Composite positive electrode material and preparation method thereof, positive plate and secondary battery
By using composite positive electrode material in lithium cobalt oxide material and combining P63mc and crystalline positive electrode material design, the performance degradation problem of lithium cobalt oxide material at high voltage and low temperature is solved, and the cyclic stability at high voltage and Discharge performance at low temperatures is improved.
Patent Information
- Application Number
- CN202410852894.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-08
AI Technical Summary
Lithium cobalt oxide materials have performance degradation problems in high-rate charging and discharge and long-term circulation use, especially when structural collapse and irreversible phase change at high voltages lead to cyclic attenuation, and the improvement effect of doping coating is poor, and low-temperature performance deteriorates.
Using composite positive electrode materials, including P63mc crystal positive electrode materials and crystal positive electrode materials, through optimized particle size and proportion design, combined with the chemical formula of LiNiaMn2-a-bNbO4@LixNayCo1-zMzO2, the material structure is optimized using the characteristic peak strength relationship of XRD diffraction pattern. , improve the reversibility of the material and lithium ion diffusion channels, taking into account high voltage and low temperature performance.
Maintain good cycling performance at high voltages of 4.55V and above, and improve discharge performance under low temperature conditions, avoid irreversible capacity loss and structural collapse, and improve the structural stability and dynamic performance of the material.
Smart Images

Figure CN118919669A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of secondary batteries, and in particular to a composite positive electrode material and a preparation method thereof, a positive electrode sheet and a secondary battery. Background Art
[0002] Lithium cobalt oxide (LiCoO2) is one of the earliest commercially used materials in the field of lithium-ion battery positive electrode materials. With its high theoretical specific capacity and good electrochemical properties, it occupies an important position in many fields such as mobile electronic devices, electric vehicles and energy storage systems.
[0003] However, with the increasing requirements for lithium-ion battery performance, lithium cobalt oxide materials have exposed several limiting factors in commercial applications, especially the increasingly prominent performance degradation problem during high-rate charge and discharge and long-term cycle use. With the increase in energy density, at voltages of 4.55V and above, lithium cobalt oxide will undergo an irreversible phase transition from O3 to H1-3 and structural collapse, bringing serious cycle attenuation and safety risks, and the degree of irreversible phase transition of the material will increase. The effect of improving the cycle by doping and coating is not good; doping and coating will deteriorate the material kinetics and lead to deterioration of low-temperature performance.
[0004] Therefore, it is necessary to develop a composite positive electrode material that can effectively improve the material structure stability and low-temperature dynamics while taking into account the battery's cycle performance and low-temperature performance at high voltage. Summary of the invention
[0005] The purpose of the present invention is to provide a composite positive electrode material to address the deficiencies of the prior art, which can effectively improve the material structure stability and low-temperature kinetics while taking into account the cycle performance and low-temperature performance of the battery at high voltage.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] A composite positive electrode material comprises a first positive electrode active material and a second positive electrode active material, wherein the first positive electrode active material comprises a P63mc crystalline positive electrode active material, and the second positive electrode active material comprises Crystalline positive electrode active material;
[0008] The XRD diffraction spectrum of the composite positive electrode material contains at least three diffraction peaks in the range of 17.8° to 19°; wherein, there is a first diffraction peak in the range of 17.8° to 18.3°, with a peak intensity of I1; there are a second diffraction peak and a third diffraction peak in the range of 18.3° to 19.0°, with peak intensities of I2 and I3 respectively; the diffraction peak intensities I1, I2 and I3 satisfy the relationship: I2 / I1≥2, I3 / I1≥2, 0.5≤I3 / I2≤2.
[0009] Among them, the P63mc crystalline cathode material is highly reversible at high voltage, reducing irreversible capacity loss; The positive electrode material with crystalline structure has three-dimensional lithium ion diffusion channel, and lithium ions can be quickly released under high voltage, which improves the low-temperature discharge performance of the composite material. The particle size design and proportion design of the crystalline positive electrode material can make the composite material have both cycle performance and low temperature performance.
