Pre-lithiated positive electrode, preparation method and lithium ion battery
By forming an acid-based cladding layer on the surface of lithium oxide to isolate moisture and carbon dioxide in the air, the problem of instability of lithium oxide in lithium-ion batteries is solved, and the electrical performance and lithium-enhancing efficiency of lithium-ion batteries are improved.
Patent Information
- Application Number
- CN202410926735.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-11
AI Technical Summary
Lithium oxide in lithium-ion batteries has active chemical properties as a positive electrode lithium supplement additive and is prone to react with moisture and carbon dioxide in the air, resulting in a decrease in the specific capacity of lithium supplement and side reaction to produce gas, affecting battery performance.
By forming a cladding layer on the surface of lithium oxide, and reacting with lithium oxide using acids such as boric acid, phosphoric acid or polyphosphoric acid, a stable cladding layer is formed to isolate moisture and carbon dioxide in the air and prevent adverse reactions of lithium oxide.
It improves the stability of lithium oxide and the electrical performance of lithium-ion batteries, significantly improving the first charge and discharge capacity and Coulomb efficiency.
Smart Images

Figure BDA0004938422770000051
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a pre-lithiation positive electrode, a preparation method and a lithium ion battery. Background Art
[0002] As one of the most promising high-energy density storage devices, lithium-ion batteries have the advantages of high energy density, long cycle life, high safety, and environmental friendliness. They are widely used in electronic products, electric vehicles, aerospace, large energy storage power stations, etc. With the rapid development of new energy vehicles and the increase in driving range, higher requirements are placed on the energy density of batteries.
[0003] In order to further improve the energy density of lithium-ion batteries, replenishing lithium at the positive or negative electrode is an effective method. Compared with replenishing lithium at the negative electrode, replenishing lithium at the positive electrode is simpler, has relatively lower requirements on equipment and environment, is safer to use, and has relatively low cost.
[0004] Chinese patent CN107863567A discloses a lithium supplement additive and its preparation method and application. By doping lithium oxide powder with copper, the conductivity of lithium oxide powder is improved and the lithium oxide powder is used as a lithium supplement additive. As a positive electrode lithium supplement additive, although lithium oxide has a high specific capacity for lithium supplementation, lithium oxide has active chemical properties and easily absorbs moisture and carbon dioxide in the air to react and generate LiOH and Li2CO3. On the one hand, this will lead to a decrease in the specific capacity of lithium supplementation and poor lithium supplementation effect; on the other hand, the generated LiOH and Li2CO3 react with the electrolyte to cause serious gas production, affecting the performance of the lithium battery. Summary of the invention
[0005] The purpose of the present invention is to provide a pre-lithiation positive electrode with stable chemical properties; another purpose of the present invention is to provide a method for preparing a pre-lithiation positive electrode with stable chemical properties; another purpose of the present invention is to provide a lithium-ion battery with better first charge and discharge capacity and coulombic efficiency.
[0006] The present invention provides a pre-lithiation positive electrode, comprising a positive electrode current collector and a positive electrode active layer, wherein the positive electrode active layer comprises coated lithium oxide and a conductive agent; in parts by weight, the raw materials of the coated lithium oxide include:
[0007] 2-8 parts of lithium oxide;
[0008] Acid 0.1-0.8 parts.
[0009] Furthermore, in parts by weight, the raw materials for coating lithium oxide include:
[0010] 2-8 parts of lithium oxide;
[0011] Acid 0.4-0.8 parts.
[0012] Properly increasing the amount of acid can increase the thickness of the lithium oxide coating layer, thereby improving the stability of the coated lithium oxide.
[0013] The positive electrode current collector is aluminum foil. The conductive agent is selected from one or more of conductive carbon black, carbon nanotubes, and Ketjen black.
[0014] An appropriate amount of acid reacts with lithium oxide under suitable conditions to form a coating on the surface of lithium oxide, thereby isolating the lithium oxide from the air, thereby effectively preventing the lithium oxide from reacting with water and carbon dioxide in the air.
[0015] Furthermore, in the raw material for coating lithium oxide, the acid is selected from one or more of boric acid, phosphoric acid, polyphosphoric acid, oxalic acid, and silicic acid;
[0016] Furthermore, in the raw material for coating lithium oxide, the acid is selected from one of boric acid, phosphoric acid and polyphosphoric acid.
[0017] Boric acid, phosphoric acid, and polyphosphoric acid can form a more thermodynamically and kinetically stable coating on the surface of lithium oxide.
