Electrode plate and preparation method thereof, battery and battery application
By preparing an electrode active layer on the substrate and stacking it with the current collector, the problem of binder floating was solved, the structural strength and cycle performance of the electrode sheet were enhanced, the production process was simplified, and the electrochemical performance and energy density of the battery were improved.
Patent Information
- Application Number
- CN202310502131.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-05-06
AI Technical Summary
The existing electrode sheets suffer from excessive binder content on the surface of the active layer due to the floating of binder during the drying process. This affects the electrochemical performance and structural stability, leading to problems such as powder shedding and material loss. Furthermore, traditional improvement methods are complex and costly.
By preparing an electrode active layer on the substrate and flipping it over to stack it with the current collector, a high binder content is ensured on the side of the electrode active layer closest to the current collector. A conductive binder layer is used to enhance the bonding strength, and a release surface is used to control the release force and thickness, thereby achieving efficient bonding between the electrode active layer and the current collector.
It significantly improves the structural strength and cycle performance of the electrode sheets, reduces powder shedding and material loss, enhances the cycle performance and energy density of the battery, simplifies the production process, and improves the production efficiency and yield of the electrode sheets.
Smart Images

Figure CN118919658A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of battery technology, and specifically relates to an electrode sheet and a preparation method thereof, a battery and battery applications. Background Art
[0002] Lithium-ion batteries have rapidly become popular in the fields of automotive power supply, 3C electronic products, and energy storage devices due to their high energy density and low self-discharge. With the popularization of lithium battery applications, the electrochemical properties of lithium batteries, such as cycle performance and production efficiency, are increasingly valued.
[0003] The electrode sheet is one of the important components in the battery, which generally includes a current collector and an electrode active layer combined with the current collector. Therefore, the quality of the electrode sheet is a key factor affecting the improvement of the electrochemical performance of the battery. However, based on the current production process of the electrode sheet, the binder in the electrode active layer contained in the electrode sheet will migrate to the surface of the electrode active layer through capillary force during the drying process as the solvent migrates to the electrode active layer during the evaporation process, resulting in the phenomenon of the binder floating, which leads to the performance of the electrode sheet, thereby at least affecting the electrochemical performance of the battery. Summary of the invention
[0004] In view of the above problems, the present application provides an electrode sheet and a preparation method thereof, a battery and a battery application, which can solve the problem that the binder in the electrode active layer contained in the electrode sheet floats up, resulting in the degradation of the performance of the electrode sheet and the battery.
[0005] In a first aspect, an embodiment of the present application provides a method for preparing an electrode sheet. The method for preparing an electrode sheet in an embodiment of the present application comprises the following steps:
[0006] Providing a substrate and a current collector, wherein the substrate has a release surface;
[0007] preparing an electrode active layer on the release surface of the substrate;
[0008] forming a conductive adhesive layer on the surface of the current collector and / or on the surface of the electrode active layer away from the substrate;
[0009] Performing a lamination and bonding treatment on the surface of the electrode active layer facing away from the substrate and the surface of the current collector to obtain a composite film;
[0010] During or after the lamination and bonding process, the substrate and the electrode active layer are separated to obtain an electrode sheet.
[0011] In the electrode sheet prepared by the preparation method of the electrode sheet of the embodiment of the present application, the content of the binder on the side of the electrode active layer close to the current collector is higher than that on the side away from the current collector. In this way, the bonding strength between the electrode active layer and the current collector is significantly enhanced, the structural strength of the electrode sheet is significantly enhanced, and the occurrence of undesirable phenomena such as powdering and material falling of the electrode active layer can be significantly reduced, thereby significantly improving the cycle performance of the electrode sheet and the battery.
[0012] In some embodiments, the release force of the release surface is 800-1200 gf / 25 mm. By selectively controlling the release force of the release surface, the quality of the prepared electrode active layer can be effectively improved, and the efficiency of the separation process of the electrode active layer and the substrate can be improved, and the adverse effects of the electrode active layer including damage during the separation process can be reduced, thereby improving the quality of the prepared electrode sheet.
[0013] In some embodiments, the release surface is coated with a release agent.
[0014] In an exemplary embodiment, the release agent includes at least one of a silicon-containing release agent and an alkane-based non-silicon release agent.
[0015] By coating the release agent on the release surface, or further selecting and controlling the type of the release agent, the release surface is endowed with good release performance and the quality of the prepared electrode active layer is improved.
[0016] In some embodiments, the substrate is a film that can be used for winding. The film that can be used for winding can realize substrate unwinding and winding processing, and the electrode active layer can be continuously prepared, thereby effectively improving the preparation efficiency of the electrode active layer.
[0017] In some embodiments, when the substrate is a film that can be rolled up, the thickness of the film is 20 to 100 μm, and can be 30 to 50 μm. This thickness range can effectively carry out unwinding and winding processing, and more importantly, has good mechanical properties, thereby improving the quality and thickness of the electrode active layer.
[0018] In some embodiments, the thickness of the electrode active layer is 50 to 250 μm, and can be 80 to 200 μm.
[0019] In some embodiments, the electrode active layer is a negative electrode active layer.
[0020] The electrode active layer prepared on the substrate, such as the negative electrode active layer, can be controlled to have a relatively large thickness, thereby significantly improving the energy density of the battery.
[0021] In the embodiment, the current collector is a negative electrode current collector, and the thickness of the negative electrode current collector is 4 to 6 μm. Within the thickness range of the negative electrode current collector, the negative electrode active layer can be made thicker than the thickness of the negative electrode active layer contained in the conventional negative electrode sheet, such as the thickness of the negative electrode active layer can be controlled to be 50 to 250 μm as mentioned above. Thereby, the energy density of the negative electrode sheet is improved.
[0022] In some embodiments, the conductive adhesive layer is formed to have a thickness of 1 to 3 μm.
[0023] In some embodiments, the conductive adhesive used to form the conductive adhesive layer includes at least one of a conductive pressure sensitive adhesive, a conductive acrylate adhesive, a conductive polyurethane adhesive, and a conductive polyimide resin adhesive.
[0024] The conductive adhesive layers and the conductive adhesive contained therein have strong bonding force and good conductivity, and can improve the structural strength and cycle performance of the electrode sheet and reduce the internal resistance.
[0025] In some embodiments, the lamination bonding process includes a step of laminating the composite film. The lamination process makes the electrode active layer and the current collector more firmly laminated under the action of the conductive adhesive layer, thereby enhancing the lamination bonding strength between the electrode active layer and the current collector and improving the structural strength and cyclability of the electrode sheet.
[0026] In an embodiment, the lamination treatment of the composite film comprises at least one of the following conditions (1) to (3):
[0027] (1) The pressure is 0.3-5 MPa, and can be selected as 0.5-3 MPa;
[0028] (2) The temperature is 10-100°C, and can be selected as 20-75°C;
[0029] (3) The pressing process is a roller pressing process.
[0030] In an embodiment, the conductive adhesive layer is a conductive pressure-sensitive adhesive layer.
[0031] By controlling at least one of the above (1) to (3) conditions for the lamination process, the strength of the stacking bond between the electrode active layer and the current collector can be enhanced, and the structural strength and cyclability of the electrode sheet can be improved. Among them, when the roller pressing process is adopted, the continuous production of the electrode sheet can be achieved, and the production efficiency of the electrode sheet is improved.
[0032] In a second aspect, the present application also provides an electrode sheet. The present application embodiment electrode sheet comprises a current collector and an electrode active layer combined with the current collector, the electrode active layer contains a binder, a conductive adhesive layer is stacked between the electrode active layer and the current collector; and in the electrode active layer, the content of the binder on the side close to the current collector is higher than the content of the binder on the side away from the current collector.
[0033] The distribution of the binder in the electrode active layer of the electrode sheet of the present application embodiment can cooperate with the conductive adhesive layer to significantly enhance the bonding strength between the electrode active layer and the current collector surface, thereby significantly improving the cycle performance of the electrode sheet and significantly improving the electrolyte wettability of the electrode active layer.
[0034] In some embodiments, the thickness of the electrode active layer is 50 to 250 μm, and can be 80 to 200 μm.
[0035] In some embodiments, the electrode active layer is a negative electrode active layer.
