High-luminous-efficiency flip LED chip and preparation method thereof

By setting periodic conductive vias on the dielectric layer and depositing a metal reflective layer, combined with the DBR layer, the problem that the metal reflective layer in the prior art cannot take into account both reflectivity and conductivity, and the luminous efficiency of the flip-fit ​​LED chip is improved and Reflectivity uniformity.

CN118919613APending Publication Date: 2024-11-08JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411006580.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing metal reflective layer cannot take into account both high reflectivity and conductivity in flip-mounted LED chips, resulting in low luminous efficiency.

Method used

By setting periodic conductive vias on the dielectric layer and depositing a metal reflective layer in the vias, combining the DBR layer to increase the reflectivity, forming a transparent protective layer and electrode, the structure and material distribution of the metal reflective layer are optimized.

Benefits of technology

The high luminous efficiency of the high-light efficiency flip LED chip is achieved, taking into account both reflectivity and conductivity, and improving the problem of uneven reflectivity in the spectral range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919613A_ABST
    Figure CN118919613A_ABST
Patent Text Reader

Abstract

The invention discloses a high-luminous-efficiency flip LED chip and a preparation method thereof, and the preparation method comprises the following steps: providing a substrate, and forming an epitaxial layer on the substrate; forming a transparent conductive layer on the P-type semiconductor layer, and etching to form an N-type semiconductor mesa and a P-type semiconductor mesa; forming dielectric layers on the N-type semiconductor mesa, the P-type semiconductor mesa and the mesa side wall; a periodic conductive through hole is formed in the dielectric layer on the P-type semiconductor mesa, the transparent conductive layer is exposed, and a metal reflecting layer is formed in the periodic conductive through hole and on the dielectric layer; forming a through hole in the dielectric layer on the N-type semiconductor mesa to expose the N-type semiconductor mesa; forming a transparent protection layer on the metal reflection layer and the dielectric layer, forming an electrode through hole in the transparent protection layer, and exposing the metal reflection layer and the N-type semiconductor mesa respectively; and forming a P electrode and an N electrode in the electrode through hole. By implementing the flip LED chip, the lighting effect of the flip LED chip can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field, and in particular to a high-light-efficiency flip-chip LED chip and a preparation method thereof. Background Art

[0002] With the rapid development of semiconductor lighting technology, light-emitting diodes (LEDs) have become the mainstream choice of the new generation of lighting sources due to their high efficiency, energy saving, and environmental protection. Among the many LED technologies, flip-chip LED (FCLED) chips have gradually attracted widespread attention in the industry due to their superior thermal management performance and high light efficiency. In order to further improve the performance of flip-chip LEDs, the introduction of metal reflective layer structures has become an important research direction.

[0003] The metal reflective layer structure is a design that uses a metal with a high reflectivity such as silver or aluminum as a reflective layer on the surface of the LED chip. Metals such as silver or aluminum as reflective layer materials have excellent reflective performance, heat dissipation performance and process compatibility, etc., which can significantly improve the light extraction efficiency of flip-chip LED chips. However, the metal reflective layer is generally made by depositing metals such as Cr or Ni on highly reflective metals such as Ag or Al for electrical contact and adhesion, but the addition of metals such as Cr or Ni greatly reduces the reflective effect of the metal reflective layer. Existing metal reflective layers cannot take into account the requirements of reflectivity and conductivity. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a high-light-efficiency flip-chip LED chip, wherein the prepared flip-chip LED chip has high luminous efficiency.

[0005] Another technical problem to be solved by the present invention is to provide a method for preparing a high-light-efficiency flip-chip LED chip. The preparation method is simple and the prepared flip-chip LED chip has high luminous efficiency.

