control the valve size of the electronic valve of the gas inlet assembly and the valve size of the electronic valve of the exhaust assembly to control the chamber pressure of the process chamber 10.

[0081] The upper electrode assembly includes an upper RF power supply 16, a first matcher 17 electrically connected to the upper RF power supply 16, and an RF coil 18 electrically connected to the first matcher 17. The upper RF power supply 16 can be electrically connected to the RF coil 18 in the process chamber 10 through the first matcher 17, and is used to load RF power to the RF coil 18, so that the RF coil 18 couples the RF power into the process chamber 10 through the dielectric window 19, and ionizes the gas in the process chamber 10 into plasma 20. The control device can also be used to control the RF power level loaded by the upper RF power supply 16 to the RF coil 18 through the first matcher 17.

[0082] The lower electrode assembly includes a lower RF power supply 21, a second matcher 22 electrically connected to the lower RF power supply 21, and a carrier device electrically connected to the second matcher 22, and the carrier device includes an electrostatic chuck 11, etc. The lower RF power supply 21 is electrically connected to the carrier device through the second matcher 22, and is used to apply bias power to the carrier device to accelerate the plasma. The carrier device is used to carry the substrate 13 and heat or cool the substrate 13.

[0083] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0084] The above embodiments only express several implementation methods of this specification, and the descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of this specification, which all belong to the protection scope of this specification. Therefore, the protection scope of the patent of this specification shall be based on the attached claims.

Claims

1. A method for etching a semiconductor structure, characterized in that: The semiconductor structure includes a substrate and a mask layer located on one side of the substrate, the substrate includes a first channel region and a second channel region, the first channel region includes a P-type channel region, the second channel region includes an N-type channel region, the first channel region and the second channel region have different substrate materials, the mask layer includes a pattern-dense region and a pattern-sparse region, the pattern density of the pattern-dense region is greater than the pattern density of the pattern-sparse region, and the etching method includes: Performing a first etching step, wherein the first etching step is used to etch the substrates of the first channel region and the second channel region using a first etching gas and a first passivation gas to form grooves; the first passivation gas is used to react with the substrate of the first channel region to generate a first by-product, and the first by-product is used to adhere to the surface of the substrate of the first channel region to suppress the etching rate of the substrate of the first channel region; A second etching step is performed, wherein the second etching step is used to etch the substrate in the pattern-dense area and the pattern-sparse area using a second etching gas and a second passivation gas to form a groove; the second passivation gas is used to react with the substrate to generate a second by-product, and the second by-product is used to adhere to the surface of the substrate, and the adhesion amount of the second by-product on the substrate surface in the pattern-sparse area is greater than the adhesion amount of the second by-product on the substrate surface in the pattern-dense area, so as to suppress the etching rate of the substrate in the pattern-sparse area.

2. The etching method according to claim 1, characterized in that: After performing the second etching step, the method further comprises: A third etching step is performed, wherein the third etching step is used to etch the substrate to form a groove; in the third etching step, the etching selectivity ratio of the substrate to the mask layer is greater than the etching selectivity ratio of the substrate to the mask layer in the second etching step or the first etching step.

3. The etching method according to claim 2, characterized in that: The performing of the third etching step comprises: Performing a first sub-etching step, wherein the first sub-etching step is used to etch the by-products in the groove using a third etching gas to remove the by-products in the groove; Performing a second sub-etching step, wherein the second sub-etching step is used to process the inner wall of the groove using a fourth etching gas to form a passivation layer on the inner wall surface of the groove; A third sub-etching step is performed, where the third sub-etching step is used to etch the substrate using a fifth etching gas so that the depth of the groove is a first preset depth.

4. The etching method according to claim 1, characterized in that: The material of the substrate of the first channel region includes silicon germanium material, and the material of the substrate of the second channel region includes silicon material.

5. The etching method according to claim 4, characterized in that: The first etching gas includes at least one of fluorine-containing gas, chlorine-containing gas, bromine-containing gas, and carbon-fluorine gas; the first passivation gas includes hydrofluorocarbon gas; and / or, The second etching gas includes at least one of fluorine-containing gas, chlorine-containing gas, bromine-containing gas, hydrofluorocarbon gas, and carbon fluorine gas; the second passivation gas includes at least one of hydrofluorocarbon gas, sulfur-containing gas, carbon fluorine gas, and oxygen-containing gas.

6. The etching method according to claim 5, characterized in that: The fluorine-containing gas in the first etching gas includes at least SF6 or NF3, the chlorine-containing gas includes at least Cl2, the bromine-containing gas includes at least HBr, and the carbon-fluorine-containing gas includes at least C x F y The hydrofluorocarbon gas in the first passivation gas includes at least CH x F y ; The fluorine-containing gas in the second etching gas includes at least SF6 or NF3, the chlorine-containing gas includes at least Cl2, the bromine-containing gas includes at least HBr, the carbon fluorine gas includes at least CF4, and the hydrofluorocarbon gas includes at least CHF3; the hydrofluorocarbon gas in the second passivation gas includes CH2F2 or CH3F, the sulfur-containing gas includes at least COS or SO2, the carbon fluorine gas includes at least C4F6 or C4F8, and the oxygen-containing gas includes at least O2.

7. The etching method according to claim 5 or 6, characterized in that: The proportion of the first passivation gas in the process gas of the first etching step is greater than the proportion of the first etching gas; and / or the proportion of the second passivation gas in the process gas of the second etching step is greater than the proportion of the first etching gas.

8. The etching method according to claim 4, characterized in that: The lower RF power of the second etching step is greater than the lower RF power of the first etching step.

9. The etching method according to claim 1, characterized in that: The depth of the groove formed in the first etching step is less than or equal to a second preset depth, and the second preset depth is the minimum value of the thickness of the material of the substrate of the first channel region and the thickness of the material of the substrate of the second channel region.

10. A semiconductor process equipment, characterized in that: It includes a process chamber, an air intake assembly, an upper electrode assembly, a lower electrode assembly and a controller. The controller includes at least one processor and at least one memory. A computer program is stored in the memory. When the computer program is executed by the processor, the etching method according to any one of claims 1 to 9 is implemented.