[0010] Preferably, the average particle size of the first positive electrode active material is D1, and the average particle size of the second positive electrode active material is D2, and the value range of D1 is: 5μm≤D1≤20μm; R1 is too large, which is not conducive to lithium ion diffusion; R1 is too small, the active surface of the reaction with the electrolyte increases, the side reactions increase, and it is not conducive to circulation. The value range of D2 is: 1μm≤D2≤10μm; R2 is too large, the kinetic performance is poor, and it worsens at low temperatures; R2 is too small, which makes manganese dissolution more severe and is not conducive to processing.
[0011] Preferably, the chemical formula of the composite positive electrode material is:
[0012] LiNi a Mn 2-a-b N b O4@Li x Na y Co 1-z M z O2, wherein M and N include at least one of Al, Mg, Ti, La, Y, Zn, Ni, Mn, Co, V, and Si elements; wherein 0≤a≤0.6, 0≤b<0.02; 0.7≤x<1, 0.01<y<0.1, 0≤z<0.02.
[0013] Preferably, the first positive electrode active material is Li x Na y Co 1-z M z O2, the second positive electrode active material is LiNi a Mn 2-a- b N b O4.
[0014] Preferably, the mass of the first positive electrode active material is m1, and the mass of the second positive electrode active material is m2, wherein m1 and m2 satisfy the relationship: 0<m2 / m1≤1. The second positive electrode active material has a low gram capacity, and a high ratio of m2 / m1 will result in a decrease in the gram capacity of the composite material.
[0015] In addition, the present invention also provides a method for preparing a composite positive electrode material, comprising the following steps:
[0016] S1: Mix the cobalt salt solution and the salt solution of the doping element M evenly, add an excess of the precipitant solution, stir and filter to obtain a precipitate; sinter the precipitate at 400°C to 600°C for 6 to 12 hours to obtain (Co 1-z M z )3O4 powder;
[0017] S2:Co 1-z M z )3O4 and sodium salt are mixed uniformly; sintered at 800℃~1100℃ for 45~52h to obtain Na with P63mc crystal structure n Co 1-z M z O2, where 0.5≤n≤0.7;
[0018] S3: Put Na n Co 1-z M z O2 is dispersed in the lithium salt solution, mixed evenly in a ratio of Li to Na molar ratio ≥5, reacted in a reactor at 140-160°C for 22-26h, filtered, rinsed with deionized water, dried, and crushed to obtain Li x Na y Co 1- z M z O2 positive electrode active material;
[0019] S4: The nickel salt solution, the manganese salt solution, and the salt solution doped with element N are mixed evenly according to the molar ratio of Ni, Mn, and N being a: (2-ab): b to form a mixed solution, and then the mixed solution is mixed with the carbonate solution according to the molar ratio of (Ni+N+Mn) to carbonate ions being 1:2, and filtered to obtain Ni a Mn 2-a-b N b CO3 precipitation; then Ni a Mn 2-a-b N b The CO3 precipitate is mixed evenly with the lithium salt to make the molar ratio of Li to (Ni+Mn+N) be (1.0-1.4): (1.8-2.2), and then sintered at 750-1000℃ for 8-12h to obtain LiNi a Mn 2-a-b N b O4 positive electrode active material;
[0020] S5: After mixing the materials prepared in steps S3 and S4 according to a certain proportion, sintering at 700-800° C. for 5-8 hours, a composite positive electrode material is obtained.
[0021] Preferably, in step S1, the molar ratio of Co to M in the cobalt salt solution and the salt solution of the doping element M is (1-z):z, where 0≤z<0.02. When z is too large, the doping amount is too much, which is not conducive to particle growth.
[0022] Among them, if the value of n in step S2 is too large, it will lead to the presence of impurities in the P63mc material after ion exchange, and if it is too small, it will lead to a low Li / Co ratio of the P63mc material after ion exchange, which is not conducive to gram capacity.
[0023] Preferably, in step S2, (Co 1-z M z )3O4 and Na2CO3 are mixed in a molar ratio of Na to Co of (0.5-0.7):(1-1.2).
[0024] Preferably, the molar ratio of Li to Na in step S3 is 10. Too low a Li / Na ion exchange efficiency is low.
[0025] Preferably, in step S3, the molar ratio of (Ni+N+Mn) to carbonate ions is 1:2, and the excess carbonate ions allow the metal ions to be fully precipitated.
