Semiconductor package, method of forming same, and method of forming dummy die
By using a 30W/mK to 100W/mK thermal conductivity adjustment layer and bonding film structure in semiconductor packaging technology, combined with cutting groove and protective layer technology, the problem of insufficient thermal conductivity and warpage control in the package is solved. Improves the heat dissipation performance and bonding quality of the package.
Patent Information
- Application Number
- CN202410900654.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-10-30
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing semiconductor packaging technology, thermal conductivity and warpage control are insufficient, which affects the heat dissipation performance and bonding quality of the package.
Using an adjustment layer and bonding film structure with a thermal conductivity of 30W/mK to 100W/mK, the adjustment layer and bonding film are deposited on the semiconductor substrate, and a cutting groove and a protective layer are formed on the substrate, combined with backside grinding. and extend the process to form an improved pseudo-die to improve thermal conductivity and warpage control.
The heat dissipation performance and bonding quality of the package are significantly improved, and the heat transfer and bonding strength between the pseudo-die and other dies are enhanced.
Smart Images

Figure CN118919502A_ABST
Abstract
Description
Technical Field
[0001] Embodiments of the present application relate to a semiconductor package and a method of forming the same, and a method of forming a dummy die. Background Art
[0002] Semiconductor devices are used in a variety of electronic applications, such as personal computers, cell phones, digital cameras, and other electronic devices, as examples. Semiconductor devices are typically manufactured by sequentially depositing insulating or dielectric layers, conductive layers, and semiconductor material layers over a semiconductor substrate, and patterning the various material layers using photolithography to form circuit components and elements thereon. Tens or hundreds of integrated circuits are typically manufactured on a single semiconductor wafer, and the individual dies on the wafer are separated by sawing along scribe lines between the integrated circuits. For example, the individual dies are typically packaged individually in a multi-chip module or other type of package.
[0003] Three-dimensional integrated circuits (3DICs) are a relatively new development in semiconductor packaging in which multiple semiconductor dies are stacked on top of each other, such as package-on-package (PoP) and system-in-package (SiP) packaging technologies. 3DICs can provide improved integration density and other advantages, such as faster speeds and higher bandwidth, as examples, because the length of the interconnects between the stacked dies is reduced. Summary of the invention
[0004] Some embodiments of the present application provide a semiconductor package, comprising: a first die having a first bonding film; a second die stacked above the first die and bonded to the first die via the first bonding film; and a dummy die stacked above the first die and bonded to the first die via the first bonding film, wherein the dummy die comprises: a substrate; an adjustment layer formed above the substrate, wherein the adjustment layer has a thermal conductivity in a range between 30 W / mK and 100 W / mK; and a second bonding film formed above the adjustment layer, wherein the second bonding film is bonded to the first bonding film.
[0005] Other embodiments of the present application provide a method for forming a semiconductor package, comprising: bonding a first die to a second die, wherein the first die includes a first bonding film, and the second die is bonded to the first bonding film; and bonding a dummy die to the first die, wherein the dummy die includes: a substrate; an adjustment layer formed above the substrate, wherein the adjustment layer has a thermal conductivity in a range between 30 W / mK and 100 W / mK; and a second bonding film formed above the adjustment layer, and the first bonding film is bonded to the second bonding film.
[0006] Still other embodiments of the present application provide a method for forming a dummy die, comprising: depositing an adjustment layer on the front side of a semiconductor substrate; depositing a bonding film on the adjustment layer; forming a cutting pattern above the bonding film; using the cutting pattern to etch through the bonding film, the adjustment layer and into the semiconductor substrate to form a cutting groove; depositing a protective layer in the cutting groove and on the bonding film; attaching a carrier wafer to the protective layer; and grinding the semiconductor substrate from the back side to expose the protective layer in the cutting groove. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] When read in conjunction with the accompanying drawings, various aspects of the disclosed embodiments can be best understood from the following detailed description. It should be noted that, in accordance with standard practice in the industry, the various components are not drawn to scale. In fact, for clarity of discussion, the size of the various components may be arbitrarily increased or reduced.
[0008] Figure 1 is a flow chart of forming a dummy die according to an embodiment of the present disclosure.
[0009] Figures 2 to 8 , 9A to 9E and Fig.10 Various processing stages during dummy die fabrication according to an embodiment of the present disclosure are schematically illustrated.
[0010] Fig.11 Improved thermal conductivity in a dummy die according to an embodiment of the present disclosure is shown.
[0011] Fig. 12A and Fig. 12B Improved warpage control in a dummy die according to an embodiment of the present disclosure is schematically illustrated.
[0012] Fig.13 is a flow chart of forming an integrated circuit package according to an embodiment of the present disclosure.
[0013] Fig.14 , Fig.15 , FIG. 16A to FIG. 16C , FIG. 17A to FIG. 17B and Figures 18 to 21 Various processing stages during the fabrication of an integrated circuit package according to an embodiment of the present disclosure are schematically illustrated.
[0014] Fig. 22 is a flow chart of forming an integrated circuit package according to an embodiment of the present disclosure.
[0015] FIG. 23A to FIG. 23D , FIG. 24A to FIG. 24C and Fig.25 Various processing stages during the fabrication of an integrated circuit package according to an embodiment of the present disclosure are schematically illustrated. DETAILED DESCRIPTION
[0016] The following disclosure provides many different embodiments or examples for realizing different features of the disclosed embodiments. Specific examples of components and arrangements are described below to simplify the disclosed embodiments. Of course, these are merely examples and are not intended to be limiting. For example, in the following description, forming a first component above or on a second component may include an embodiment in which the first component and the second component are directly contacted, and may also include an embodiment in which an additional component may be formed between the first component and the second component so that the first component and the second component may not be in direct contact. In addition, the disclosed embodiments may repeat reference numerals and / or characters in various examples. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or configurations discussed.
[0017] Additionally, for ease of description, spatially relative terms such as "below," "beneath," "lower," "above," "upper," etc. may be used herein to describe the relationship of one element or component to another (or additional) elements or components as illustrated in the figures. The spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein should likewise be interpreted accordingly.
[0018] The embodiments will be described with respect to embodiments in a specific context, namely, integrated circuit packages. However, other embodiments may also be applicable to other electrically connected components, including but not limited to stacked package assemblies, die-to-die assemblies, wafer-to-wafer assemblies, die-to-substrate assemblies, die-to-wafer assemblies, assembled packages, processing substrates, interposers, etc., or mounting input components, boards, dies or other components, or connected packages or mounting combinations for any type of integrated circuit or electronic component. The various embodiments described herein allow functional components (such as, for example, integrated circuit dies) of varying functions and sizes (such as, for example, height) to be packaged in the same integrated circuit package. The various embodiments described herein can be integrated into chip-on-wafer-on-substrate (CoWoS) processes and chip-on-chip-on-substrate (CoCoS) processes.
[0019] Embodiments of the present disclosure relate to a dummy die having an adjustment layer to increase thermal conductivity and warpage control. The adjustment layer may include one or more material layers having a thermal conductivity in a range between about 30 W / mK and about 100 W / mK. In some embodiments, the adjustment layer may include silicon nitride or silicon carbide. In some embodiments, the dummy die may be bonded to another die by a bonding film including a dummy conductor formed therein to further improve thermal conductivity.
[0020] Figure 1 is a flow chart of a method 100 for forming a dummy die according to an embodiment of the present disclosure. In particular, method 100 forms a dummy die for use in a SoIC (system on integrated circuit) package with improved thermal conductivity. The dummy die can be considered as a device-free die. The dummy die is substantially free of any electronic devices. For example, the dummy die is substantially free of any active components or functional components, such as transistors, capacitors, resistors, diodes, photodiodes, fuse devices, and / or other similar devices. The dummy die may include a semiconductor substrate and a bonding structure. An embodiment of the present disclosure provides a dummy die with a bonding structure having improved thermal conductivity and / or improved warpage adjustment.