[0036] The electrode active layer contained in the electrode sheet of the embodiment of the present application, such as the negative electrode active layer, can be controlled to have a relatively large thickness, thereby significantly improving the energy density of the battery.
[0037] In some embodiments, the current collector is a negative electrode current collector, and the thickness of the negative electrode current collector is 4-6 μm.
[0038] When the electrode sheet of the embodiment of the present application is a negative electrode sheet, the thickness of the negative electrode current collector contained therein is within the thickness range, and the negative electrode active layer can be made thicker than the thickness of the negative electrode active layer contained in the conventional negative electrode sheet, such as the thickness of the negative electrode active layer can be controlled to be the above-mentioned 50 to 250 μm, thereby improving the energy density of the negative electrode sheet.
[0039] In some embodiments, the thickness of the conductive adhesive layer is 0.3-3 μm, and can be 0.5-1.5 μm.
[0040] In some embodiments, in some embodiments, the sheet resistance of the conductive adhesive layer is 0.001-0.1Ω, and can be optionally 0.001-0.01Ω.
[0041] The conductive adhesive layer within this thickness range effectively improves the strength of the stacking bond between the electrode active layer and the current collector, and can also reduce the resistance value at the interface between the electrode active layer and the current collector.
[0042] In a third aspect, the present application also provides a battery. The battery of the present application comprises an electrode, which is an electrode sheet prepared by the electrode sheet preparation method of the above application or an electrode sheet of the above application.
[0043] The battery of the embodiment of the present application has good cycle performance, and further has high energy density, and also has high rate performance.
[0044] In some embodiments, the battery includes any one of a battery cell, a battery module, and a battery pack.
[0045] In a fourth aspect, the embodiments of the present application further provide an electric device. The electric device of the embodiments of the present application includes a power supply unit or an energy storage unit, and the power supply unit or the energy storage unit contains a battery, and the battery includes the battery of the embodiments of the present application. The power supply unit or the energy storage unit of the electric device of the embodiments of the present application has good cycle performance and long service life, and can also have high energy density and other properties.
[0046] In a fifth aspect, the present application also provides an energy storage device, including an energy storage unit, wherein the energy storage unit contains a battery, wherein the battery includes the battery of the above-mentioned application embodiment. The energy storage device has good cycle performance, long service life, and further high energy density.
[0047] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present application. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the drawings:
[0049] Figure 1 This is a flowchart of a method for preparing an electrode sheet according to some embodiments of the present application;
[0050] Figure 2 The schematic diagram of the preparation method of the electrode sheet of some embodiments of the present application and the component structure of each step;
[0051] Figure 3 This is a schematic diagram of the structure of electrode sheets in some embodiments of the present application;
[0052] Figure 4 This is a schematic structural diagram of an implementation of a battery cell according to an embodiment of the present application;
[0053] Figure 5 for Figure 4 An exploded schematic diagram of the battery cell shown;
[0054] Figure 6This is a schematic structural diagram of an implementation scheme of a battery module according to an embodiment of the present application;
[0055] Figure 7 This is a schematic structural diagram of an implementation scheme of a battery pack according to an embodiment of the present application;
[0056] Figure 8 for Figure 7 A schematic diagram of the exploded structure of the battery pack shown;
[0057] Fig. 9 A schematic diagram of an embodiment of an electrical device including a battery according to an embodiment of the present application as a power source;
[0058] The reference numerals in the specific implementation manner are as follows:
[0059] 10-substrate, 11-release surface, 12-conductive adhesive layer;
[0060] 20-electrode sheet, 21-current collector, 22-electrode active layer, 23-conductive adhesive layer; 221-surface, 222-adhesive;
[0061] 30-battery cell, 31-housing, 32-electrode assembly, 33-cover plate;
[0062] 40-battery module;
[0063] 50-battery pack, 51-box, 52-lower box. DETAILED DESCRIPTION
[0064] The following embodiments of the technical solution of the present application will be described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0065] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0066] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0067] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0068] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0069] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0070] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.
[0071] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.
[0072] With the rapid popularization of lithium battery applications, especially in electric vehicles, the requirements for electrochemical performance of lithium battery, such as cycle performance, are becoming increasingly higher. Among them, the electrode sheet structure generally includes a current collector and an electrode active layer combined with the current collector. Therefore, the electrode sheet is a component used to provide active substances for battery chemical reactions and transmit electrons, and is one of the important components of the battery.
[0073] At present, the preparation process of electrode sheets usually includes: coating a slurry containing electrode active materials, conductive agents, binders and solvents on the surface of the current collector, and then drying, rolling, etc. Among them, the purpose of drying is mainly to remove the solvent in the slurry. However, during the drying process, the slurry solvent will migrate and evaporate to the surface of the electrode sheet through capillary force, while the density of the binder is relatively light, and it is easy to migrate and converge to the surface of the electrode active layer as the solvent migrates and evaporates to the surface of the electrode active layer, which leads to the problem of binder floating. The floating phenomenon of the binder will cause the binder content of the surface layer of the electrode active layer contained in the electrode sheet to be greater than the content on the side close to the current collector. On the one hand, the pores on the surface of the electrode active layer are blocked, reducing the wetting effect of the electrode active layer; the surface of the electrode active layer close to the current collector has a low binder content, resulting in a decrease in the adhesion between the electrode active layer and the current collector, which reduces the structural stability of the electrode sheet, and is prone to undesirable phenomena such as powdering and material falling off, and the electrode sheet is prone to edge burrs and other problems in the subsequent cutting process. This affects the electrochemical properties of the battery, including cycle performance.
[0074] In order to alleviate or solve the floating phenomenon of the binder contained in the electrode active layer in the electrode sheet, the relevant technology is generally to replace the binder or control the electrode active layer process, such as using multiple film formations to set the electrode active layer to a multi-layer structure. However, these methods still cannot effectively control the floating phenomenon of the binder, and will also lead to complicated electrode sheet production processes, thereby reducing the electrode sheet yield and increasing production costs.
[0075] In order to alleviate or overcome the floating phenomenon of the binder contained in the electrode active layer of the electrode sheet, the conventional electrode sheet production process is improved, the electrode active layer is first prepared separately, and then the electrode active layer is turned over, specifically, the surface with a high binder content in the electrode active layer is stacked and combined with the current collector. By preparing the electrode active layer separately and turning the electrode active layer over and stacking it with the current collector, it is effectively ensured that the binder content of the surface layer of the electrode active layer contained in the electrode sheet (the side of the surface layer of the electrode active layer away from the current collector) is lower than the binder content close to the current collector. Thereby, the surface of the electrode active layer contained in the electrode sheet (the side away from the current collector) has good electrolyte wettability, and the bonding strength between the electrode active layer and the current collector is effectively improved, so that the occurrence of undesirable phenomena such as powdering and material falling of the electrode sheet can be significantly reduced, and the electrochemical properties such as the cycle performance of the battery are significantly improved, and the production efficiency of the electrode sheet can also be effectively improved. Based on the above-mentioned research scheme, the embodiment of the present application proposes the following technical scheme.
[0076] Preparation method of electrode sheet
[0077] In the first aspect, the present application provides a method for preparing an electrode sheet. In some embodiments, the process flow of the method for preparing an electrode sheet provided in the present application is as follows: Figure 1 and Figure 2 As shown, the method for preparing the electrode sheet 20 provided in the embodiment of the present application comprises the following steps:
[0078] S10: providing a substrate 10 having a release surface 11 and a current collector 21;
[0079] S20: preparing an electrode active layer 22 on the release surface 11 of the substrate 10;
[0080] S30: forming a conductive adhesive layer 12 on the surface of the current collector 21 and / or the surface 221 of the electrode active layer 22 facing away from the substrate 10;
[0081] S40: performing a lamination and bonding treatment on the surface 221 of the electrode active layer 22 which is away from the substrate 1 and the surface of the current collector 2 to obtain a composite film;
[0082] S50 : during or after the lamination and bonding process, the substrate 10 and the electrode active layer 22 are separated to obtain the electrode sheet 20 .