[0006] In order to solve the above problems, the present invention discloses a method for preparing a high-light-efficiency flip-chip LED chip, comprising the following steps:

[0007] (1) providing a substrate, and forming an epitaxial layer on the substrate, wherein the epitaxial layer includes an N-type semiconductor layer, an active layer, and a P-type semiconductor layer deposited in sequence;

[0008] (2) forming a transparent conductive layer on the P-type semiconductor layer, etching a portion of the epitaxial layer until the N-type semiconductor layer is exposed, and forming an N-type semiconductor mesa and a P-type semiconductor mesa;

[0009] (3) forming a dielectric layer on the N-type semiconductor mesa, the P-type semiconductor mesa, and the sidewalls of the mesa;

[0010] (4) opening periodic conductive through holes in the dielectric layer on the P-type semiconductor mesa to expose the transparent conductive layer, and forming a metal reflective layer in the periodic conductive through holes and on the dielectric layer; and opening through holes in the dielectric layer on the N-type semiconductor mesa to expose the N-type semiconductor mesa;

[0011] (5) forming a transparent protective layer on the metal reflective layer and the dielectric layer, and opening electrode through holes in the transparent protective layer to expose the metal reflective layer and the N-type semiconductor table respectively;

[0012] (6) A P electrode and an N electrode are formed in the electrode through hole.

[0013] As an improvement of the above technical solution, it also includes forming a DBR layer on the dielectric layer; opening periodic conductive through holes in the dielectric layer and the DBR layer on the P-type semiconductor table to expose the transparent conductive layer, and forming a metal reflective layer in the periodic conductive through holes and on the DBR layer; and opening through holes in the dielectric layer and the DBR layer on the N-type semiconductor table to expose the N-type semiconductor layer.

[0014] As an improvement of the above technical solution, the diameter of the periodic conductive through-holes is 0.4 nm to 0.8 nm, and the distance between two adjacent periodic conductive through-holes is 10 nm to 20 nm.

[0015] As an improvement of the above technical solution, the DBR layer is a periodic structure formed by alternating stacking of two or more of SiO2, Ti3O5, TiO2, Si3N4, MgF2, CaF2, and ZrO2, with a period number of 2 to 10, and the thickness of the DBR layer is 100nm to 600nm.

[0016] As an improvement of the above technical solution, the DBR layer is a periodic structure formed by alternating Ti3O5 layers and SiO2 layers, with the number of periods being 2 to 4. In each period, the thickness of the Ti3O5 layer is 40nm to 70nm, and the thickness of the SiO2 layer is 30nm to 60nm.

[0017] As an improvement of the above technical solution, the material of the metal reflective layer is one or more of Ag, Al, Ni, Ti, and Au, and the thickness of the metal reflective layer is 100 nm to 150 nm.

[0018] As an improvement of the above technical solution, the material of the dielectric layer is one or more of SiO2, Al2O3, and ZnO, and the thickness of the dielectric layer is 450nm to 550nm.

[0019] As an improvement of the above technical solution, the material of the transparent protective layer is one or more of SiO2, Si3N4, TiO2, and the thickness of the transparent protective layer is 500nm to 800nm.

[0020] As an improvement of the above technical solution, the material of the P electrode and the N electrode is one or more of Cr, Ti, Ni, Pt, Au, Zn, Al, and Cu.

[0021] Correspondingly, the present invention further discloses a high-light-efficiency flip-chip LED chip, and the high-light-efficiency flip-chip LED chip is prepared by the above-mentioned preparation method of the high-light-efficiency flip-chip LED chip.

[0022] The implementation of the present invention has the following beneficial effects:

[0023] 1. The present invention sets periodic conductive through holes in the dielectric layer and deposits a metal reflective layer in the periodic conductive through holes. Compared with the traditional direct deposition of the metal reflective layer, this structure can take into account the requirements of reflectivity and conductivity. At the same time, the emitted light can utilize the reflection effect of the side walls of the periodic conductive through holes to increase the probability of light emission, thereby improving the light extraction efficiency of the chip.

[0024] 2. The present invention introduces a DBR layer into the metal reflective layer, which can improve its reflectivity in the entire spectral range and improve the problem of uneven reflectivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a schematic structural diagram of a high-light-efficiency flip-chip LED chip provided by the present invention after step S1;

[0026] Figure 2 is a schematic structural diagram of the high-light-efficiency flip-chip LED chip provided by the present invention after step S2;

[0027] Figure 3 is a schematic structural diagram of the high-light-efficiency flip-chip LED chip provided by the present invention after step S3;

[0028] Figure 4 is a schematic structural diagram of a high-light-efficiency flip-chip LED chip provided by the present invention after step S4;

[0029] Figure 5 is a schematic structural diagram of a high-light-efficiency flip-chip LED chip provided by the present invention after step S41;

[0030] Figure 6 is a schematic structural diagram of the high-light-efficiency flip-chip LED chip provided by the present invention after step S5;

[0031] Figure 7 is a schematic structural diagram of a high-light-efficiency flip-chip LED chip provided in Example 1 of the present invention;

[0032] Figure 8 It is a schematic structural diagram of a high-light-efficiency flip-chip LED chip provided in Example 2 of the present invention. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in further detail below.