[0021] Figures 2 to 8 , 9A to 9E and Fig.10 Schematically illustrates various processing stages during the manufacture of a dummy substrate 200 according to an embodiment of the present disclosure. In particular, Figures 2 to 8 , 9A to 9E and Fig.10 Forming a dummy device using method 100 is shown.
[0022] In operation 102, an adhesion layer 204 is deposited on a semiconductor substrate 202, such as Figure 2 as shown in . Figure 2 is a schematic partial cross-sectional view of a semiconductor substrate 202. A plurality of dummy substrates 200 will be formed from the semiconductor substrate 202.
[0023] The semiconductor substrate 202 is formed of one or more semiconductor materials. In some embodiments, the semiconductor substrate 202 is a supporting substrate, including: an elemental semiconductor, such as silicon or germanium in a crystalline, polycrystalline or amorphous structure; a compound semiconductor, such as silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide and / or indium antimonide; an alloy semiconductor, such as, for example, silicon germanium (SiGe), gallium arsenide phosphide (GaAsP), aluminum indium arsenide (AlInAs), aluminum gallium arsenide (AlGaAs), gallium indium arsenide (GaInAs), gallium indium phosphide (GaInP), etc.; combinations thereof or other suitable materials. In some embodiments, the semiconductor substrate 202 may include one or more dopants. The semiconductor substrate 202 may also be in the form of silicon on insulator (SOI). The SOI substrate may include a semiconductor material layer (e.g., silicon, germanium, etc.) formed above an insulating layer (e.g., buried oxide, etc.), and the insulating layer is formed on a silicon substrate. In addition, other substrates that may be used include multilayer substrates, gradient substrates, hybrid orientation substrates, any combination thereof, etc.
[0024] Adhesion layer 204 is deposited on front side 202f of semiconductor substrate 202. In some embodiments, adhesion layer 204 may be formed by flowing an oxidizing precursor to a process chamber. In some embodiments, before forming adhesion layer 204, one or more cleaning processes may be performed to remove native oxide and / or contaminants from semiconductor substrate 202.
[0025] Adhesion layer 204 provides adhesion between subsequent layers to be formed on semiconductor substrate 202. In some embodiments, when semiconductor substrate 202 comprises silicon, adhesion layer 204 comprises silicon oxide. In some embodiments, adhesion layer 204 is formed of USG (undoped quartz glass). In some embodiments, adhesion layer 204 has a thickness of about 1000 nm. Peace If the thickness of the adhesive layer 204 is less than The bonding effect of the bonding layer 204 may not provide sufficient bonding for subsequent layers to the semiconductor substrate 202 to sustain subsequent processes, such as grinding and planarization. For example, cracks may form in the bonding layer 204. Then, the ductility of the adhesive layer 204 may be reduced, and warpage may be formed in the adhesive layer 204 .
[0026] In operation 104, an adjustment layer 206 is deposited on the semiconductor substrate 202 over the adhesion layer 204, such as Figure 2 In some embodiments, the tuning layer 206 provides improved thermal conductivity in the subsequently formed dummy substrate 200. In addition, the tuning layer 206 also provides stress modulation or warpage adjustment to the semiconductor substrate 202.
[0027] The adjustment layer 206 has a thickness T1. In some embodiments, the thickness T1 is about Peace Less than Thickness greater than 1000 mm may not provide adequate thermal conductivity or stress modulation / warpage adjustment. A thickness of 100 Å may generate excessive stress and cause the adjustment layer 206 to peel off from the semiconductor substrate 202 .
[0028] In some embodiments, the adjustment layer 206 may be a thermally conductive layer having a thermal conductivity in a range between about 30 W / mK and about 100 W / mK. In some embodiments, the adjustment layer 206 may include a suitable dielectric film, such as a semiconductor nitride or a semiconductor carbide. In some embodiments, the adjustment layer 206 may include silicon nitride (Si3N4 or SiN), Si-rich silicon nitride, N-rich silicon nitride, silicon carbide, etc.
[0029] In some embodiments, the tuning layer 206 may be silicon nitride. The tuning layer 206 may be formed by flowing a precursor containing a nitrogen source and a semiconductor source. In some embodiments, the tuning layer 206 is formed at a low temperature range to improve thermal conductivity and avoid forming hot spots in the SoIC.
[0030] In operation 106, a bonding film 208 is deposited over the adjustment layer 206, such as Figure 3 as shown in . Figure 3 1 is a partial cross-sectional view of the dummy substrate 200 after operation 106. The bonding film 208 is configured to bond the dummy die to be formed to other dies during subsequent packaging. In particular, the bonding film 208 can be selected from any material suitable for bonding the adjustment layer 206 to another die or to another bonding film. The bonding film 208 can be formed to have any suitable material for bonding in packaging. In some embodiments, the bonding film 208 is formed of an oxide material. For example, the bonding film 208 is formed of USG. In some embodiments, the bonding film 208 has a thickness of about 100 mm. Peace The thickness of the bonding film 208 may be selected based on the waiting time. Because the bonding film 208 may absorb moisture during the waiting time, if there is a longer waiting time for the dummy substrate 200 during packaging, it is desirable to have a thinner bonding film 208 to avoid trapping excessive moisture in the IC package.
[0031] In operation 108, a photoresist layer 210 is deposited over the bonding film 208, and a cutting pattern is formed in the photoresist layer 210, such as Figure 4 as shown in . Figure 4 2 is a partial cross-sectional view of the dummy substrate 200 after operation 108. A photoresist layer 210 may be deposited over the bonding film 208. A photolithography process is then performed to form a cutting pattern having grooves 212 in the photoresist layer 210. The photoresist layer 210 is selectively removed to form the grooves 212. The grooves 212 may form a grid defining a plurality of rectangular regions. Figure 4 As shown in FIG. 2 , the bonding film 208 is exposed at the bottom of the trench 212 .
[0032] In operation 110, one or more etching processes are performed to etch through the bonding film 208, the adjustment layer 206, the adhesion layer 204 and into the semiconductor substrate 202 to form the cutting groove 214, as shown in FIG. Figure 5 as shown in . Figure 51 is a partial cross-sectional view of the dummy substrate 200 after operation 110. The patterned photoresist layer 210 is used as a mask to form cutting grooves 214. The cutting grooves 214 can form a grid in the bonding film 208, the adjustment layer 206, the adhesive layer 204, and enter the semiconductor substrate 202, thereby forming a plurality of dummy regions 216. The cutting grooves 214 are formed to enter the semiconductor substrate 202 but not pass through the semiconductor substrate 202, so that the dummy regions 216 remain connected through the semiconductor substrate 202. The cutting grooves 214 are deep enough so that when the semiconductor substrate 202 is ground down from the back side, the dummy regions 216 can be separated from each other. In some embodiments, the cutting grooves 214 have a width W1 in a range between about 6 microns and about 10 microns.
[0033] In operation 112, a protective layer 218 is deposited to fill the cut trench 214 and cover the dummy region 216. Figure 6 as shown in . Figure 6 1 is a partial cross-sectional view of the pseudo substrate 200 after operation 112. The protective layer 218 is used to cover and protect the exposed portions of the bonding film 208 and the semiconductor substrate 202, the adhesive layer 204 and the adjustment layer 206 during subsequent processing. The protective layer 218 can be formed of any material that can isolate the pseudo region 216 from the processing environment during subsequent processing. The protective layer 218 can also be easily removed from the pseudo region 216. In some embodiments, the protective layer 218 can be formed of a photoresist material. In some embodiments, the protective layer 218 can be deposited on the pseudo region 216 by a spin coating process and a subsequent curing process (e.g., a low temperature curing technology). However, any suitable coating, any suitable deposition technology, and any suitable curing technology can also be used. Optionally, the protective layer 218 can be a curable resin, a polyimide coating, a polybenzoxazole (PBO), an epoxy resin film, etc.