[0083] Among them, the release surface 11 of the substrate 10 in step S10 refers to a surface that is easily separated from the electrode active layer 22 formed on its surface in step S20, and its function is the same as that of the release film surface. The electrode active layer 22 in step S20 refers to the positive electrode active layer or negative electrode active layer in the conventional sense, such as an electrode active material layer including an electrode active material, a conductive agent and a binder. The stacking and bonding treatment of the electrode active layer 22 and the current collector 2 refers to bonding the electrode active layer 22 and the current collector 2 together through the conductive adhesive layer 12 in step S30. The separation treatment of the substrate 10 and the electrode active layer 22 in step S50 refers to peeling or separating the substrate 10 from the surface of the electrode active layer 22.
[0084] Therefore, the preparation method of the electrode sheet 20 of the embodiment of the present application adopts the method of preparing the electrode active layer 22 separately, and then flipping it and laminating it on the surface of the current collector 21 to form the electrode sheet 20. Therefore, in the prepared electrode sheet 20, the side of the electrode active layer 22 contained therein close to the current collector 21 (that is, the side where the binder floats and gathers) has a binder 222 (such as Figure 2 The content of the electrode active layer 22 is higher than that on the side away from the current collector 21, thereby significantly enhancing the bonding strength between the electrode active layer 22 and the current collector 21, significantly enhancing the structural strength of the electrode sheet 20, and significantly reducing the occurrence of adverse phenomena such as powdering and material falling of the electrode active layer 22, thereby significantly improving the cycle performance of the electrode sheet 20 and the battery.
[0085] On the basis of giving the prepared electrode sheet 20 a high structural strength, since the preparation method of the electrode sheet 20 in the embodiment of the present application is to separate the electrode active layer 22 from the current collector 21 and prepare it separately, the electrode active layer 22 and the current collector 21 can be prepared separately or processed separately, which significantly improves the preparation efficiency of the electrode sheet 20. At the same time, the electrode active layer 22 is combined with the current collector 21 after being turned over in the manner in step S40, avoiding the problems of complex production process, low yield rate, high production cost caused by the multi-layer preparation of the electrode active layer to reduce the floating phenomenon of the binder, thereby improving the yield rate of the electrode sheet 20 on the basis of improving the high production efficiency of the electrode sheet 20.
[0086] Step S10:
[0087] The substrate 10 provided in step S10 is as follows Figure 2 As shown in Figure A, the current collector 21 provided is as follows Figure 2 As shown in Figure B.
[0088] The substrate 10 in step S10 is a substrate for the electrode active layer 22 prepared in step S20, and can also be called a carrier. Therefore, any substrate having a release surface 11 is within the scope disclosed in the embodiment of the present application.
[0089] In the embodiment, the substrate 10 may be a film that can be rolled up. In this way, the substrate unwinding and winding process can be realized, and the electrode active layer 22 in step S20 can be continuously prepared, thereby effectively improving the preparation efficiency of the electrode active layer 22.
[0090] In the embodiment, when the substrate 10 can be a film that can be used for winding, the thickness of the film can be 20-100 μm, optionally 30-50 μm, and in the exemplary embodiment, it can be 20-30 μm, 30-40 μm, 40-50 μm, 50-60 μm, 60-70 μm, 70-80 μm, 80-90 μm, 90-100 μm and other typical but not exclusive thickness ranges. This thickness range can effectively carry out unwinding and winding processing, and more importantly, it has good mechanical properties, which improves the quality and thickness of the electrode active layer 22 prepared in step S20. Among them, the thickness of the substrate 10 film is the distance between one surface of the film and the other surface relative to it. The thickness of each component below, such as the thickness of the current collector 21, the electrode active layer 22, the conductive adhesive layer 23, the conductive adhesive layer 12, etc., is the distance between one surface and the other surface relative to it.
[0091] In the exemplary embodiment, the substrate 10 may be an organic film, such as any one of PET film and PI film or a composite film of two or more thereof, or may be a composite film of two or more materials contained in the film layers.
[0092] The release surface 11 of the substrate 10 in step S10 not only enables the electrode active layer 22 in step S20 to be prepared on its surface, but also enables the electrode active layer 22 to be released from the substrate, that is, separated from the electrode active layer 22 during the separation process in step S50.
[0093] In the embodiment, the release force of the release surface 11 of the substrate 10 can be 800-1200 gf / 25mm, and in the exemplary embodiment, it can be 800-850 gf / 25mm, 850-900 gf / 25mm, 900-950 gf / 25mm, 950-1000 gf / 25mm, 1000-1050 gf / 25mm, 1050-1100 gf / 25mm, 1100-1150 gf / 25mm, 1150-1200 gf / 25mm, etc. The release force of the release surface 11 can be selectively controlled to effectively improve the quality of the electrode active layer 22 prepared in step S20, and the efficiency of the separation process in step S50 is also improved, and the adverse effects of the electrode active layer 22 including damage caused during the separation process are reduced, thereby improving the quality of the prepared electrode sheet 20. Among them, the release force data is obtained by testing using the TESA 7475TAPE method (the release force data below is tested using the same test method). Specifically, a TESA 7475 test tape with a length of 200 mm and a width of 25 mm is attached to the release surface 11 of the substrate 10, and then a 25 kg pressure roller is used to roll it back and forth three times with its own weight. After being placed under test conditions for 20 minutes, it is peeled off using a tensile tester at 300 mm / min and 180°, and the average of the 8 values is taken.
[0094] In the embodiment, the release surface 11 of the substrate 10 is coated with a release agent. In the exemplary embodiment, the release agent may include at least one of a silicon-containing release agent and an alkane-based non-silicon release agent. The silicon-containing release agent generally refers to an organic silicon release agent. In the exemplary embodiment, the organic silicon release agent may include polydimethylsiloxane (PDMS), methyl silicone oil, silane coupling agent, polydimethylsiloxane, hydrogenated polydimethylsiloxane (Hydrogenated PDMS) and other release agents. Alkane non-silicone release agents include fatty alcohol polyoxyethylene ethers (such as lauryl alcohol polyoxyethylene ether), fatty acid polyoxyethylene esters (such as lauryl acid polyoxyethylene ester), fatty alcohol polyoxypropylene ethers (such as lauryl alcohol polyoxypropylene ether), fatty acid polyoxypropylene esters (such as lauryl acid polyoxypropylene ester), fatty alcohol polyethylene ethers (such as lauryl alcohol polyethylene ether), fatty acid polyethylene esters (such as lauryl acid polyethylene ester), fatty alcohol polypropylene ethers (such as lauryl alcohol polyoxyethylene ether), fatty acid polypropylene esters (such as lauryl acid polypropylene ester) and the like release agents.
[0095] By coating the release agent on the release surface 11, or further selecting and controlling the type of the release agent, the release surface 11 is endowed with good release performance and the quality of the prepared electrode active layer 22 is improved. In addition, the amount of the release agent coated on the release surface 11, such as the content of the release agent per unit area, can be controlled to adjust the release force of the release surface 11, such as the release force of the release surface 11 can be adjusted to the above-mentioned 800-1200 gf / 25 mm.
[0096] The current collector 21 provided in step S10 may be a positive electrode current collector or a negative electrode current collector. In the embodiment, the current collector 21 includes but is not limited to a metal current collector, a carbon current collector, a conductive resin current collector, a composite current collector of metal and resin, and more specifically, copper, nickel, titanium, iron and their respective alloys, stainless steel, carbon fiber, carbon nanotube (CNT), graphite, etc. The current collector 21 may be flexibly selected according to the positive or negative polarity of the electrode sheet 20.
[0097] Since the electrode active layer 22 contained in the prepared electrode sheet 20 is first formed on the substrate 10, when the current collector 21 is within the conventional current collector thickness range, the electrode active layer 22 can be prepared with a thickness thicker than that of the electrode active layer contained in the relevant conventional electrode sheet, so that the energy density (such as mass energy density) of the prepared electrode sheet 20 can be effectively improved. When the electrode active layer 22 is a negative electrode active layer, the thickness of the negative electrode active layer can be controlled to be within the thickness range of 50 to 250 μm in step S20. Thereby, the energy density of the negative electrode sheet and the battery is improved.