[0034] A method for preparing a high-light-efficiency flip-chip LED chip, characterized by comprising the following steps:

[0035] S1, such as Figure 1 As shown, a substrate 100 is provided, and an epitaxial layer 200 is formed on the substrate 100 . The epitaxial layer 200 includes an N-type semiconductor layer 201 , an active layer 202 , and a P-type semiconductor layer 203 which are deposited in sequence.

[0036] In one embodiment, the epitaxial layer includes a gallium nitride buffer layer, an N-GaN layer, an InGaN / GaN MQWs layer, a P-AlGaN layer, and a P-GaN layer.

[0037] After the epitaxial wafer is prepared, the epitaxial wafer is cleaned, including ultrasonic treatment in acetone for 3 minutes to 6 minutes, shaking in isopropanol for 20 seconds to 40 seconds, and soaking in a sulfuric acid and hydrogen peroxide mixed solution for 3 minutes to 8 minutes.

[0038] S2, such as Figure 2 As shown, a transparent conductive layer 300 is formed on the P-type semiconductor layer, and a portion of the epitaxial layer is etched until the N-type semiconductor layer is exposed, thereby forming an N-type semiconductor mesa 11 and a P-type semiconductor mesa 12 .

[0039] Specifically, a pattern is made on the transparent conductive layer by photolithography technology, and the transparent conductive layer in a specific area is etched by wet etching using a photoresist as a mask, and then the epitaxial layer is etched to the N-type semiconductor layer by dry etching to form an N-type semiconductor table. The material of the transparent conductive layer can be one or more of ITO, InO, SnO, ATO, and ZnO. The current density directly below the transparent conductive layer is reduced, and the current is evenly distributed throughout the device, thereby improving the light extraction efficiency of the device.

[0040] S3, such as Figure 3 As shown, a dielectric layer 400 is formed on the N-type semiconductor mesa 11 , the P-type semiconductor mesa 12 and the mesa sidewall 13 .

[0041] The material of the dielectric layer is one or more of SiO2, Al2O3, and TiO2, and the thickness of the dielectric layer is 450nm to 550nm, and exemplarily is 460nm, 480nm, 500nm, 520nm or 540nm, but not limited thereto.

[0042] S4, such as Figure 4 As shown, a periodic conductive through hole 401 is opened in the dielectric layer 400 on the P-type semiconductor mesa 12 to expose the transparent conductive layer 300, and a metal reflective layer 500 is formed in the periodic conductive through hole 401 and on the dielectric layer 400; a through hole is opened in the dielectric layer 400 on the N-type semiconductor mesa 12 to expose the N-type semiconductor mesa 11.

[0043] Specifically, the diameter of the periodic conductive via 401 is 0.4nm to 0.8nm, and is exemplarily 0.45nm, 0.5nm, 0.55nm, 0.6nm, and 0.7nm, but not limited thereto. If the diameter of the periodic conductive via is less than 0.4nm, less light can be reflected by the side wall, and the effect of improving the luminous efficiency is not significant; if the diameter of the periodic conductive via is greater than 0.8nm, the improvement rate of the luminous efficiency is not high while increasing the amount of metal used in the metal reflective layer. The distance between two adjacent periodic conductive vias is 10nm to 20nm, and is exemplarily 12nm, 14nm, 15nm, 16nm or 18nm, but not limited thereto. Compared with directly setting the metal reflective layer on the P-type semiconductor layer, the setting of the periodic conductive via not only realizes the contact between the metal reflective layer and the transparent conductive layer, but also can make full use of the side wall of the periodic conductive via for light reflection.

[0044] The reflective layer can be made of a metal with a high reflectivity. Specifically, the material of the metal reflective layer can be one or more of Ag, Al, Ni, Ti, and Au. The thickness of the metal reflective layer is 100nm to 150nm. It should be noted that the thickness of the metal reflective layer does not include the portion in the periodic conductive vias. If the thickness of the metal reflective layer is less than 100nm, a good reflection effect cannot be obtained; if the thickness of the metal reflective layer is greater than 150nm, the cost is increased while the improvement of the reflection effect is not obvious.