[0034] In operation 114, backside grinding tape 220 and carrier wafer 222 are attached to protective layer 218, such as Figure 7 as shown in . Figure 7 is a partial cross-sectional view of the dummy substrate 200 after operation 114. First, the backside grinding tape 220 is attached to the protective layer 218. Then, the carrier wafer 222 is attached to the backside grinding tape 220 so that the semiconductor substrate 202 can be thinned downward from the backside 202b.
[0035] In operation 116, the semiconductor substrate 202 is turned over, and a backside grinding process is performed to thin the semiconductor substrate 202 downward from the back side 202b, as shown in FIG. Figure 8 as shown in . Figure 8 is a partial cross-sectional view of the dummy substrate 200 after operation 118. According to the design, the backside grinding process reduces the thickness of the semiconductor substrate 202 to a target thickness.
[0036] In some embodiments, a backside grinding process is performed to reduce the thickness of the semiconductor substrate 202 and to “cut” the dummy substrate 200 into a plurality of dummy dies 224. Figure 8 As shown in , the backside grinding process removes the portion of the semiconductor substrate 202 where the groove 214 is not cut, and exposes the protective layer 218. In some embodiments, the concentration of the protective layer 218 in the grinding waste can be used as an end point for the backside grinding process. After the backside grinding process, the thickness of the semiconductor substrate 202 is reduced to a thickness T2. In some embodiments, the thickness T2 is in a range between about 50 microns and about 100 microns.
[0037] Although the dummy dies 224 are manufactured after operation 114, the plurality of dummy dies 224 remain connected by the protective layer 218. The dummy dies 224 are separated by the dicing grooves 214 filled with the protective layer 218. The bonding film 208 on each dummy die 224 contacts the protective layer 218, and the protective layer 218 is attached to the backside grinding tape 220.
[0038] In operation 118, one or more expansion processes are performed to increase the distance between dummy dies 224, such as 9A to 9E as shown in . Fig. 9A is a partial cross-sectional view of dummy die 224 after operation 118 . Fig. 9B and Fig. 9C is a schematic top view of the plurality of dummy dies 224 before and after the expansion process. Fig.9D and Fig.9E 2 is a schematic top view of the plurality of dummy dies 224 before and after the second expansion process.
[0039] After the backside grinding process, the plurality of dummy dies 224 are flipped over and attached to the expansion strip 226 on the frame 228. Fig. 9A As shown in FIG. 2 , a plurality of dummy dies 224 are attached to an extended tape 226 at the back side 202b. The carrier wafer 222 and the backside grinding tape 220 are then removed. The extended tape 226 is then stretched so that the dicing grooves 214 between the dummy dies 224 are widened.
[0040] In some embodiments, ultraviolet radiation 230 may be applied to extension tape 226 so that extension tape 226 may relax and stretch to increase the distance between adjacent dummy dies 224. Fig. 9B As shown in FIG. 1 , before the expansion process, the distance between adjacent dummy dies 224 is the width W1 of the cutting groove 214. As discussed above, the width W1 is in the range between about 6 microns and about 10 microns. Fig. 9CAs shown in FIG, after stretching the extended tape 226, the distance between adjacent dummy dies 224 is width W1'. In some embodiments, width W1' may be in the range between about 60 microns and about 65 microns. The extended distance W1' allows the dummy dies 224 to be individually picked up from the extended tape 226 for subsequent packaging.
[0041] In some embodiments, one or more additional expansion processes may be performed to further increase the distance between adjacent dummy dies 224 for ease of processing. Fig.9D As shown in , dummy die 224 may be transferred from extended strip 226 on frame 228 to second extended strip 226' on second frame 228'. Fig.9E In the embodiment, the second expansion band 226' is stretched and the distance between adjacent dummy dies 224 is increased to a distance W1". In some embodiments, the width W1" may be in a range between about 450 microns and about 550 microns. Although two expansion processes are shown in the example, more or fewer expansions may be used to achieve the desired distance between the dummy dies 224 so that the dummy dies 224 may be picked up by a die handling tool.
[0042] In operation 120, dummy die 224 is cleaned and prepared for subsequent packaging, such as Fig.10 as shown in . Fig.10 1 is a partial cross-sectional view of dummy die 224 after operation 120. Dummy die 224 is cleaned by a suitable process to remove protective layer 218, for example, by an ashing process when protective layer 218 includes a photoresist material. After cleaning, bonding film 208 on each dummy die 224 is exposed. Extended distance W1" allows dummy die 224 to be individually picked up from extended tape 226' for packaging.
[0043] The dummy die 224 according to an embodiment of the present disclosure includes a trimming layer, such as trimming layer 206, deposited on the semiconductor substrate 202 to replace an oxide-based bonding film. The trimming layer 206 is formed of a material with a higher thermal conductivity, thereby improving heat dissipation in the IC package. The trimming layer 206 may also be a high stress layer to improve wafer warpage control, thereby improving bonding quality.
[0044] Fig.11 The thermal conductivity and temperature curves of silicon oxide and silicon nitride are included. Curve 250 is the thermal conductivity and temperature curve of silicon oxide. Curve 252 is the thermal conductivity and temperature curve of silicon nitride. According to the prior art, silicon oxide is used in dummy dies. Silicon oxide promotes the bonding between the dummy die and other dies in the IC package. According to an embodiment of the present disclosure, the adjustment layer 206 is used to replace the silicon oxide in the dummy die. The adjustment layer 206 can be formed of silicon nitride. Fig.11As shown in , the thermal conductivity of silicon nitride is much higher than that of silicon oxide, especially at low temperatures. For example, at 25°C, the thermal conductivity of silicon nitride is about 55 W / mK, while the thermal conductivity of silicon oxide is about 25 W / mK. Therefore, by replacing the silicon oxide layer with the trimming layer 206 having silicon nitride, the embodiments of the present disclosure improve the heat dissipation in the bonding area between the dummy die and the device die.
[0045] In some embodiments, the tuning layer 206 is designed to achieve a desired warp. For example, a negative warp may be desired in a dummy die to improve bonding quality. Negative warp is defined when the substrate warps toward its back side. Fig. 12A is a schematic cross-sectional view of a dummy die 224 to illustrate negative warpage. Fig. 12A 2, the dummy die 224 is positioned with the back side 202b of the semiconductor substrate 202 facing upward and the bonding film 208 facing downward. When the dummy die 224 has no warpage, the outline 260 of the dummy die 224 is planar. When the dummy die 224 has a negative warpage, the outline of the dummy die 224 is represented by a curve 262. In the case of a negative warpage, the bonding film 208 will first contact the die to be bonded at the center region, and the contact area will expand from the center region to the edge region, thereby improving high bonding quality.
[0046] In the prior art, negative warpage is achieved by depositing a certain thickness of silicon oxide. For example, a silicon oxide layer having a thickness ranging between about 15k angstroms and 20k angstroms is applied to a semiconductor substrate to achieve negative warpage to improve bonding quality. The adjustment layer 206 according to an embodiment of the present disclosure can achieve the same or greater negative warpage with a smaller thickness.