[0018] The present invention also provides a method for preparing a pre-lithiation positive electrode, comprising the following steps:
[0019] S1. Prepare the positive electrode current collector;
[0020] S2, preparing coated lithium oxide slurry: mixing lithium oxide and an organic solvent evenly to obtain lithium oxide slurry; mixing an acid and an organic solvent evenly to obtain an acid solution; adding the acid solution to the lithium oxide slurry, stirring sufficiently, reacting evenly, and obtaining coated lithium oxide slurry;
[0021] S3, preparing positive electrode active layer slurry: adding a conductive agent to the coated lithium oxide slurry obtained in the above step S2, stirring and mixing well to obtain a positive electrode active layer slurry;
[0022] S4, coating the positive electrode active layer slurry obtained in step S3 on the surface of the positive electrode current collector;
[0023] S5, drying, cold pressing, and obtaining the pre-lithiation positive electrode as described above.
[0024] Further, in step S2, the organic solvent is selected from one of N-methylpyrrolidone, ethylene carbonate, fluoroethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, methyl formate, ethyl formate, methyl acetate, ethyl acetate, ethyl propionate, propyl propionate, ethyl butyrate, propyl butyrate, ethylene glycol dimethyl ether, 1,3-dioxolane, 1,3-dioxane, dimethyl sulfoxide, and polyethylene glycol.
[0025] Furthermore, in step S2, the organic solvent is selected from one of N-methylpyrrolidone, dimethyl sulfoxide, and 1,3-dioxolane.
[0026] Furthermore, in step S2, in the lithium oxide slurry, the ratio of lithium oxide to organic solvent is 1:2-6 by mass; and in the acid solution, the mass ratio of the acid to the acid solution is 1-2%.
[0027] Furthermore, in step S3, the ratio of the lithium oxide: the acid: the conductive agent is 2-6:0.1-0.6:1 by mass.
[0028] Furthermore, in step S4, the coating surface density of the positive electrode active layer slurry is 10-20 g / m 2 .
[0029] The present invention also provides a lithium ion battery, comprising a pre-lithiation positive electrode prepared by the above preparation method.
[0030] The present invention discloses a pre-lithiation positive electrode, which uses coated lithium oxide as a positive electrode lithium supplement additive, and the coating layer has a protective effect on the lithium oxide, can isolate moisture and carbon dioxide in the air, prevent the lithium oxide from reacting to generate LiOH and Li2CO3, and effectively improve the stability of the pre-lithiation positive electrode in the air, thereby improving the electrical performance of the assembled lithium ion battery. DETAILED DESCRIPTION
[0031] The contents of the present application are described in more detail below through examples, but the following examples are only used to illustrate the contents of the present application rather than to limit them. Therefore, any changes within the meaning and scope equivalent to the claims of the present application should be deemed to be included in the scope of the claims.
[0032] The reagents, methods and equipment used in this application are conventional reagents, methods and equipment in the art. Unless otherwise specified, the reagents and materials used in this application are commercially available.
[0033] Example 1
[0034] Preparation of pre-lithiation cathode:
[0035] (1) Prepare aluminum foil as the positive electrode current collector.
[0036] (2) Preparation of coated lithium oxide slurry: 4 g of lithium oxide was added to 16 g of N-methylpyrrolidone solvent, and the mixture was stirred thoroughly to obtain lithium oxide slurry. 0.2 g of boric acid was added to N-methylpyrrolidone solvent to prepare 20 g of acid solution. The acid solution was slowly dripped into the lithium oxide slurry, and the mixture was stirred thoroughly to obtain coated lithium oxide slurry.
[0037] (3) Preparation of positive electrode active layer slurry: Add 1 g of conductive carbon black to the coated lithium oxide slurry and stir thoroughly to achieve a uniform reaction.
[0038] (4) The positive electrode active layer slurry is evenly coated on the surface of the aluminum foil, with a coating surface density of 14.6 g / m 2 (single side, based on the mass of the solid component excluding the solvent).
[0039] (5) drying and cold pressing to produce a pre-lithiation positive electrode.
[0040] Example 2
[0041] The preparation process is the same as that of Example 1, except that the amount of boric acid added in step (2) is different, that is, 0.4 g.
[0042] Example 3
[0043] The preparation process is the same as that of Example 1, except that the acid in step (2) is 0.2 g of phosphoric acid.
[0044] Example 4
[0045] The preparation process is the same as that of Example 1, except that the acid in step (2) is 0.4 g of phosphoric acid.
[0046] Example 5
[0047] The preparation process is the same as that of Example 1, except that the acid in step (2) is 0.2 g of polyphosphoric acid.
[0048] Example 6
[0049] The preparation process is the same as that of Example 1, except that the acid in step (2) is 0.4 g of polyphosphoric acid.