[0045] In one embodiment, the following steps are also included:

[0046] S41, such as Figure 5As shown, a DBR layer 600 is formed on the dielectric layer 400; periodic conductive through holes 601 are opened in the dielectric layer 400 and the DBR layer 600 on the P-type semiconductor table 12 to expose the transparent conductive layer 300, and a metal reflective layer 500 is formed in the periodic conductive through holes 601 and on the DBR layer 600; through holes are opened in the dielectric layer 400 and the DBR layer 600 on the N-type semiconductor table 11 to expose the N-type semiconductor layer 11.

[0047] The DBR layer is a periodic structure formed by alternating two or more of SiO2, Ti3O5, TiO2, Si3N4, MgF2, CaF2, and ZrO2, and the number of periods is 2 to 10, and 3, 5, 7, 8, or 9 are exemplary, but not limited to these. The provision of the dielectric layer ensures the insulation performance and enriches the selection range of DBR materials. The thickness of the DBR layer is 100nm to 600nm, and 150nm, 200nm, 300nm, 400nm, or 500nm are exemplary, but not limited to these.

[0048] Preferably, the DBR layer is a periodic structure formed by alternating Ti3O5 layers and SiO2 layers, the number of periods is 2 to 4, and in each period, the thickness of the Ti3O5 layer is 40nm to 70nm, and the thickness of the SiO2 layer is 30nm to 60nm.

[0049] By opening periodic conductive through holes on the dielectric layer and the DBR layer and depositing a metal reflective layer, the DBR layer combined with the metal reflective layer can improve its reflectivity in the entire spectral range, improve the problem of uneven reflectivity, and greatly improve the luminous efficiency of the LED chip.

[0050] S5, forming a transparent protective layer 700 on the metal reflective layer 500 and the dielectric layer 400, and opening electrode through holes in the transparent protective layer 700 to expose the metal reflective layer 500 and the N-type semiconductor mesa 11 respectively.

[0051] In one embodiment, Figure 6 As shown, a transparent protective layer 700 is formed on the metal reflective layer 500 and the DBR layer 600 , and an electrode through hole is opened in the transparent protective layer 700 to expose the metal reflective layer 500 and the N-type semiconductor mesa 11 respectively.

[0052] The material of the transparent protective layer may be one or more of SiO2, Si3N4, and TiO2, and the thickness of the transparent protective layer is 500nm to 800nm.

[0053] S6. Form a P electrode 71 and an N electrode 72 in the electrode through hole.

[0054] The material of the P electrode and the N electrode is one or more of Cr, Ti, Ni, Pt, Au, Zn, Al, and Cu.

[0055] The present invention will be further described below with specific embodiments:

[0056] Example 1

[0057] This embodiment provides a method for preparing a high-light-efficiency flip-chip LED chip, comprising the following steps:

[0058] S1. Provide a sapphire substrate, and sequentially grow an N-type semiconductor layer, an active layer, and a P-type semiconductor layer on the sapphire substrate. The N-type semiconductor layer includes a 1μm GaN buffer layer and a 4μm N-GaN layer grown sequentially. The active layer is obtained by periodically overlapping an InGaN layer and a GaN layer. The growth cycle is 3. In each cycle, the thickness of the InGaN layer is 3nm, the thickness of the GaN layer is 12nm, and the P-type semiconductor layer includes a P-AlGaN layer and a P-GaN layer. The thickness of the P-type semiconductor layer is 20nm. The obtained epitaxial wafer is sequentially ultrasonicated in acetone for 5min, shaken in isopropanol for 30s, and immersed in a sulfuric acid and hydrogen peroxide mixed solution (the volume ratio of sulfuric acid to hydrogen peroxide is 5:1) at 90°C for 5min.

[0059] S2. Deposit an ITO transparent conductive layer with a thickness of 15 nm on the epitaxial wafer by magnetron sputtering, make a pattern on the ITO transparent conductive layer by photolithography technology, etch the ITO in a specific area by wet etching using photoresist as a mask, and then continue to etch the epitaxial layer to the N-GaN layer by dry etching process.

[0060] S3. Form a 500nm SiO2 dielectric layer on the N-type semiconductor mesas, the P-type semiconductor mesas and the sidewalls of the mesas.