[0047] Fig. 12B The warpage corresponding to the thickness of the adjustment layer 206 is schematically shown. Line 264 marks the negative warpage in a wafer having a silicon oxide film with a thickness between 15k angstroms and 20k angstroms. Line 266 indicates the warpage value from the adjustment layer 206 according to an embodiment of the present disclosure. The adjustment layer 206 is formed of silicon nitride. When the adjustment layer 206 has a thickness of 3.5k angstroms, the negative warpage in the dummy die 224 is slightly less than the negative warpage achieved by the silicon oxide film with a thickness between 15k angstroms and 20k angstroms. When the adjustment layer 206 has a thickness of 4.5k angstroms, the negative warpage in the dummy die 224 is about 50% greater than the negative warpage achieved by the silicon oxide film with a thickness between 15k angstroms and 20k angstroms. When the adjustment layer 206 has a thickness of 5.5k angstroms, the negative warpage in the dummy die 224 is about twice the negative warpage achieved by the silicon oxide film with a thickness between 15k angstroms and 20k angstroms.
[0048] like Fig. 12BAs shown in , the trimming layer 206 according to the disclosed embodiment can achieve the same or more negative warpage with a much thinner film. The reduced thickness between the dummy die and the die to be bonded further improves heat dissipation.
[0049] Fig.13 is a flow chart illustrating a method 300 of forming an integrated circuit package according to an embodiment of the present disclosure. A dummy die according to an embodiment of the present disclosure may be used in the method 300. Figures 14 to 21 Various processing stages during the fabrication of an integrated circuit (IC) package 400 according to an embodiment of the present disclosure are schematically illustrated. The IC package 400 may be fabricated using the method 300.
[0050] Method 300 can be used to form a 3DIC (three-dimensional integrated circuit) package. In a typical formation process for forming a 3DIC, two tube core layers are stacked vertically, and an electrical connection is formed between the two tube core layers. For example, the top tube core is stacked above the bottom tube core. The top tube core and the bottom tube core can have different sizes. A dummy tube core can be used to make up for the size difference between the top tube core and the bottom tube core. In method 300, the larger bottom tube core is bonded to the smaller top tube core and one or more dummy tube cores. It should be noted that the terms "top tube core" and "bottom tube core" are used for clarity of description and do not necessarily refer to the physical position of the tube core.
[0051] In operation 302, a first die 406 is attached to a carrier wafer 402 for bonding to a second die, such as Fig.14 as shown in . Fig.14 is a schematic cross-sectional view of IC package 400 after operation 302 . A first die 406 may be referred to as a bottom die, and is attached to carrier wafer 402 via adhesive layer 404 .
[0052] The first die 406 may be a logic die, a memory die, a 3DIC die, a CPU (computing processing unit) die, a GPU (graphics processing unit) die, a SoC (system on chip) die, a MEMS die, etc. The first die 406 may be a single die or a composite die, such as a chiplet having two or more dies. In some embodiments, the first die 406 may be a chiplet including two or more cores, a CPU processor, a GPU processor, and a bus network connecting the two or more cores. From a top view, the first die 406 may be a quadrilateral, rectangular, or square shape.
[0053] Carrier wafer 402 may include, for example, glass, silicon oxide, aluminum oxide, etc. Adhesive layer 404 is applied to carrier wafer 402. Alternatively, carrier wafer 402 may include a carrier tape. Adhesive layer 404 may be used to adhere carrier wafer 402 to other devices such as first die 406. In some embodiments, adhesive layer 404 may be a thermal release film. In some embodiments, adhesive layer 404 may be an ultraviolet (UV) glue that loses its adhesive properties when exposed to UV light. Any suitable adhesive may be utilized, and all such adhesives are fully intended to be included within the scope of the disclosed embodiments.
[0054] The first die 406 may include a substrate 412, a device layer 414 formed in and on the substrate 412, and an interconnect structure 416 formed on the device layer 414. The interconnect structure 416 may include multiple layers of dielectric material with conductive features 418 formed therein.
[0055] The substrate 412 may include bulk silicon (doped or undoped) or an active layer of an SOI substrate. Typically, the SOI substrate includes a semiconductor material layer such as silicon, germanium, silicon germanium, SOI, silicon germanium on insulator (SGOI), or a combination thereof. Other substrates that may be used include multilayer substrates, gradient substrates, or hybrid orientation substrates. The substrate 412 has a front side 408 and a back side 410. The device layer 414 is formed on the front side 408 of the substrate 412. In operation 302, the first die 406 is attached to the carrier wafer 402 so that the back side 410 of the substrate 412 faces upward for subsequent bonding.
[0056] The device layer 414 includes various devices, such as transistors, capacitors, resistors, inductors, etc., which may be used to generate the desired structural and functional requirements for the design of the first die 406 .
[0057] An interconnect structure 416 is formed over the device layer 414 over the front side 408 of the substrate 412. Conductive features 418 embedded in the interconnect structure 416 are designed to connect the various devices in the device layer 414 to form a functional circuit. The interconnect structure 416 is formed of alternating layers of dielectric material and conductive material and can be formed by any suitable process, such as deposition, damascene, dual damascene, etc.
[0058] In operation 304, a bonding film 420 is deposited over the first die 406, such as Fig.15 as shown in . Fig.15 is a schematic cross-sectional view of IC package 400 after operation 304. In some embodiments, before depositing bonding film 420, a grinding process may be performed to thin down substrate 412 to a desired thickness.
[0059] Although Fig.14Only a single first die 406 in the first layer is shown in FIG, but during the packaging process, multiple dies may be placed over the carrier wafer 402 for simultaneous processing. Filling material 419 may be injected into the cavity between adjacent dies. In some embodiments, the filling material 419 may include epoxy, resin, molding compound resin, etc. After the filling material 419 is placed in the cavity between the dies, the filling material 419 may be cured to harden the filling material 419 for optimal protection. The precise curing process depends at least in part on the specific material selected for the filling material 419. In some embodiments, the filling material 419 may be cured by heating the filling material 419 to a temperature between about 100° C. and about 130° C. A chemical mechanical polishing (CMP) process may be performed to remove the filling material 419 deposited over the first die 406 and to thin down the substrate 412 in the first die 406.
[0060] In some embodiments, the bonding film 420 may be formed of silicon oxide, silicon oxynitride, silicon nitride, or a low-k dielectric material having a k value lower than about 3.0. The low-k dielectric material may include a carbon-containing low-k dielectric material, hydrogen silsesquioxane (HSQ), methyl silsesquioxane (MSQ), etc. In some embodiments, the bonding film 420 may be formed by a suitable manufacturing technique, such as chemical vapor deposition (CVD), high density plasma chemical vapor deposition (HDPCVD), or plasma enhanced chemical vapor deposition (PECVD).
[0061] In operation 306, a bonding pad feature 422, also referred to as a bonding pad metal (BPM), is formed in the bonding film 420, such as Fig.16A , Fig. 16B and Fig. 16C as shown in . Fig.16A is a schematic cross-sectional view of IC package 400 after operation 306 . Fig. 16B is an IC package along Fig.16A Floor plan of the BB line. Fig. 16C is an IC package along Fig.16A Floor plan on the CC line.
[0062] The bonding pad component 422 can be formed of copper or other suitable metals to facilitate subsequent bonding. In some embodiments, the bonding pad component 422 can be formed by suitable manufacturing techniques, such as electroplating or deposition. In some embodiments, the bonding pad component 422 can be formed by a damascene process, such as a single damascene process or a dual damascene process. The bonding pad component 422 is configured to bond with the bonding pad component on the second tube core. The bonding pad component 422 is arranged in an area corresponding to the second tube core and is arranged in a pattern matching the bonding pad component in the second tube core. Fig. 16BThe distribution of the bonding pad components 422 in the bonding film 420 is schematically shown. The number of the bonding pad components 422 may be less than or greater than Fig. 16B 406a and 406b. The bonding pad component 422 may be specified based on requirements and / or design layout. In some embodiments, the top surface of the bonding pad component 422 and the top surface of the bonding film 420 are substantially coplanar to provide a suitable surface for subsequent bonding. For example, flatness can be achieved by a flattening step such as a chemical mechanical polishing (CMP) step or a mechanical grinding step. After flattening, the first die 406 has a substantially flat bonding surface 406b, including the area of the bonding film 420 and the area of the bonding pad component 422.