[0050] Example 7
[0051] The preparation process is the same as that of Example 2, except that the solvent of the acid in step (2) is different, namely, dimethyl sulfoxide.
[0052] Example 8
[0053] The preparation process is the same as that of Example 2, except that the solvent of the acid in step (2) is different, namely, 1,3-dioxolane.
[0054] Example 9
[0055] The preparation process is the same as that of Example 1, except that the acid in step (2) is 0.4 g of oxalic acid.
[0056] Example 10
[0057] The preparation process is the same as that of Example 1, except that the acid in step (2) is 0.4 g of silicic acid.
[0058] Comparative Example
[0059] The preparation process is the same as that of Example 1, except that no acid solution is added in step (2).
[0060] The compositions of Examples 1-10 are shown in Table 1.
[0061] Table 1 Composition of Examples 1-10
[0062] serial number Solvents Solute Example 1 N-Methylpyrrolidone Boric acid (5% by mass of lithium oxide) Example 2 N-Methylpyrrolidone Boric acid (10% by mass of lithium oxide) Example 3 N-Methylpyrrolidone Phosphoric acid (5% by mass of lithium oxide) Example 4 N-Methylpyrrolidone Phosphoric acid (10% by mass of lithium oxide) Example 5 N-Methylpyrrolidone Polyphosphoric acid (5% by mass of lithium oxide) Example 6 N-Methylpyrrolidone Polyphosphoric acid (10% by mass of lithium oxide) Example 7 Dimethyl sulfoxide Boric acid (10% by mass of lithium oxide) Example 8 1,3-Dioxolane Boric acid (10% by mass of lithium oxide) Example 9 N-Methylpyrrolidone Oxalic acid (10% by mass of lithium oxide) Example 10 N-Methylpyrrolidone Silicic acid (10% by mass of lithium oxide) Comparative Example N-Methylpyrrolidone /
[0063] Assemble into lithium-ion battery:
[0064] The pre-lithiated positive electrodes prepared in Examples 1-10 and the comparative examples were respectively assembled with the negative electrode, the separator, and the electrolyte to form a lithium-ion battery.
[0065] Preparation of electrolyte:
[0066] In an argon atmosphere glove box with a water content of <10ppm and an oxygen content of <10ppm, ethylene carbonate, diethyl carbonate, ethyl methyl carbonate and fluoroethylene carbonate are mixed according to mass percentages of 20%, 30%, 40% and 10% to obtain a mixed organic solvent, and then fully dried lithium salt lithium hexafluorophosphate is dissolved in the mixed organic solvent, the concentration of lithium hexafluorophosphate is 1 mol / L, and the additive is vinylene carbonate, which accounts for 1% by mass of the electrolyte. After stirring evenly, an electrolyte is obtained.
[0067] Diaphragm: A polyethylene porous membrane coated with alumina ceramic on both sides is used as the diaphragm.
[0068] Negative electrode: A metallic lithium sheet (0.6 mm thick, 99.9% purity) was used as the negative electrode.
[0069] Convert to lithium-ion battery:
[0070] The pre-lithiated positive electrode sheets prepared in Examples 1-10 and the comparative example were cut into discs with a diameter of 12 mm respectively, and then the positive electrode sheets, separators and metal lithium sheets were stacked in order with the separator in the middle to play an isolating role, and button cells were assembled. The amount of electrolyte added to each button cell was 150 μL.
[0071] Battery performance test:
[0072] At 25°C, the lithium ion batteries assembled in Examples 1-10 and the comparative example were first charged at a constant current of 0.02C to a voltage of 3.2V, then charged at a constant current of 0.2C to a voltage of 4.1V, and then charged at a constant current of 0.01C to a voltage of 4.35V. This was the first charging process. The first charging specific capacity of the battery assembled immediately after the positive electrode was prepared and the battery assembled after being placed in an environment of 10% humidity at 25°C for 3 days was tested respectively. The test results of the embodiments are shown in Table 2.
[0073] Table 2 First charge specific capacity of lithium ion batteries of Examples 1-10 and Comparative Examples
[0074]
[0075] Result analysis:
[0076] Compared with Examples 1-10, since the lithium oxide in Comparative Example 1 was not coated, the lithium oxide reacted with moisture and CO2 in the air, resulting in failure. The charging capacity in the first week after placement was greatly reduced.
[0077] Compared with Examples 9-10, the first charge specific capacity of the lithium-ion battery of Examples 1-8 is significantly better than that of Examples 9-10 after the electrode has been placed in an environment with a humidity of 10% for 3 days. This is because the added boric acid, phosphoric acid or polyphosphoric acid is used to coat the lithium oxide, and the resulting lithium borate or lithium phosphate coating has significantly better stability in the air than the lithium oxalate or lithium silicate coating. Therefore, it can significantly improve the stability of the pre-lithiation positive electrode in the air and effectively improve the first charge specific capacity.