[0098] Of course, the preparation method of the embodiment of the present application can also require the mechanical properties of the current collector 21 to be lower than the current collector contained in the conventional electrode sheet. Therefore, in the embodiment, the thickness of the current collector 21 can be thinner than the current collector contained in the conventional electrode sheet. For example, in the embodiment, when the current collector 21 is a negative electrode current collector, the thickness of the negative electrode current collector can be controlled to be 4 to 6 μm. In the demonstration example, it can be 4 to 4.5 μm, 4.5 to 5 μm, 5 to 5.5 μm, 5.5 to 6 μm, etc., which are typical but not the only limiting thicknesses. Of course, the thickness of the negative electrode current collector can also be adjusted to be relatively lower. Similarly, when the current collector 21 is a positive electrode current collector, the thickness of the positive electrode current collector can also be significantly reduced. In this way, the thickness of the current collector 21 contained in the electrode sheet 20 can be effectively reduced, and the thickness of the electrode active layer 22 can be correspondingly increased, thereby significantly improving the energy density of the electrode sheet 20 and the battery.
[0099] Step S20:
[0100] After the electrode active layer 22 is prepared on the release surface 11 of the substrate 10 in step S20, in one embodiment, the composite structure formed by the electrode active layer 22 and the substrate 10 is as follows: Figure 2 As shown in Figure C of FIG. Of course, when the substrate 10 has two release surfaces 11 disposed opposite to each other, the electrode active layer 22 can be prepared on both release surfaces 11 .
[0101] In step S20, the electrode active layer 22 can be prepared on the release surface 11 according to the conventional method of the electrode active layer, except that the conventional electrode active layer is prepared on the surface of the current collector, while in the electrode sheet preparation method of the embodiment of the present application, the electrode active layer is prepared on the release surface 11 of the substrate 10. Of course, the electrode active layer can also be prepared by an improved method of the conventional electrode active layer, or by a new method. As long as the electrode active layer is prepared on the release surface 11 of the substrate 10, it is within the scope disclosed in the embodiment of the present application.
[0102] In addition, the structure of the prepared electrode active layer 22 can be a single-layer electrode active layer or a composite structure electrode active layer formed by stacking multiple layers. Based on the preparation method of the electrode sheet 20 of the embodiment of the present application, the electrode active layer 22 can be a single layer, and it can still ensure that the content of the binder 222 on the side of the electrode active layer 22 close to the current collector 21 contained in the prepared electrode sheet 20 is higher than the content of the binder 222 on the side away from the current collector 21, such as Figure 2 The E to G diagram and Figure 3 In this way, the preparation efficiency of the electrode active layer 22 can be significantly improved on the basis of improving the structural strength and cycle performance of the prepared electrode sheet 20.
[0103] The method steps for preparing the electrode active layer 22 may include: preparing a slurry containing an electrode active material and a binder 222 and a solvent or further containing components such as a conductive agent and other additives, and forming the slurry into a film (wet film) on the release surface 11 of the substrate 10; then performing a drying process to evaporate the solvent, thereby drying the wet film; and then rolling the dried film layer to form the electrode active layer 22.
[0104] Among them, since the slurry contains a solvent, the solvent will gradually evaporate during the drying process of the wet film. The organic binder is an organic matter, which is a light component or can be miscible with the solvent. Therefore, in the process of gradual evaporation of the solvent and gradual migration from the inside of the wet film to the surface of the wet film, the binder will also migrate and converge toward the surface of the wet film along with the solvent. In this way, like the conventionally prepared electrode active layer, the electrode active layer 22 prepared in step S20 also has the phenomenon of binder floating. Specifically, Figure 2 As shown in Figure C, in the surface layer of the electrode active layer 22 facing away from the substrate 10, that is, in the surface layer having the surface 221 of the electrode active layer 22, the content of the binder 222 is higher than the content of the binder 222 in the surface layer close to the substrate 10.
[0105] In addition, since the electrode active layer 22 is prepared on the release surface 11 of the substrate 10, the mechanical properties of the substrate 10 can be enhanced by controlling the thickness, material and other factors of the substrate 10, so that the thickness of the prepared electrode active layer 22 can be effectively controlled, such as the thickness of the prepared electrode active layer 22 can be significantly increased. For example, in some embodiments, the thickness of the prepared electrode active layer 22 can be controlled to be 50-250 μm, and can be 80-200 μm. In the exemplary embodiment, it can be 50-80 μm, 80-100 μm, 100-120 μm, 120-150 μm, 150-180 μm, 200-220 μm, 220-250 μm and other typical but not exclusive limiting thickness ranges. Therefore, the electrode active layer 22 prepared on the substrate 10 in step S20 can be controlled to be relatively large in thickness, so that the energy density of the electrode sheet and the battery can be significantly improved. In addition, since the upper limit of the thickness of the electrode active layer 22 is relatively high, the thickness of the electrode active layer 22 can be flexibly adjusted and controlled within a relatively wide range according to production needs.
[0106] The electrode active layer 22 prepared in step S20 can be a positive electrode active layer or a negative electrode active layer. For example, in the embodiment, when the electrode active layer 22 is a negative electrode active layer, at this time, the thickness of the negative electrode active layer, that is, the electrode active layer 22, can be 50 to 250 μm, and can be 80 to 200 μm. Since conventional negative electrode sheet collectors such as copper foil are generally thin, if the negative electrode active layer is prepared on the surface of the negative electrode sheet collector such as copper foil according to the convention, the negative electrode active layer contained in the conventional negative electrode sheet is thin, which limits the improvement of the energy density of the battery. In the preparation method of the embodiment of the present application, since the electrode active layer 22 is prepared on the release surface 11 of the substrate 10, when the negative electrode active layer is prepared, the negative electrode active layer can be prepared relatively thick. For example, compared with the conventional method of directly preparing the negative electrode active layer on the negative electrode collector, the thickness of the negative electrode active layer prepared by the preparation method of the embodiment of the present application can be increased by 30% to 50%, which significantly improves the energy density of the electrode sheet and the battery.
[0107] Furthermore, since the electrode active layer 22 is prepared on the release surface 11 of the substrate 10 and then transferred and bonded to the current collector 21 in step S40, the thickness requirement of the current collector 21 in the preparation method of the embodiment of the present application can be reduced, such as the thickness requirement described in step S10.
[0108] In the embodiment, when the electrode active layer 22 prepared in step S20 is a negative electrode active layer, the negative electrode active material contained in the negative electrode active layer may include one or more of carbon-based active materials, titanium-based active materials, silicon-based active materials, nitrides, metallic lithium, etc. In the exemplary example, the carbon-based material may include one or more of graphite, hard carbon, soft carbon, mesophase carbon microspheres, graphene, etc.; in the exemplary example, the titanium-based active material includes one or more of lithium titanate, titanium dioxide, etc.; in the exemplary example, the silicon-based active material includes one or more of silicon, silicon dioxide, etc.; in the exemplary example, the nitride includes lithium nitride, etc.
[0109] In the embodiment, when the electrode active layer 22 prepared in step S20 is a positive electrode active layer, the positive electrode active material contained in the positive electrode active layer may include one or more of metal inorganic active materials and organic active materials. In the exemplary embodiment, the metal inorganic active material may include one or more of lithium iron phosphate, lithium manganese iron phosphate, lithium cobalt oxide, lithium manganese oxide, nickel cobalt manganese iron lithium, nickel cobalt aluminum oxide, etc. In the exemplary embodiment, the organic active material may include one or more of quinone compounds, carboxylate compounds, anhydride compounds, amide compounds, etc.
[0110] In the embodiment, the binder 222 contained in the electrode active layer 22 prepared in step S20 may include one or more of an oil-soluble binder, a water-soluble binder, an emulsion-type binder, etc. In an exemplary embodiment, the oil-soluble binder may include one or more of polyvinylidene fluoride, polyimide, polytetrafluoroethylene, polybutyl acrylate, polyacrylonitrile, etc.; in an exemplary embodiment, the water-soluble binder may include one or more of carboxymethyl cellulose, carboxymethyl cellulose salt, polyacrylic acid, polyacrylic acid salt, polyvinyl alcohol, sodium alginate, cyclodextrin, etc.; in an exemplary embodiment, the emulsion-type binder may include one or more of styrene-butadiene rubber, vinyl acetate resin, acrylic resin, and chlorinated rubber.
[0111] In an embodiment, when the electrode active layer 22 prepared in step S20 contains a conductive agent, the conductive agent may include one or more of acetylene black (SP), carbon nanotubes, conductive carbon black (super-P), Ketjen black, carbon fiber, graphene, and the like.