[0063] In some embodiments, a portion of the bonding pad component 422 is connected to a semiconductor through-hole (TSV) 424. TSV 424 is embedded in the substrate. In some embodiments, TSV 424 can be formed by copper or other suitable metals that are easy to form DD (dielectric-dielectric) and MM (metal-metal) bonding. In some embodiments, TSV 424 can be formed simultaneously with the bonding pad component 422 by a damascene process. In other embodiments, TSV 424 can be pre-fabricated with the device layer 414 during the front-end process. TSV 424 can be used to provide electrical connection between the first tube core 406 and the second tube core to be bonded to the first tube core 406. The first end of TSV 424 contacts the bonding pad component 422, and the second end of TSV 424 contacts the conductive component 418 in the interconnect structure 416. Conductive component 418 can be connected to active components and / or passive components in the device layer 414.
[0064] Fig. 16C The distribution of TSVs 424 in the substrate 412 is schematically shown. The number of TSVs 424 may be less than or greater than Fig. 16C The number and layout of TSVs 424 are specified based on requirements and / or design layout.
[0065] In operation 308, the second die 426 and one or more dummy dies 224 are bonded to the first die 406, such as FIG. 17A to FIG. 17B as shown in . Fig.17A is a schematic cross-sectional view of IC package 400 after operation 308 . Fig. 17B is an IC package along Fig.17A Floor plan of the BB line.
[0066] The second die 426 may be a logic die, a memory die, a 3DIC die, a CPU die, a GPU die, a SoC die, a MEMS die, etc. The second die 426 may be a single die or a composite die, such as a chiplet having two or more dies. In some embodiments, the second die 426 may be a memory die.
[0067] The second die 426 may include a substrate 428, a device layer 430 formed in and on the substrate 428, and an interconnect structure 432 formed on the device layer 430. The interconnect structure 432 may include a multilayer dielectric material having a conductive feature 434 formed therein. The second die 426 may include a dielectric layer 436 formed over the interconnect structure 432. The dielectric layer 436 includes a bonding pad 438 and a bonding via 440 embedded therein. A bonding film 442 is formed on the dielectric layer 436. A bonding pad feature 444 is formed in the bonding film 442.
[0068] Substrate 428 may include bulk silicon (doped or undoped) or an active layer of an SOI substrate. Typically, an SOI substrate includes a semiconductor material layer such as silicon, germanium, silicon germanium, SOI, silicon germanium on insulator (SGOI), or a combination thereof. Other substrates that may be used include multilayer substrates, gradient substrates, or hybrid orientation substrates. Device layer 430 is formed on the front side of substrate 428. In operation 308, second die 426 is bonded to first die 406 with the back side of substrate 428 facing upward.
[0069] The device layer 430 includes various devices, such as transistors, capacitors, resistors, inductors, etc., which may be used to generate the desired structural and functional requirements for the design of the second die 426 .
[0070] An interconnect structure 432 is formed over the front side of the substrate 428, over the device layer 430. Conductive features 434 embedded in the interconnect structure 432 are designed to connect the various devices in the device layer 430 to form a functional circuit. The interconnect structure 432 is formed of alternating layers of dielectric material and conductive material, and can be formed by any suitable process, such as deposition, damascene, dual damascene, etc.
[0071] The dielectric layer 436 may include one or more dielectric layers. In some embodiments, the material of the dielectric layer 436 may be silicon oxide, silicon nitride, silicon oxynitride, or a dielectric layer formed of other suitable dielectric materials. In some embodiments, the dielectric layer 436 may be undoped silicon glass, low-k material, ultra-low-k material, silicon oxide, etc. The bonding pad 438 and the bonding via 440 may be formed of aluminum, aluminum copper, or other suitable conductive materials.
[0072] In some embodiments, the bonding film 442 may be formed of silicon oxide, silicon oxynitride, silicon nitride, or a low-k dielectric material having a k value lower than about 3.0. The low-k dielectric material may include a carbon-containing low-k dielectric material, hydrogen silsesquioxane (HSQ), methyl silsesquioxane (MSQ), etc. In some embodiments, the bonding film 442 may be formed by a suitable manufacturing technique, such as chemical vapor deposition (CVD), high density plasma chemical vapor deposition (HDPCVD), or plasma enhanced chemical vapor deposition (PECVD).
[0073] The bonding pad component 444 can be formed of copper or other suitable metals to facilitate subsequent bonding. In some embodiments, the bonding pad component 444 can be formed by suitable manufacturing techniques, such as electroplating or deposition. In some embodiments, the bonding pad component 444 can be formed by a damascene process, such as a single damascene process or a dual damascene process. The bonding pad component 444 is configured to bond with the bonding pad component 422 on the first tube core 406. In some embodiments, the bonding pad component 444 is arranged in the same layout mirrored with the bonding pad component 422. A portion of the bonding pad component 444 contacts the bonding pad 438 through the bonding through hole 440 to provide an electrical connection to the components in the device layer 430.
[0074] In some embodiments, the top surface of the bonding pad component 444 and the top surface of the bonding film 442 are substantially coplanar to provide a suitable surface for subsequent bonding. For example, flatness can be achieved by a planarization step such as a chemical mechanical polishing (CMP) step or a mechanical grinding step. After planarization, the second die 426 has a substantially flat bonding surface 426b, including the area of the bonding film 442 and the area of the bonding pad component 444.
[0075] In some embodiments, the first die 406 and the second die 426 may be bonded surface-to-surface, such as Fig.17A The bonding film 442 of the second die 426 is bonded to the bonding film 420 of the first die 406 by dielectric-to-dielectric bonding, and the bonding pad component 444 of the second die 426 is bonded to the bonding pad component 422 of the first die 406 by metal-to-metal bonding. The bonding process may be referred to as DD and MM bonding.
[0076] Before the second die 426 is bonded to the first die 406, the second die 426 can be picked up and placed on the bonding surface 406b of the first die 406 so that the bonding surface 406b of the first die 406 is in direct contact with the bonding surface 426b of the second die 426, and the bonding pad components 422 and 444 are aligned and in direct contact. In some embodiments, in order to promote DD and MM bonding between the first die 406 and the second die 426, surface preparation can be performed on the bonding surfaces of the first die 406 and the second die 426. For example, the surface preparation can include surface cleaning and activation. In some embodiments, the bonding surface 406b of the first die 406 and the bonding surface 426b of the second die 426 can be cleaned by wet cleaning.
[0077] After bonding, a DD and MM bonding surface is formed between the first die 406 and the second die 426. In some embodiments, the metal-to-metal bonding at the DD and MM bonding interface is a copper-to-copper bonding. In some embodiments, the dielectric-to-dielectric bonding at the DD and MM bonding interface is achieved using a generated Si-O-Si bond. After bonding, the first die 406 is electrically connected to the second die 426 through the bonding between the bonding pad component 444 and the bonding pad component 422. During the DD and MM bonding process, a low temperature heating process is performed at a temperature range between about 100°C and about 280°C to strengthen the dielectric-to-dielectric bonding at the DD and MM bonding interface. A high temperature heating process is performed at a temperature in a range between about 100°C and about 400°C to promote metal-to-metal bonding at the DD and MM bonding interface.