[0061] S4. Periodic conductive through holes are opened in the SiO2 dielectric layer on the P-type semiconductor table to expose the ITO transparent conductive layer. The diameter of the periodic conductive through holes is 0.4nm, and the distance between two adjacent periodic conductive through holes is 10nm. Ag reflective layers are formed in the periodic conductive through holes and on the SiO2 dielectric layer. The thickness of the Ag reflective layer is 100nm. Through holes are opened in the SiO2 dielectric layer on the N-type semiconductor table to expose the N-type semiconductor table.

[0062] S5. A SiO2 transparent protective layer is formed on the Ag reflective layer and the SiO2 dielectric layer. The thickness of the SiO2 transparent protective layer is 600 nm. Electrode through holes are opened in the SiO2 transparent protective layer to expose the Ag reflective layer and the N-type semiconductor table, respectively.

[0063] S6. Form a P electrode and an N electrode in the electrode through hole, and the P electrode and the N electrode are both Ti / Al / Ni / Au.

[0064] Example 2

[0065] The present embodiment provides a method for preparing a high-light-efficiency flip-chip LED chip, which differs from Embodiment 1 in that S4 further includes forming a DBR layer on the SiO2 dielectric layer, the DBR layer being a periodic structure formed by alternating Ti3O5 layers and SiO2 layers, the number of periods being 2, and in each period, the thickness of the Ti3O5 layer is 40nm, and the thickness of the SiO2 layer is 30nm; periodic conductive through holes are opened in the SiO2 dielectric layer and the DBR layer on the P-type semiconductor table, the diameter of the periodic conductive through holes is 0.4nm, and the distance between two adjacent periodic conductive through holes is 10nm, exposing the ITO transparent conductive layer, and forming an Ag reflective layer in the periodic conductive through holes and on the DBR layer, the thickness of the Ag reflective layer is 150nm; through holes are opened in the SiO2 dielectric layer and the DBR layer on the N-type semiconductor table to expose the N-type semiconductor layer.

[0066] The rest are the same as in Example 1.

[0067] Example 3

[0068] This embodiment provides a method for preparing a high-light-efficiency flip-chip LED chip, which differs from Embodiment 2 in that the DBR layer is a periodic structure formed by alternating Ti3O5 layers and SiO2 layers, the number of periods is 3, and in each period, the thickness of the Ti3O5 layer is 60nm, and the thickness of the SiO2 layer is 40nm; after opening periodic conductive through holes, an Ag reflective layer is deposited, and the thickness of the Ag reflective layer is 120nm.

[0069] The rest is the same as Example 2.

[0070] Example 4

[0071] This embodiment provides a method for preparing a high-light-efficiency flip-chip LED chip, which differs from Embodiment 2 in that the DBR layer is a periodic structure formed by alternating Ti3O5 layers and SiO2 layers, the number of periods is 4, and in each period, the thickness of the Ti3O5 layer is 70nm, and the thickness of the SiO2 layer is 60nm; after opening periodic conductive through holes, an Ag reflective layer is deposited, and the thickness of the Ag reflective layer is 120nm.

[0072] The rest is the same as Example 2.

[0073] Example 5

[0074] This embodiment provides a method for preparing a high-light-efficiency flip-chip LED chip, which differs from Embodiment 2 in that the thickness of the SiO2 dielectric layer is 450 nm.

[0075] The rest is the same as Example 2.

[0076] Example 6

[0077] This embodiment provides a method for preparing a high-light-efficiency flip-chip LED chip, which differs from Embodiment 2 in that the thickness of the SiO2 dielectric layer is 550 nm.

[0078] The rest is the same as Example 2.

[0079] Comparative Example 1

[0080] This comparative example provides a method for preparing a flip-chip LED chip, which differs from Example 1 in that steps S3 to S5 are not performed, and an Ag reflective layer with a thickness of 120 nm is evaporated on the P-type semiconductor table using electron beam evaporation technology, and a SiO2 transparent protective layer with a thickness of 600 nm is deposited on the Ag reflective layer, the N-type semiconductor table and the side wall of the table, and electrode through holes are etched by dry etching to expose the Ag reflective layer and the N-type semiconductor table respectively.

[0081] The rest are the same as in Example 1.