[0112] In the embodiment, when the electrode active layer 22 prepared in step S20 contains other additives, the additives may include but are not limited to functional components such as lithium supplementation.
[0113] The above-mentioned positive electrode active material, negative electrode active material, binder 222 and conductive agent and other materials can be selected according to the application or production requirements of the electrode sheet 20.
[0114] Step S30:
[0115] The conductive adhesive layer 12 formed in step S30 may be formed on the surface 221 of the electrode active layer 22 prepared in step S20 that is away from the substrate 10, or may be formed on the surface of the current collector 21 provided in step S20. Of course, the conductive adhesive layer 12 may be formed on both the surface 221 of the electrode active layer 22 and the surface of the current collector 21.
[0116] When the conductive adhesive layer 12 is formed on the surface of the current collector 21, in one embodiment, the composite structure formed by the conductive adhesive layer 12 and the current collector 21 is as follows: Figure 2 As shown in Figure D, of course, the conductive adhesive layer 12 can be formed on both opposite surfaces of the current collector 21.
[0117] In the embodiment, the thickness of the formed conductive adhesive layer 12 can be 1 to 3 μm. The conductive adhesive layer 12 in this thickness range can effectively achieve the stacking and bonding of the electrode active layer 22 and the current collector, and improve the structural strength of the prepared electrode sheet 20. Of course, the thickness of the conductive adhesive layer 12 can also be adjusted to other thickness ranges according to production requirements.
[0118] In the embodiment, the conductive adhesive used to form the conductive adhesive layer 12 includes at least one of a conductive pressure-sensitive adhesive, a conductive acrylate adhesive, a conductive polyurethane adhesive, and a conductive polyimide resin adhesive. In the exemplary embodiment, the conductive acrylate adhesive refers to a mixture of an acrylate adhesive and a conductive agent, the conductive polyurethane adhesive refers to a mixture of a polyurethane adhesive and a conductive agent, and the conductive polyimide resin adhesive refers to a mixture of a polyimide resin adhesive and a conductive agent. Among them, the conductive agent may include but is not limited to metal particles, conductive carbon and other conductive agents. These conductive adhesives have strong bonding force and good conductivity, can improve the structural strength and cycle performance of the electrode sheet, and reduce the internal resistance.
[0119] The method of forming the conductive adhesive layer 12 may be, but is not limited to, brush coating, roller coating, spray coating, and the like.
[0120] Step S40:
[0121] After the electrode active layer 22 and the current collector 21 are bonded according to the requirements of the lamination bonding process in step S40, a composite film is formed. In one embodiment, the composite film structure formed is as follows Figure 2 As shown in Figures E and F. Figure E shows a composite film structure in which the electrode active layer 22 and the current collector 21 are laminated and bonded according to the requirements of the lamination bonding treatment, and Figure F shows a composite film structure diagram after the conductive adhesive layer 12 is pressed or cured on the basis of the structure shown in Figure E.
[0122] Of course, the electrode active layer 22 may be laminated and bonded on both opposite surfaces of the current collector 21 , so that in the formed composite film, the electrode active layer 22 is laminated and bonded on both opposite surfaces of the current collector 21 contained therein through the conductive adhesive layer 12 .
[0123] Therefore, after the lamination and bonding process in step S40, the outer surface of the electrode active layer 22 prepared in step S20 becomes the inner surface of the electrode active layer 22 contained in the electrode sheet 20; at the same time, the conductive adhesive layer 12 becomes Figure 2 The conductive adhesive layer 23 is shown in FIG. F. At this time, the surface 221 of the electrode active layer 22 is close to the current collector 21. That is, after the electrode active layer 22 is bonded to the current collector 21, the surface layer where the binder 222 floats and aggregates during the drying process is close to the surface of the current collector 21. In this way, the strength of the stacking bond between the electrode active layer 22 and the current collector is effectively enhanced, and the structural strength of the prepared electrode sheet 20 is improved. The surface layer of the electrode active layer 22 close to the substrate 10 is far away from the surface of the current collector 10, and the content of the binder 222 in the surface layer is low due to the migration of the binder 222, so that it has a rich pore structure. After the substrate 10 is separated in step S50, the surface layer with a low content of the binder 222 has excellent electrolyte infiltration efficiency.
[0124] In some embodiments, the lamination bonding process in step S40 includes the step of laminating the composite film. The lamination process refers to applying pressure to two opposite surfaces of the composite film, so that the electrode active layer 22 and the current collector 21 are laminated more firmly under the action of the conductive adhesive layer 12 under the action of the external pressure, so as to enhance the lamination bonding strength between the electrode active layer 22 and the current collector 21, and improve the structural strength and cyclability of the electrode sheet 20.
[0125] In the embodiment, the lamination treatment of the composite film includes at least one of the following conditions (1) to (3):
[0126] (1) The pressure is 0.3-5 MPa, and may be 0.5-3 MPa. In the exemplary embodiment, the pressure may be 0.3-1 MPa, 1-2 MPa, 2-3 MPa, 3-4 MPa, 4-5 MPa, etc., which are typical but not the only limiting pressure ranges. In this pressure range, the pressing time should be sufficient to allow the electrode active layer 22 and the current collector 21 to be fully pressed together, thereby improving the bonding strength between the two.
[0127] (2) The temperature is 10-100° C., and can be 20-75° C. In the exemplary embodiment, it can be 10-30° C., 30-50° C., 50-70° C., 70-90° C., 90-100° C., etc. Typical but not exclusive limiting temperatures. The temperature of the lamination process can be flexibly controlled according to the type of the conductive adhesive.
[0128] (3) The pressing process is a roller pressing process.
[0129] By controlling at least one of the above (1) to (3), such as a combination of one or more of the above, the lamination strength between the electrode active layer 22 and the current collector 21 is further enhanced, thereby improving the structural strength and cyclability of the electrode sheet 20. When the rolling process is adopted, the continuous production of the electrode sheet 20 can be achieved, thereby improving the production efficiency of the electrode sheet.
[0130] In addition, the lamination process can be flexibly selected according to the different conductive adhesives contained in the conductive adhesive layer 12. For example, when the conductive adhesive layer 12 is a conductive hot melt adhesive layer, the temperature of the lamination process can be controlled to be 10-100°C, and can be optionally 20-75°C.
[0131] Embodiment, after the lamination and bonding process in the above step S40, the conductive adhesive layer 12 is pressed and cured to form a Figure 2 Middle G map and Figure 3The conductive adhesive layer 23 shown in . In the embodiment, the thickness of the conductive adhesive layer 23 can be 1-3 μm, and in the exemplary example, it can be a typical but not only limiting thickness range of 1-2 μm, 2-3 μm, etc. In the embodiment, the film resistance of the conductive adhesive layer 23 can be 0.001-0.1, and can be optionally 0.001-0.01. In the exemplary example, it can be controlled to be a typical but not only limiting film resistance of 0.001-0.005 μm, 0.005-0.01 μm, 0.01-0.03 μm, 0.03-0.05 μm, 0.05-0.08 μm, 0.08-0.10 μm, etc. Wherein, the film resistance refers to the resistance value measured along the thickness direction of the conductive adhesive layer 23. By controlling the thickness of the conductive adhesive layer 23, the stacking strength between the electrode active layer 22 and the current collector 21 can be effectively improved, and the structural strength and cyclability of the electrode sheet 20 can be improved. At the same time, the resistance between the interface of the electrode active layer 22 and the current collector 21 can be effectively reduced, thereby reducing the resistance of the prepared electrode sheet 20, thereby reducing the internal resistance of the battery and improving the battery's performance such as rate.
[0132] Step S50:
[0133] The separation process in step S50 is to separate the substrate 10 from the surface of the electrode active layer 22, so that the electrode active layer 22 is exposed, specifically, the surface of the side with less content of the binder 222 is exposed. In one embodiment, the electrode sheet structure obtained after the substrate 10 is separated is as follows: Figure 2 As shown in Figure G in FIG. Of course, the electrode sheet structure obtained after separating the substrate 10 can also be Figure 3 The structure shown is that the electrode active layer 22 is laminated and bonded on two opposite surfaces of the current collector 21 through the conductive adhesive layer 23.