[0078] like Fig. 17B As shown in , the second die 426 is smaller than the first die 406. One or more dummy dies 224 are bonded to the first die 406 such that the bottom and top layers are substantially the same size. Fig. 17B Four dummy dies 224 are depicted. Fewer or more dummy dies 224 may be included, depending on the design of IC package 400.
[0079] The shape and size of each dummy die 224 may be selected based on the shape, size, and relative position of the first die 406 and the second die 426. The surface area of each dummy die 224 may be selected based on the surface area of the larger die or first die 406 in the IC package 400. In some embodiments, the ratio of the surface area of each dummy die 224 to the surface area of the first die 406 may be in a range between about 7.5% and about 10%. The shape of the dummy die 224 may be rectangular, square, or other shapes that fit the layout.
[0080] Before bonding the dummy die 224 to the first die 406, the dummy die 224 may be bonded to the first die 406 from a frame such as Fig.10 The dummy die 224 is picked up by a frame 228 in the first die 406 and placed on the bonding surface 406 b of the first die 406, so that the bonding surface 406 b of the first die 406 is in direct contact with the bonding film 208 of the dummy die 224. In some embodiments, in order to facilitate DD and MM bonding between the dummy die 224 and the second die 426, surface preparation may be performed on the bonding surfaces of the first die 406 and the dummy die 224. The surface preparation may include surface cleaning and activation.
[0081] The dummy die 224 is stacked on and bonded to the first die 406. The dummy die 224 is disposed side by side with each other and with the second die 426. In some embodiments, the dummy die 224 is fusion bonded to the first die 406. In other words, the dummy die 224 is bonded to the first die 406 by dielectric-to-dielectric bonding. In some embodiments, the dummy die 224 may be bonded by a low temperature heating process at a temperature in a range between about 100° C. and about 280° C. to strengthen the dielectric-to-dielectric bonding. In some embodiments, bonding the dummy die 224 to the first die 406 and bonding the second die 426 to the first die 406 may be implemented in the same DD and MM bonding processes. Alternatively, bonding the dummy die 224 to the first die 406 and bonding the second die 426 to the first die 406 may be implemented in different bonding processes.
[0082] In operation 310, a dielectric film 446 is deposited over the IC package 400 to fill the gap between the dummy die 224 and the second die 426, as shown in FIG. Fig.18 as shown in . Fig.18 4 is a schematic cross-sectional view of IC package 400 after operation 310. In some embodiments, dielectric film 446 may include an oxide material, such as silicon oxide (SiO), TEOS, BPTEOS, etc. Dielectric film 446 may also be a nitride material. Dielectric film 446 may also be a low-k dielectric material, a polymer material, other dielectric materials, etc., or a combination thereof. Dielectric film 446 may also be formed by plasma enhanced chemical vapor deposition (PECVD), low pressure CVD (LPCVD), plasma vapor deposition (PVD), etc.
[0083] In operation 312, a planarization process is performed, such as Fig.19 as shown in . Fig.19 is a schematic cross-sectional view of IC package 400 after operation 312. The planarization process removes excess dielectric film 446 over dummy die 224 and second die 426. The planarization process may also be used to thin down dummy die 224 and second die 426 and to create a planar surface 448 for further processing.
[0084] In operation 314, a second carrier wafer 450 is attached to the IC package 400 on the surface 448, such as Fig. 20 as shown in . Fig. 20 4 is a schematic cross-sectional view of the IC package 400 after operation 314. In some embodiments, a bonding film 452 is formed over the second carrier wafer 450. A bonding film 454 is formed over the flat surface 448 of the IC package 400. In some embodiments, the bonding film 208 is formed of an oxide material. For example, the bonding films 452, 454 may include a dielectric material such as silicon oxide, silicon oxynitride, etc.
[0085] The IC package 400 is attached to the second carrier wafer 450 by bonding the bonding films 452, 454. After the second carrier wafer 450 is attached to the IC package 400, the first carrier wafer 402 may be removed and the IC package 400 may be flipped to form contacts over the front side of the first die 406. In some embodiments, surface preparation, such as surface cleaning and activation, may be performed to expose the topmost layer of the conductive features 418 for subsequent processing.
[0086] In operation 316, an RDL (redistribution layer) structure 456 and external connectors 464 are formed over the first die 406, such as Fig.21 as shown in . Fig.21 is a schematic cross-sectional view of IC package 400 after operation 314 .
[0087] The RDL structure 456 may include one or more conductive layers 462 formed in one or more passivation layers 458. In some embodiments, the RDL structure 456 may include a protective layer 460 disposed above the passivation layer 458. The passivation layer 458 may be formed of a nitride-based material. The protective layer 460 may be formed of silicon oxide, silicon nitride, or a combination thereof. The conductive layer 462 may include a metal such as aluminum, copper, tungsten, titanium, and a combination thereof. The RDL structure 456 may be formed by: depositing the conductive layer 462 by chemical vapor deposition; and then etching the undesired portion, leaving the RDL structure 456. Other materials and processes (such as well-known damascene processes) may optionally be used to form the RDL structure 456.
[0088] The external connector 464 may be a contact bump, such as a microbump or a controlled collapse chip connection (C4) bump. The external connector 464 may include a material such as tin or other suitable materials such as silver or copper. In some embodiments, the external connector 464 is a tin solder bump formed by any suitable method such as evaporation, electroplating, printing, solder transfer, ball placement, etc. Once the tin layer has been formed on the structure, reflow is performed to shape the material into a desired bump shape. A protective layer 466 may be formed between the RDL structure 456 and the external connector 464. In some embodiments, the protective layer 466 may be formed of polyimide or the like.
[0089] like Fig.21 As shown in , the substrate 202 in the dummy die 224 and the substrate 412 of the first die 406 are bonded via the bonding film 420, the bonding film 208, the adjustment layer 206, and the adhesive layer 204. During operation, the heat generated in the device layer 414 can be dissipated from the substrate 412 to the substrate 202 via the bonding layer (i.e., the bonding film 420, the bonding film 208, the adjustment layer 206, and the adhesive layer 204). Because the adjustment layer 206 has an improved thermal conductivity, heat dissipation is improved. In addition, the effective bonding length between the dummy die 224 and the first die 406 is also improved because the adjustment layer 206 is used to cause warping of the dummy die 224 to improve the bonding quality. The improved bonding quality further improves the heat transfer between the dummy die 224 and the first die 406.
[0090] Fig. 22 is a flow chart illustrating a method 500 of forming an integrated circuit package according to an embodiment of the present disclosure. FIG. 23A to FIG. 23B , FIG. 24A to FIG. 24C and Fig.25 Various processing stages during the manufacture of an IC package 600 using the method 500 are schematically illustrated.
[0091] Method 500 is similar to method 300, except that method 500 includes operations 506 and 508 instead of operations 306 and 308 in method 300. In operation 506, a dummy conductor is formed in the first die. In operation 508, the dummy die is bonded to the first die in the region using the dummy conductor. Method 500 begins with operations 302 and 304. The corresponding stages may be Fig.14 and Fig.15 Depicted in.
[0092] In operation 506, a dummy conductor 602 is formed in the bonding film 420 in addition to the bonding pad part 422, as shown in FIG. FIG. 23A to FIG. 23B as shown in . Fig.23A is a schematic cross-sectional view of IC package 600 after operation 506 . Fig. 23B is a plan view of the IC package 600 . Fig.23Cand Fig.23D is a partial cross-sectional view showing a dummy conductor according to an embodiment of the present disclosure.
[0093] The dummy conductor 602 is a conductive feature, such as a via or a line, formed in the bonding film 420. The dummy conductor 602 is configured to further improve thermal conductivity between the first die 406 and the dummy die 224.