[0078] Compared with Examples 2, 4, and 6, in Examples 1, 3, and 5, due to the small amount of acid added and the insufficient thickness of the coating layer, the first charge specific capacity of the electrode after being placed in an environment with a humidity of 10% for 3 days is lower than that of Examples 2, 4, and 6. It can be seen that sufficient acid needs to be added to form a coating layer of sufficient thickness to isolate moisture and CO2 in the air.
[0079] The initial charge specific capacity of the lithium-ion batteries of Examples 7 and 8 (after the pole pieces were placed in a 10% humidity environment for 3 days) was similar to that of Example 2, indicating that the solvent had little effect on the coating results.
[0080] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A pre-lithiation positive electrode, comprising a positive electrode current collector and a positive electrode active layer, characterized in that: The positive electrode active layer includes coated lithium oxide and a conductive agent; In parts by weight, the raw materials for coating lithium oxide include: 2-8 parts of lithium oxide; Acid 0.1-0.8 parts.
2. A pre-lithiation positive electrode according to claim 1, characterized in that: In the raw material for coating lithium oxide, the acid is selected from one or more of boric acid, phosphoric acid, polyphosphoric acid, oxalic acid and silicic acid.
3. A pre-lithiation positive electrode according to claim 1, characterized in that: In the raw material for coating lithium oxide, the acid is selected from one of boric acid, phosphoric acid and polyphosphoric acid.
4. A method for preparing a pre-lithiation positive electrode, characterized in that: The following steps are involved: S1. Prepare the positive electrode current collector; S2, preparing coated lithium oxide slurry: mixing lithium oxide and an organic solvent evenly to obtain lithium oxide slurry; mixing an acid and an organic solvent evenly to obtain an acid solution; adding the acid solution to the lithium oxide slurry, stirring sufficiently, reacting evenly, and obtaining coated lithium oxide slurry; S3, preparing positive electrode active layer slurry: adding a conductive agent to the coated lithium oxide slurry obtained in the above step S2, stirring and mixing well to obtain a positive electrode active layer slurry; S4, coating the positive electrode active layer slurry obtained in step S3 on the surface of the positive electrode current collector; S5, drying, cold pressing, and obtaining the pre-lithiation positive electrode as described in any one of claims 1 to 3.
5. The method for preparing a pre-lithiation positive electrode according to claim 4, characterized in that: In step S2, the organic solvent is selected from one of N-methylpyrrolidone, ethylene carbonate, fluoroethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, methyl formate, ethyl formate, methyl acetate, ethyl acetate, ethyl propionate, propyl propionate, ethyl butyrate, propyl butyrate, ethylene glycol dimethyl ether, 1,3-dioxolane, 1,3-dioxane, dimethyl sulfoxide, and polyethylene glycol.
6. The method for preparing a pre-lithiation positive electrode according to claim 5, characterized in that: In step S2, the organic solvent is selected from one of N-methylpyrrolidone, dimethyl sulfoxide, and 1,3-dioxolane.
7. The method for preparing a pre-lithiation positive electrode according to claim 4, characterized in that: In step S2, in the lithium oxide slurry, the ratio of lithium oxide to organic solvent is 1:2-6 by mass; in the acid solution, the mass ratio of the acid to the acid solution is 1-2%.
8. The method for preparing a pre-lithiation positive electrode according to claim 4, characterized in that: In step S3, the ratio of lithium oxide: acid: conductive agent is 2-6:0.1-0.6:1 by mass.
9. The method for preparing a pre-lithiation positive electrode according to claim 4, characterized in that: In step S4, the coating surface density of the positive electrode active layer slurry is 10-20 g / m 2 .
10. A lithium ion battery, characterized in that: It comprises a pre-lithiation positive electrode prepared by the preparation method according to any one of claims 5 to 9.
Citation Information
Patent Citations
Positive electrode lithium supplementing material, preparation method and application thereof
CN111370657A
Positive electrode lithium supplementing material and preparation method and application thereof
CN113526561A
Positive electrode lithium supplement agent and preparation method and application thereof
CN114530634A
Composite lithium supplement additive and lithium ion battery positive electrode lithium supplement method
CN114784268A
Lithium supplement additive, preparation method thereof and secondary battery
CN115347170A
Cited By
Pre-lithiated positive electrode, preparation method, and lithium-ion battery
WO2026011641A1