[0134] In a second aspect, the present application also provides an electrode sheet. In some embodiments, such as Figure 2 Middle G map and Figure 3 As shown, the electrode sheet 20 of the embodiment of the present application includes a current collector 21, a conductive adhesive layer 23 and an electrode active layer 22. From the current collector 21 to the electrode active layer 22, the current collector 21, the conductive adhesive layer 23 and the electrode active layer 22 are stacked in sequence, that is, the conductive adhesive layer 23 is stacked between the electrode active layer 22 and the current collector 21.
[0135] In the electrode active layer 22 , the content of the binder 222 on the side close to the current collector 21 is higher than the content of the binder 222 on the side away from the current collector 21 .
[0136] Since the electrode active layer 22 contained in the electrode sheet 20 of the embodiment of the present application has a high content of binder 222 in the surface layer on the side close to the current collector 21, the binder 222 can cooperate with the conductive adhesive layer 23 to significantly enhance the surface bonding strength between the electrode active layer 22 and the current collector 21, thereby significantly improving the cycle performance of the electrode sheet 20. In addition, the content of binder 222 on the side of the electrode active layer 22 away from the current collector 21 is relatively low, so the surface layer on this side has abundant pores, which can significantly improve the electrolyte wettability of the electrode active layer 22.
[0137] In the embodiment, the current collector 21 contained in the electrode sheet 20 of the embodiment of the present application can be a positive electrode current collector or a negative electrode current collector. Moreover, based on the structure of the electrode sheet 20 of the embodiment of the present application and the preparation method of the electrode sheet 20 of the embodiment of the present application, the thickness of the current collector 21 can be thinner than the thickness of the current collector contained in the conventional electrode sheet. Specifically, it can be the thickness requirement or material type of the current collector 21 stated in step S10 of the preparation method of the electrode sheet 20 of the embodiment of the present application.
[0138] In the embodiment, the thickness of the electrode active layer 22 contained in the electrode sheet 20 of the embodiment of the present application can be 50-250 μm, and can be 80-200 μm. In the exemplary embodiment, it can be 50-80 μm, 80-100 μm, 100-120 μm, 120-150 μm, 150-180 μm, 200-220 μm, 220-250 μm, etc., which are typical but not the only limiting thickness ranges. Therefore, the electrode active layer 22 contained in the electrode sheet 20 of the embodiment of the present application can be controlled to be relatively thick, thereby significantly improving the energy density of the battery.
[0139] In the embodiment, the electrode active layer 22 may be a negative electrode active layer. At this time, the thickness of the negative electrode active layer may be 50 to 250 μm, and may be 80 to 200 μm. The thickness of the negative electrode active layer in the electrode sheet 20 of the embodiment of the present application is increased by 30% to 50% relative to the negative electrode active layer contained in the conventional negative electrode current collector, which significantly increases the energy density of the electrode sheet and the battery.
[0140] In the embodiment, the material of the electrode active layer 22 is the same as the material contained in the electrode active layer 22 prepared in step S20 of the method for preparing the electrode sheet 20 in the above-mentioned embodiment of the application, such as including electrode material, binder 222 or further including conductive agent or other additives.
[0141] When the electrode active layer 22 is a negative electrode active layer, that is, the electrode active layer 22 contains a negative electrode active material, the current collector 21 contained in the electrode sheet 20 of the embodiment of the present application corresponds to the negative electrode current collector. In the embodiment, the thickness of the negative electrode current collector at this time can be 4 to 6 μm. Therefore, the thickness of the negative electrode current collector contained in the electrode sheet 20 of the embodiment of the present application is within the thickness range, and the thickness of the negative electrode active layer contained therein may be thicker than the negative electrode active layer contained in the conventional negative electrode sheet, such as the 50 to 250 μm mentioned above, and the thickness range can be 80 to 200 μm. Thereby, the energy density of the electrode sheet and the battery can be further improved. Of course, the negative electrode current collector can also be controlled to be thinner.
[0142] The conductive adhesive layer 23 contained in the electrode sheet 20 of the embodiment of the present application is used to laminate and bond the surface 221 of the electrode active layer 22 with the current collector 21. In the embodiment, the thickness of the conductive adhesive layer 23 can be 0.3-3 μm, and can be optionally 0.5-1.5 μm. The conductive adhesive layer 23 in this thickness range effectively improves the strength of the laminated bonding between the electrode active layer 22 and the current collector 21, improves the structural strength and cyclability of the electrode sheet 20, and can effectively reduce the resistance between the interface of the electrode active layer 22 and the current collector 21, thereby reducing the resistance of the prepared electrode sheet 20, thereby reducing the internal resistance of the battery and improving the battery's rate performance. As in the embodiment, the film resistance of the conductive adhesive layer 23 is 0.001-0.1Ω, and can be optionally 0.001-0.01. It has high conductivity and low resistance.
[0143] Battery
[0144] In a third aspect, the present application also provides a battery. The battery of the present application comprises an electrode sheet, and the electrode sheet is the electrode sheet of the above-mentioned embodiment of the present application.
[0145] Among them, when the positive electrode of the battery of the embodiment of the present application is the electrode sheet of the embodiment of the above text application, then at this time, the electrode sheet of the embodiment of the above text application is a positive electrode sheet, and the current collector 21 contained therein is a positive electrode current collector, and the electrode active layer 22 is a positive electrode active layer; when the negative electrode of the battery of the embodiment of the present application is the electrode sheet of the embodiment of the above text application, then at this time, the electrode sheet of the embodiment of the above text application is a negative electrode sheet, and the current collector 21 contained therein is a negative electrode current collector, and the electrode active layer 22 is a negative electrode active layer. Of course, the positive electrode and the negative electrode of the battery can be the electrode sheets of the embodiment of the above text application at the same time.
[0146] Since the electrode of the battery of the embodiment of the present application is the electrode sheet of the embodiment of the present application, the battery of the embodiment of the present application has good cycle performance.
[0147] In the embodiment, since the electrode active layer 22 contained in the electrode sheet 20 of the above text application embodiment can be thicker than the electrode active layer contained in the conventional electrode sheet, and the current collector 21 can be thinner than the current collector contained in the conventional electrode sheet, that is, the energy density of the electrode sheet 20 of the above text application embodiment is higher than that of the conventional electrode sheet, therefore, the battery of the embodiment of the present application can further have a high energy density on the basis of having good cycle performance, and at the same time has high rate performance and the like.
[0148] In an embodiment, the battery of the embodiment of the present application may include any one of a battery cell, a battery module, and a battery pack.
[0149] The battery cell refers to a battery housing and an electrode assembly encapsulated in the battery housing. The shape of the battery cell is not particularly limited, and it can be cylindrical, square, or any other shape. In an exemplary embodiment, the battery cell can be Figure 4 The battery cell 30 shown has a square structure.
[0150] In some embodiments, Figure 5 As shown, the outer packaging of the battery cell 30 may include a shell 31 and a cover plate 33. The shell 31 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 31 has an opening connected to the receiving cavity, and the cover plate 33 is used to cover the opening to close the receiving cavity. The positive electrode, the separator and the negative electrode contained in the battery cell 30 of the embodiment of the present application can form an electrode assembly 32 through a winding process and / or a lamination process. The electrode assembly 32 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 32. The number of electrode assemblies 32 contained in the battery cell 30 may be one or more, which can be adjusted according to actual needs.
[0151] The preparation method of the battery cell 30 is well known. In some embodiments, the positive electrode, the separator, the negative electrode and the electrolyte can be assembled to form the battery cell 30. As an example, the positive electrode, the separator and the negative electrode can be formed into an electrode assembly 32 through a winding process or a lamination process, and the electrode assembly 32 is placed in an outer package, dried and injected with electrolyte, and then vacuum packaged, left to stand, formed, shaped and other processes are performed to obtain the battery cell 30.
[0152] The battery module is assembled from the battery cells 30 , that is, it may contain a plurality of the battery cells 30 , and the specific number can be adjusted according to the application and capacity of the battery module.
[0153] In some embodiments, Figure 6 FIG. 4 is a schematic diagram of a battery module 40 as an example. Figure 6As shown, in the battery module 50, the plurality of battery cells 30 may be arranged in sequence along the length direction of the battery module 40. Of course, they may also be arranged in any other manner. Further, the plurality of battery cells 30 may be fixed by fasteners.