[0094] Similar to the bonding pad component 422, the dummy conductor 602 is a conductive component, line and / or via formed in the bonding film 420. As discussed above, at least a portion of the bonding pad component 422 is connected to the TSV 424 formed in the substrate 412 of the first die 406. The bonding pad component 422 is also intended to be connected to a conductor in the die to be bonded, such as the bonding pad component 444 in the second die 426. Unlike the bonding pad component 422, the dummy conductor 602 is electrically floating in the bonding film 420. That is, the dummy conductor 602 is not connected to any conductor in the first die 406. The dummy conductor 602 is also not connected to any conductive component in the die to be bonded, such as the dummy die 224.
[0095] The pseudo conductor 602 may be formed of copper or other suitable metals. In some embodiments, the pseudo conductor 602 may be formed by suitable manufacturing techniques, such as electroplating or deposition. The pseudo conductor 602 may be formed by forming grooves and vias in the bonding film 420 and filling the grooves and vias in the bonding film 420. In some embodiments, the pseudo conductor 602 may be formed by a damascene process, such as a single damascene process or a dual damascene process. In some embodiments, the pseudo conductor 602 may be formed simultaneously with the bonding pad component 422.
[0096] After operation 506, the top surfaces of the dummy conductor 602 and the bonding pad component 422 and the top surface of the bonding film 420 are substantially coplanar to provide a suitable surface for subsequent bonding. Flatness can be achieved, for example, by a planarization step such as a chemical mechanical polishing (CMP) step or a mechanical grinding step. After planarization, the first die 406 has a substantially flat bonding surface 606b, including the area of the bonding film 420, the area of the bonding pad component 422, and the area of the dummy conductor 602.
[0097] In some embodiments, the dummy conductor 602 may have a height H in the bonding film 420 . In some embodiments, the height H of the dummy conductor 602 may range from about 1 k angstrom to about 20 k angstrom. In some embodiments, the height H of the dummy conductor 602 may be substantially the same as the height of the bonding pad component 422 .
[0098] In some embodiments, the height H of the dummy conductor 602 may be embedded in the bonding film 420, such as Fig.23AIn other embodiments, the dummy conductor 602 may have the same thickness as the bonding film 420 so that the dummy conductor 602 is in contact with the back side 410 of the substrate 412, as shown in FIG. Fig.23C In other embodiments, the height H of the pseudo conductor 602 may be greater than the thickness of the bonding film 420, so that the pseudo conductor 602 extends into the substrate 412, as shown in FIG. Fig.23D as shown in .
[0099] Fig. 23B The distribution of the dummy conductor 602 in the bonding film 420 is schematically shown. Fig. 23B As shown in FIG. 4 , dummy conductor 602 is arranged utilizing a region of bonding film 420 that is configured to receive a dummy die in subsequent bonding. Fig. 23B is a schematic depiction of pseudo conductors 602. The number, shape, and arrangement of pseudo conductors 602 may be arranged in any suitable manner. In some embodiments, the total surface area of pseudo conductors 602 may be first selected. The shape and arrangement of pseudo conductors 602 may be determined to achieve the total surface area.
[0100] In some embodiments, the total area of dummy conductor 602 may be determined by the surface area of the dummy die to be bonded thereto. For example, the ratio of the total surface area of dummy conductor 602 bonded to the dummy die to the surface area of the dummy die may be in a range between about 0.03 and about 0.3.
[0101] In other embodiments, the surface area of the first die 406 (i.e., the die on which the dummy conductor 602 is formed) may affect the total surface area of the dummy conductor 602. For example, the ratio of the total surface area of the dummy conductor 602 to the surface area of the first die 406 may be in a range between about 0.001 and about 0.01.
[0102] In other embodiments, the surface area of the second die 426 (i.e., the non-dummy die to be bonded to the first die 406) may also affect the total surface area of the dummy conductor 602. For example, the ratio of the total surface area of the dummy conductor 602 to the surface area of the second die 426 may be in a range between about 0.003 and about 0.03.
[0103] The pseudo conductor 602 may be any suitable shape and any suitable arrangement to achieve the total surface area. For example, the pseudo conductor 602 may be a conductive via having a diameter D in the range between about 0.01 mm and about 0.1 mm. In other embodiments, the pseudo conductor 602 may be a wire having a width in the range between about 0.01 mm and about 0.1 mm and a length between about 1 mm and about 10 mm. In some embodiments, the pseudo conductor 602 may have the same shape. In other embodiments, the pseudo conductor 602 may be a combination of multiple shapes.
[0104] In some embodiments, dummy conductors 602 may be distributed in one or more dummy regions 604. Each dummy region 604 may have a shape similar to the dummy die 224 to be bonded thereto. Dummy regions 604 may be slightly smaller than the surface area of dummy die 224, thereby forming a conductor-free strip around the edge of dummy die 224 after bonding as described in operation 508.
[0105] In operation 508, the second die 426 and one or more dummy dies 224 are bonded to the first die 406, such as FIG. 24A to FIG. 24C as shown in . Fig.24A is a schematic cross-sectional view of IC package 600 after operation 508 . Fig. 24B is a plan view of the IC package 600 . Fig.24C is a partial plan view showing the distribution of dummy conductors 602 relative to dummy die 224 after bonding.
[0106] The first die 406 and the second die 426 may be surface-to-surface bonded by DD and MM bonding processes, as described above with respect to operation 308. The dummy die 224 is bonded to the first die 406 using the dummy conductor 602 in the bonding surface. The dummy die 224 is positioned side by side with each other and the second die 426, and is located above the area of the dummy conductor 602. In some embodiments, the dummy die 224 is fusion bonded to the first die 406. In some embodiments, the dummy die 224 may be bonded by a low temperature heating process at a temperature in a range between about 100° C. and about 280° C. to strengthen the dielectric-to-dielectric bond.
[0107] In some embodiments, dummy die 224 are aligned with and positioned over corresponding dummy regions 604, thereby forming a conductor-free strip 606 in an edge region of each dummy die 224, such as Fig.24C As shown in . Non-conductor strip 606 reduces the non-bonding length near the edge region of dummy die 224, thus improving the bonding quality. In some embodiments, non-conductor strip 606 may have a width BW ranging between about 1 mm and about 2 mm.
[0108] In some embodiments, bonding dummy die 224 to first die 406 and second die 426 to first die 406 may be performed in the same DD and MM bonding processes. Alternatively, bonding dummy die 224 to first die 406 and second die 426 to first die 406 may be performed in different bonding processes.
[0109] After operation 508 , operations 310 , 312 , 314 , and 316 may be performed as described above with respect to method 300 . Fig.25 is a schematic cross-sectional view of IC package 600 after operation 314 .
[0110] like Fig.25 As shown in FIG, the substrate 202 in the dummy die 224 and the substrate 412 of the first die 406 are bonded via a film stack, which includes a bonding film 420 having a dummy conductor 602, a bonding film 208, an adjustment layer 206, and an adhesive layer 204. During operation, heat generated in the device layer 414 can be dissipated from the substrate 412 to the substrate 202 via the film stack. In addition to the material in the adjustment layer 206, the thermal conductivity of the film stack is further reduced by the presence of the dummy conductor 602 in the bonding film 420.
[0111] Embodiments of the present disclosure provide a dummy die with an improved bonding structure. In particular, the dummy die according to the embodiments of the present disclosure increases the thermal conductivity through the dummy die, enhancing warpage adjustment with a thinner film. Embodiments of the present disclosure also include a dummy conductor to be bonded to the dummy die, which further increases thermal conductivity. According to embodiments of the present disclosure, the increased thermal conductivity enables improved heat dissipation in an IC package.
[0112] It should be understood that not all advantages are necessarily discussed herein, that no particular advantage is required for all embodiments or examples, and that other embodiments or examples may provide different advantages.