[0082] The flip-chip LED chips prepared in Examples 1 to 6 and Comparative Example 1 were tested, and the brightness improvement rates of Examples 1 to 6 compared with Comparative Example 1 were calculated. The specific results are as follows:

[0083] Brightness increase rate Example 1 0.9% Example 2 2.1% Example 3 4.0% Example 4 3.3% Example 5 3.6% Example 6 3.3%

[0084] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.

Claims

1. A method for preparing a high-light-efficiency flip-chip LED chip, characterized in that: The following steps are involved: (1) providing a substrate, and forming an epitaxial layer on the substrate, wherein the epitaxial layer includes an N-type semiconductor layer, an active layer, and a P-type semiconductor layer deposited in sequence; (2) forming a transparent conductive layer on the P-type semiconductor layer, etching a portion of the epitaxial layer until the N-type semiconductor layer is exposed, and forming an N-type semiconductor mesa and a P-type semiconductor mesa; (3) forming a dielectric layer on the N-type semiconductor mesa, the P-type semiconductor mesa and the sidewalls of the mesa; (4) opening periodic conductive through holes in the dielectric layer on the P-type semiconductor mesa to expose the transparent conductive layer, and forming a metal reflective layer in the periodic conductive through holes and on the dielectric layer; and opening through holes in the dielectric layer on the N-type semiconductor mesa to expose the N-type semiconductor mesa; (5) forming a transparent protective layer on the metal reflective layer and the dielectric layer, and opening electrode through holes in the transparent protective layer to expose the metal reflective layer and the N-type semiconductor table respectively; (6) A P electrode and an N electrode are formed in the electrode through hole.

2. The method for preparing a high-efficiency flip-chip LED chip according to claim 1, characterized in that: The method also includes forming a DBR layer on the dielectric layer; opening periodic conductive through holes in the dielectric layer and the DBR layer on the P-type semiconductor table to expose the transparent conductive layer, and forming a metal reflective layer in the periodic conductive through holes and on the DBR layer; and opening through holes in the dielectric layer and the DBR layer on the N-type semiconductor table to expose the N-type semiconductor layer.

3. The method for preparing a high-light-efficiency flip-chip LED chip according to claim 1 or 2, characterized in that: The diameter of the periodic conductive through holes is 0.4 nm to 0.8 nm, and the distance between two adjacent periodic conductive through holes is 10 nm to 20 nm.

4. The method for preparing a high-light-efficiency flip-chip LED chip according to claim 2, characterized in that: The DBR layer is a periodic structure formed by alternately stacking two or more of SiO2, Ti3O5, TiO2, Si3N4, MgF2, CaF2, and ZrO2, with a period number of 2 to 10. The thickness of the DBR layer is 100nm to 600nm.

5. The method for preparing a high-light-efficiency flip-chip LED chip according to claim 4, characterized in that: The DBR layer is a periodic structure formed by alternately stacking Ti3O5 layers and SiO2 layers, with the number of periods being 2 to 4. In each period, the thickness of the Ti3O5 layer is 40nm to 70nm, and the thickness of the SiO2 layer is 30nm to 60nm.

6. The method for preparing a high-light-efficiency flip-chip LED chip according to claim 1 or 2, characterized in that: The material of the metal reflective layer is one or more of Ag, Al, Ni, Ti, and Au, and the thickness of the metal reflective layer is 100 nm to 150 nm.

7. The method for preparing a high-light-efficiency flip-chip LED chip according to claim 1 or 2, characterized in that: The material of the dielectric layer is one or more of SiO2, Al2O3, and ZnO, and the thickness of the dielectric layer is 450nm to 550nm.

8. The method for preparing a high-light-efficiency flip-chip LED chip according to claim 1 or 2, characterized in that: The material of the transparent protective layer is one or more of SiO2, Si3N4, and TiO2, and the thickness of the transparent protective layer is 500nm to 800nm.

9. The method for preparing a high-light-efficiency flip-chip LED chip according to claim 1 or 2, characterized in that: The material of the P electrode and the N electrode is one or more of Cr, Ti, Ni, Pt, Au, Zn, Al, and Cu.

10. A high-light-efficiency flip-chip LED chip, characterized in that: The high-light-efficiency flip-chip LED chip is prepared by the preparation method of the high-light-efficiency flip-chip LED chip according to any one of claims 1 to 9.

Citation Information

Cited By

  • Flip LED chip with special light pattern and preparation method thereof

    CN121262949A