[0154] Optionally, the battery module 40 may further include a housing having an accommodation space, and the plurality of battery cells 30 may be accommodated in the accommodation space.
[0155] A battery pack is composed of the above-mentioned battery cells 30, that is, it may contain multiple battery cells 30, wherein multiple battery cells 30 may be assembled into the above-mentioned battery module 50. The specific number of battery cells 30 or battery modules 40 contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0156] As in the embodiment, Figure 7 and Figure 8 is a schematic diagram of an example battery pack 50. The battery pack 50 may include a battery box and a plurality of battery modules 40 disposed in the battery box. The battery box includes an upper box body 51 and a lower box body 52, wherein the upper box body 51 is used to cover the lower box body 52 and form a closed space for accommodating the battery modules 40. The plurality of battery modules 40 may be arranged in the battery box in any manner.
[0157] Electrical devices
[0158] In the fifth aspect, the embodiments of the present application also provide an electric device. The electric device in the embodiments of the present application includes a power supply unit or an energy storage unit, and of course may also include other auxiliary components or necessary components. Among them, the power supply unit or energy storage unit contains the battery of the above-mentioned embodiment of the text application. The battery contained in the power supply unit or energy storage unit may be one or more. When there are multiple batteries, multiple batteries can form a battery module or battery pack. Since the electric device in the embodiments of the present application contains the battery of the above-mentioned embodiment of the text application, the power supply unit or energy storage unit of the electric device in the embodiments of the present application has good cycle performance and long service life, and further may have high energy density and other properties, and the standby or battery life of the electric device in the embodiments of the present application is long.
[0159] Fig. 9 Schematic diagram of an electric device as an example. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the requirements of the electric device for high power and high energy density, a battery pack or a battery module may be used.
[0160] As another example, the electric device may be a mobile phone, a tablet computer, a notebook computer, etc. The electric device is usually required to be light and thin, and a secondary battery may be used as a power source.
[0161] Energy storage device
[0162] In a sixth aspect, the embodiments of the present application also provide an energy storage device, which includes an energy storage unit and, of course, other auxiliary components or necessary components. Among them, the energy storage unit contains the battery of the above-mentioned embodiment of the text application. The battery contained in the energy storage unit may be one or more. When there are multiple batteries, multiple batteries can form a battery module or battery pack. Since the energy storage device of the embodiment of the present application contains the battery of the above-mentioned embodiment of the text application, the energy storage device has good cycle performance, long service life, and further high energy density.
[0163] Example
[0164] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0165] 1. Electrode sheet and preparation method thereof
[0166] Example A1
[0167] This embodiment provides a negative electrode sheet, including a copper foil and a negative electrode active layer, the negative electrode active layer is laminated and bonded to the surface of the copper foil through a conductive pressure-sensitive adhesive, and the surface of the negative electrode active layer that is gathered due to the floating of the binder during the drying process is also the side surface with a relatively high binder content facing the copper foil surface. The thickness of the copper foil is 4 μm, the thickness of the negative electrode active layer is 150 μm of the active material layer thickness, and the thickness of the conductive pressure-sensitive adhesive layer is 1 μm.
[0168] The method for preparing the negative electrode sheet of this embodiment includes the following steps:
[0169] S1. Preparation of negative electrode active layer:
[0170] S11: using silicon-carbon material as negative electrode active material, thickener CMC, binder styrene-butadiene rubber, and conductive agent SP, the mixture is mixed in a mass ratio of 90:1:2:7, deionized water is added, and negative electrode slurry is obtained under the action of a vacuum mixer, wherein the solid content of the negative electrode slurry is 45wt%;
[0171] S12: coating the negative electrode slurry prepared in step S11 on the surface of a PET film with a thickness of 50 μm, drying at 130° C., and the thickness of the negative electrode active layer is 150 μm; wherein the release force of the surface of the PET film used for coating the negative electrode slurry is 800 gf / 25 mm;
[0172] S2. The conductive pressure-sensitive adhesive slurry is coated on the surface of the 4μm thick copper foil, and a conductive adhesive layer is formed on the surface of the copper foil after drying;
[0173] S3. After laminating the surface of the copper foil containing the conductive adhesive layer with the surface of the negative electrode active layer prepared in step S1, the surface is subjected to a cold pressing treatment at 3 MPa, and the PET film is separated at the same time to obtain a negative electrode sheet.
[0174] Example A2
[0175] This embodiment provides a negative electrode sheet, which is the same as the negative electrode sheet in Embodiment A1, except that the preparation method of the negative electrode sheet in this embodiment is:
[0176] Compared with the negative electrode sheet preparation method in Example A1, the release force of the surface of the PET film used for coating the negative electrode slurry in step S12 is set to 1200 gf / 25 mm. The other steps are the same.
[0177] Example A3
[0178] This embodiment provides a negative electrode sheet, which is the same as the negative electrode sheet in Embodiment A1, except that the preparation method of the negative electrode sheet in this embodiment is:
[0179] Compared with the method for preparing the negative electrode sheet in Example A1, the method for preparing the negative electrode sheet in this embodiment is that the cold pressing process in step S3 is replaced by a hot pressing temperature of 80°C.
[0180] Example A4
[0181] This embodiment provides a negative electrode sheet. The negative electrode sheet is different from the negative electrode sheet in Embodiment A1 in that the thickness of the negative electrode active layer is 100 μm.
[0182] The preparation method of the negative electrode sheet of this embodiment refers to the preparation method steps and conditions in Example A1, and is adjusted in combination with the negative electrode sheet of this embodiment.
[0183] Comparative Example A1
[0184] This comparative example provides a negative electrode sheet, including a copper foil and a negative electrode active layer formed on the surface of the copper foil, wherein the surface of the negative electrode active layer where the binder floats up during the drying process is stacked away from the surface of the copper foil, and the surface with a relatively high binder content is stacked away from the surface of the copper foil. The thickness of the copper foil is 4 μm, and the thickness of the negative electrode active layer is 150 μm of the active material layer thickness.
[0185] The method for preparing the negative electrode sheet of this embodiment includes the following steps:
[0186] S1. Using silicon-carbon material as the negative electrode active material, thickener CMC, binder styrene-butadiene rubber, and conductive agent SP are mixed in a mass ratio of 90:1:2:7, deionized water is added, and a negative electrode slurry is obtained under the action of a vacuum mixer, and the solid content of the negative electrode slurry is 45wt%;
[0187] S2. The negative electrode slurry prepared in step S1 is coated on the surface of a 4 μm thick copper foil, dried at 130° C., the thickness of the active material layer is 100 μm, and then cold pressed to obtain a negative electrode sheet.
[0188] Comparative Example A2
[0189] This comparative example provides a negative electrode sheet. Compared with the negative electrode sheet in comparative example A1, the negative electrode sheet is different in that the thickness of the negative electrode active layer is 150 μm.
[0190] The preparation method of the negative electrode sheet of this comparative example refers to the preparation method steps and conditions in comparative example A1, and the negative electrode slurry is directly coated on the copper foil.
[0191] The electrode sheet related performance test methods are as follows:
[0192] (1) Observation of the morphology of the current collector and the electrode active layer contained in the electrode sheet during the coating process of the electrode slurry:
[0193] The electrode slurry coating condition of each electrode sheet was observed with the naked eye, and the morphology of the current collector and the electrode active layer contained in the prepared electrode sheet was observed with the naked eye.
[0194] (2) Adhesion test: The electrode sheet prepared in each example was stretched using a tensile machine at a stretching speed of 50 mm / min, and the 180° peeling adhesion was recorded;
[0195] The test results are shown in Table 1 below:
[0196] Table 1
[0197]
[0198]
[0199] From the data in Table 1, it can be seen from the comparison of Examples A1 to A4 with Comparative Examples A1 and A2 that, under the premise of ensuring high-quality coating of the electrode slurry, no belt breakage, and the quality of the electrode sheet meeting the requirements, the electrode sheet of the present application embodiment can be significantly increased in thickness relative to Comparative Example A1. For example, the negative electrode active layer of the negative electrode sheet of the present application can be 100 μm higher, and can be as high as 200 μm thick, and the quality of the negative electrode sheet can still meet the production requirements. When Comparative Example A2 directly forms a 150 μm negative electrode active layer on the surface of the copper foil, the slurry overflows and the copper foil breaks. Then, the aluminum foil and negative electrode active layer contained in the corresponding negative electrode sheet are wrinkled and broken, and the quality requirements of production cannot be met, indicating that the coating process and the abnormality of the negative electrode sheet in Comparative Example A2 indicate that the copper foil cannot withstand the weight of the slurry during thick coating.