[0113] Some embodiments of the present disclosure relate to a semiconductor package, including: a first die having a first bonding film; a second die stacked above the first die and bonded to the first die via the first bonding film; and a dummy die stacked above the first die and bonded to the first die via the first bonding film, wherein the dummy die includes: a substrate; an adjustment layer formed above the substrate, wherein the adjustment layer has a thermal conductivity in a range between about 30 W / mK and about 100 W / mK; and a second bonding film formed above the adjustment layer, wherein the second bonding film is bonded to the first bonding film.
[0114] Some embodiments of the present disclosure relate to a method, comprising: bonding a first die to a second die, wherein the first die includes a first bonding film and the second die is bonded to the first bonding film; and bonding a dummy die to the first die, wherein the dummy die includes: a substrate; an adjustment layer formed over the substrate, wherein the adjustment layer has a thermal conductivity in a range between about 30 W / mK and about 100 W / mK; and a second bonding film formed over the adjustment layer, and the first bonding film is bonded to the second bonding film.
[0115] Some embodiments of the present disclosure relate to a method for forming a dummy die, comprising: depositing an adjustment layer on the front side of a semiconductor substrate; depositing a bonding film on the adjustment layer; forming a cutting pattern above the bonding film; etching through the bonding film, the adjustment layer and into the semiconductor substrate using the cutting pattern to form a cutting groove; depositing a protective layer in the cutting groove and on the bonding film; attaching a carrier wafer to the protective layer; and grinding the semiconductor substrate from the back side to expose the protective layer in the cutting groove.
[0116] Some embodiments of the present application provide a semiconductor package, including: a first die having a first bonding film; a second die stacked above the first die and bonded to the first die via the first bonding film; and a dummy die stacked above the first die and bonded to the first die via the first bonding film, wherein the dummy die includes: a substrate; an adjustment layer formed above the substrate, wherein the adjustment layer has a thermal conductivity in a range between 30 W / mK and 100 W / mK; and a second bonding film formed above the adjustment layer, wherein the second bonding film is bonded to the first bonding film. In some embodiments, the adjustment layer includes silicon nitride or silicon carbide. In some embodiments, the adjustment layer has a thickness between 3k angstroms and 6k angstroms. In some embodiments, the second bonding film has a thickness between 100 angstroms and 1000 angstroms. In some embodiments, the second bonding film includes silicon oxide. In some embodiments, the semiconductor package further includes: an adhesive layer disposed between the substrate and the adjustment layer. In some embodiments, the adhesive layer includes silicon oxide. In some embodiments, the semiconductor package further comprises: one or more dummy conductors formed in the first bonding film, wherein the one or more dummy conductors are in contact with the second bonding film. In some embodiments, the first bonding film comprises a band surrounding the one or more dummy conductors, the band is in contact with an edge region of the dummy die, and the one or more dummy conductors are disposed within the band.
[0117] Some other embodiments of the present application provide a method of forming a semiconductor package, comprising: bonding a first die to a second die, wherein the first die includes a first bonding film, and the second die is bonded to the first bonding film; and bonding a dummy die to the first die, wherein the dummy die includes: a substrate; an adjustment layer formed above the substrate, wherein the adjustment layer has a thermal conductivity in a range between 30 W / mK and 100 W / mK; and a second bonding film formed above the adjustment layer, and the first bonding film is bonded to the second bonding film. In some embodiments, the adjustment layer includes silicon nitride or silicon carbide. In some embodiments, the method further includes: forming one or more dummy conductors in the first bonding film, wherein bonding the dummy die to the first die includes placing the dummy die above the one or more dummy conductors. In some embodiments, bonding the first die to the second die and bonding the dummy die to the first die are performed simultaneously. In some embodiments, the method further includes: depositing a dielectric material between the second die and the dummy die; and forming external connectors over the first die, wherein the external connectors and the first bonding film are disposed over opposite sides of the first die.
[0118] Some further embodiments of the present application provide a method for forming a dummy die, comprising: depositing an adjustment layer on the front side of a semiconductor substrate; depositing a bonding film on the adjustment layer; forming a cutting pattern above the bonding film; etching through the bonding film, the adjustment layer and into the semiconductor substrate using the cutting pattern to form a cutting groove; depositing a protective layer in the cutting groove and on the bonding film; attaching a carrier wafer to the protective layer; and grinding the semiconductor substrate from the back side to expose the protective layer in the cutting groove. In some embodiments, the method further comprises: depositing an adhesive layer on the front side of the semiconductor substrate, and the adjustment layer is deposited on the adhesive layer. In some embodiments, the adhesive layer comprises silicon oxide. In some embodiments, the adjustment layer comprises silicon nitride or silicon carbide. In some embodiments, the method further comprises: attaching an extension tape to the back side of the semiconductor substrate after grinding the semiconductor substrate; and stretching the extension tape to widen the cutting groove. In some embodiments, the method further comprises: removing the protective layer to expose the bonding film.
[0119] The features of several embodiments are summarized above so that those skilled in the art can better understand the various aspects of the embodiments of the present disclosure. Those skilled in the art should understand that they can easily use the embodiments of the present disclosure as a basis to design or modify other processes and structures for performing the same purpose and / or achieving the same advantages as the embodiments introduced herein. Those skilled in the art should also appreciate that such equivalent constructions do not deviate from the spirit and scope of the embodiments of the present disclosure, and that they can make various changes, substitutions and modifications herein without departing from the spirit and scope of the embodiments of the present disclosure.
Claims
1. A semiconductor package, comprising: A first die having a first bonding film; a second die stacked over the first die and bonded to the first die via the first bonding film; as well as a dummy die stacked above the first die and bonded to the first die via the first bonding film, wherein the dummy die comprises: substrate; an adjusting layer formed over the substrate, wherein the adjusting layer has a thermal conductivity in a range between 30 W / mK and 100 W / mK; and A second bonding film is formed on the adjustment layer, wherein the second bonding film is bonded to the first bonding film.
2. The semiconductor package according to claim 1, wherein: The adjustment layer includes silicon nitride or silicon carbide.
3. The semiconductor package according to claim 2, wherein: The tuning layer has a thickness between 3k angstroms and 6k angstroms.
4. The semiconductor package according to claim 3, wherein: The second bonding film has a thickness between 100 angstroms and 1000 angstroms.
5. The semiconductor package according to claim 2, wherein: The second bonding film includes silicon oxide.
6. The semiconductor package according to claim 5, further comprising: An adhesive layer is disposed between the substrate and the adjustment layer.
7. The semiconductor package according to claim 6, wherein: The adhesive layer includes silicon oxide.
8. The semiconductor package according to claim 1, further comprising: One or more dummy conductors are formed in the first bonding film, wherein the one or more dummy conductors are in contact with the second bonding film.
9. A method of forming a semiconductor package, comprising: bonding a first die to a second die, wherein the first die includes a first bonding film and the second die is bonded to the first bonding film; and Bonding a dummy die to the first die, wherein the dummy die comprises: substrate; an adjusting layer formed over the substrate, wherein the adjusting layer has a thermal conductivity in a range between 30 W / mK and 100 W / mK; and A second bonding film is formed over the adjustment layer, and the first bonding film is bonded to the second bonding film.
10. A method for forming a dummy die, comprising: depositing a trimming layer on a front side of a semiconductor substrate; depositing a bonding film on the adjustment layer; forming a cutting pattern above the bonding film; etching through the bonding film, the adjustment layer, and into the semiconductor substrate using the cutting pattern to form a cutting groove; depositing a protective layer in the dicing groove and on the bonding film; attaching a carrier wafer to the protective layer; as well as The semiconductor substrate is ground from a back side to expose the protection layer in the cutting grooves.