[0200] In addition, during the test, the positive electrode sheet was prepared according to the methods of the above-mentioned embodiments A1 to A4. The thickness of the positive electrode current collector can be reduced and the thickness of the positive electrode active layer can be increased accordingly, and the quality of the positive electrode sheet can be ensured to meet the production requirements, without wrinkling of the positive electrode current collector and the positive electrode active layer, or breaking of the belt.
[0201] Therefore, by adopting the preparation method of the electrode sheet of the embodiment of the present application, the thickness of the electrode active layer can be relatively increased, and the electrode sheet can be produced normally, while the quality of the prepared electrode sheet meets the requirements, and the production efficiency of the electrode sheet can be improved.
[0202] 2. Secondary battery cell example
[0203] Examples B1 to B4 and Comparative Example B1;
[0204] Embodiments B1 to B4 and Comparative Example B1 each provide a secondary battery cell. Each secondary battery cell includes an electrode assembly formed of a positive electrode, a separator, and a negative electrode, and also includes an electrolyte.
[0205] The secondary battery cells in Examples B1 to B4 and Comparative Example B1 are assembled as follows:
[0206] Positive electrode sheet: The positive electrode active slurry is composed of NCM333, conductive carbon black SP and binder PVDF in a weight ratio of 97:1:2. After drying and cold pressing, it becomes the positive electrode sheet.
[0207] Negative electrode sheet: the negative electrode sheet provided by Examples A1 to A4 and Comparative Example A1 (the electrode sheet prepared in Comparative Example A2 was abandoned for assembly of battery cells due to obvious quality problems);
[0208] Electrolyte: The organic solvent is a mixed solution containing ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC), wherein the volume ratio of EC, EMC and DEC is 20:20:60. In an argon atmosphere glove box with a water content of <0.1ppm, fully dried lithium salt LiPF6 is dissolved in the organic solvent and mixed evenly to obtain an electrolyte. The concentration of the lithium salt is 1 mol / L.
[0209] Diaphragm: Use 10μm thick polypropylene isolation membrane.
[0210] Battery assembly: Assemble the hard shell cells of each lithium iron phosphate battery according to the battery assembly requirements and processes.
[0211] Secondary battery monomer related performance test:
[0212] Rate performance test: Each secondary battery cell assembled as above was discharged at 1C current, left to stand for 2 hours, and then charged at 3C current; 3C charging capacity / initial capacity*100% was calculated.
[0213] Capacity retention rate test: After 500 cycles of charge and discharge at 1C current, calculate its charge / discharge capacity / initial capacity*100%, which is the capacity retention rate.
[0214] Capacity test method: charge at 1C constant current to 4.2V at 25℃, then charge at constant voltage to current ≤0.5C, then discharge at 1C constant current to 2.8V. The discharge capacity is the battery capacity. Single cell mass energy density = battery capacity*3.6 / cell mass.
[0215] The relevant performance tests of secondary battery cells are shown in Table 2 below:
[0216] Table 2
[0217] Example Ratio 3C (%) 500cycle capacity retention rate % Capacity density Wh / kg Example A1 90.8 88 235 Example A2 91.0 87 238 Example A3 92.3 91 237 Example A4 90.1 87 251 Comparative Example A1 87.5 80 220
[0218] It can be seen from the data in Table 2 that the battery containing the embodiment of the present application has a significantly improved cycle performance relative to the battery provided by the comparative example due to the electrode sheet of the embodiment of the present application. It can be seen that, under the same conditions, the structural strength of the electrode sheet of the embodiment of the present application has been significantly improved, which has contributed to the cycle performance of the battery.
[0219] Furthermore, the battery rate performance is significantly improved. It can be seen that the electrode sheet of the embodiment of the present application can contribute to the energy density of the battery because the thickness of the electrode active layer can be made thicker, or the thickness of the current collector can be made relatively thinner.
[0220] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A method for preparing an electrode sheet, comprising the following steps: A substrate and a current collector are provided, wherein The substrate has a release surface; preparing an electrode active layer on the release surface of the substrate; forming a conductive adhesive layer on the surface of the current collector and / or on the surface of the electrode active layer away from the substrate; Performing a lamination bonding process on the surface of the electrode active layer facing away from the substrate and the surface of the current collector; A composite membrane is obtained; During or after the lamination and bonding process, the substrate and the electrode active layer are separated to obtain an electrode sheet.
2. The preparation method according to claim 1, characterized in that: The release force of the release surface is 800 to 1200 gf / 25 mm; and / or The release surface is coated with a release agent.
3. The preparation method according to claim 2, characterized in that: The release agent includes at least one of a silicon-containing release agent and an alkane-based non-silicon release agent.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The substrate is a film that can be used for winding.
5. The preparation method according to claim 4, characterized in that: The thickness of the film is 20-100 μm, and can be optionally 30-50 μm.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The thickness of the electrode active layer is 50 to 250 μm, and can be optionally 80 to 200 μm.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The electrode active layer is a negative electrode active layer.
8. The preparation method according to claim 7, characterized in that: The current collector is a negative electrode current collector, and the thickness of the negative electrode current collector is 4 to 6 μm.
9. The preparation method according to any one of claims 1 to 8, characterized in that: The thickness of the conductive adhesive layer is 1 to 3 μm; and / or The conductive adhesive used to form the conductive adhesive layer includes at least one of a conductive pressure sensitive adhesive, a conductive acrylate adhesive, a conductive polyurethane adhesive, and a conductive polyimide resin adhesive.
10. The preparation method according to any one of claims 1 to 9, characterized in that: The lamination bonding process includes the step of laminating the composite film.
11. The preparation method according to claim 10, characterized in that: The lamination treatment of the composite film includes at least one of the following conditions (1) to (3): (1) The pressure is 0.3-5 MPa, and can be selected as 0.5-3 MPa; (2) The temperature is 10-100°C, and can be selected as 20-75°C; (3) The pressing process is a roller pressing process.
12. The preparation method according to claim 11, characterized in that: The conductive adhesive layer is a conductive pressure-sensitive adhesive layer.
13. An electrode sheet comprising a current collector and an electrode active layer combined with the current collector, wherein the electrode active layer contains a binder, characterized in that: A conductive adhesive layer is stacked between the electrode active layer and the current collector; and in the electrode active layer, the content of the adhesive on the side close to the current collector is higher than the content of the adhesive on the side away from the current collector.
14. The electrode sheet according to claim 1, characterized in that: The thickness of the electrode active layer is 50 to 250 μm, and can be optionally 80 to 200 μm.
15. The preparation method according to any one of claims 13 to 14, characterized in that: The electrode active layer is a negative electrode active layer; and / or The current collector is a negative electrode current collector, and the thickness of the negative electrode current collector is 4 to 6 μm.
16. The preparation method according to any one of claims 13 to 15, characterized in that: The thickness of the conductive adhesive layer is 0.3 to 3 μm, and can be 0.5 to 1.5 μm; and / or The sheet resistance of the conductive adhesive layer is 0.001-0.1Ω, and can be optionally 0.001-0.01Ω.
17. A battery, characterized in that: The battery comprises an electrode sheet prepared by the preparation method according to any one of claims 1 to 12 or an electrode sheet according to claims 13 to 16.
18. The battery according to claim 17, characterized in that The battery includes any one of a battery cell, a battery module, and a battery pack.
19. An electrical device, characterized in that: It comprises a power supply unit or an energy storage unit, wherein the power supply unit or the energy storage unit contains a battery, and the battery comprises the battery according to claim 17 or 18.
20. An energy storage device, characterized in that: An energy storage unit is included, the energy storage unit comprising a battery, the battery comprising the battery of claim 17 or 18.
Citation Information
Patent Citations
Battery pole piece as well as manufacturing method thereof and lithium ion battery
CN108417776A
Raw electrode piece for manufacturing battery pole piece and manufacturing method of raw electrode piece
CN115986048A
Laminate type battery and method for producing the same
US20170279113A1