[0026] Preferably, in step S4, the molar ratio of Li to (Ni+Mn+N) is 1.2:2, and the excess lithium salt prevents the volatilization of Li during high-temperature calcination, resulting in lithium deficiency.
[0027] In addition, the present invention also provides a positive electrode sheet, comprising the above-mentioned composite positive electrode material.
[0028] In addition, the present invention also provides a secondary battery, including a battery cell formed by winding a negative electrode sheet, a positive electrode sheet and a separator, an electrolyte, and a shell that encapsulates the battery cell and the electrolyte, wherein the positive electrode sheet is the above-mentioned positive electrode sheet.
[0029] Compared with the prior art, the beneficial effect of the present invention is that the composite positive electrode material provided by the present invention can still have good cycle performance and low temperature performance at a high voltage of 4.55V and above. Among them, the P63mc crystal positive electrode material in the composite material has a unique coplanar connection of LiO6 octahedron and CoO6 octahedron, and only the slip of the CoO2 layer and the arrangement of Li vacancies appear under high voltage, which is highly reversible and avoids the cycle attenuation caused by irreversible capacity loss; the positive electrode material with Fd3m crystal phase structure has a three-dimensional lithium ion diffusion channel, and lithium ions can be quickly released under high voltage, which improves the low-temperature discharge performance of the composite positive electrode material. DETAILED DESCRIPTION
[0030] In order to make the technical solutions and advantages of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] According to a first aspect of the present application, the present application provides a composite positive electrode material, comprising a first positive electrode active material and a second positive electrode active material, wherein the first positive electrode active material comprises a P63mc crystal type positive electrode active material, and the second positive electrode active material comprises a Fd3m crystal type positive electrode active material;
[0032] The XRD diffraction spectrum of the composite positive electrode material contains at least three diffraction peaks in the range of 17.8° to 19°; wherein, there is a first diffraction peak in the range of 17.8° to 18.3°, with a peak intensity of I1; there are a second diffraction peak and a third diffraction peak in the range of 18.3° to 19.0°, with peak intensities of I2 and I3 respectively; the diffraction peak intensities I1, I2 and I3 satisfy the relationship: I2 / I1≥2, I3 / I1≥2, 0.5≤I3 / I2≤2.
[0033] In some embodiments, the average particle size of the first positive electrode active material is D1, and the average particle size of the second positive electrode active material is D2; wherein the value range of D1 is: 5μm≤D1≤20μm, for example, it can be 5μm, 7μm, 9μm, 11μm, 13μm, 15μm, 17μm, 19μm, 20μm; the value range of D2 is: 1μm≤D2≤10μm, for example, it can be 1μm, 2μm, 4μm, 6μm, 8μm, 10μm.
[0034] In some embodiments, the chemical formula of the composite cathode material is: LiNi a Mn 2-a-b N b O4@Li x Na y Co 1-z M z O2, wherein M and N include at least one of Al, Mg, Ti, La, Y, Zn, Ni, Mn, Co, V, and Si elements; wherein 0≤a≤0.6, 0≤b<0.02; 0.7≤x<1, 0.01<y<0.1, 0≤z<0.02.
[0035] In some embodiments, the first cathode active material is Li x Na y Co 1-z M zO2, the second positive electrode active material is LiNi a Mn 2-a-b N b O4.
[0036] In some embodiments, the mass of the first positive electrode active material is m1, and the mass of the second positive electrode active material is m2, wherein m1 and m2 satisfy the relationship: 0<m2 / m1≤1.
[0037] According to a second aspect of the present application, the present application provides a method for preparing a composite positive electrode material, comprising the following steps:
[0038] S1: Mix the cobalt salt solution and the salt solution of the doping element M evenly, add an excess of the precipitant solution, stir and filter to obtain a precipitate; sinter the precipitate at 400°C to 600°C for 6 to 12 hours to obtain (Co 1-z M z )3O4 powder;
[0039] S2:Co 1-z M z )3O4 and sodium salt are mixed uniformly; sintered at 800℃~1100℃ for 45~52h to obtain Na2O4 with P63mc crystal structure n Co 1-z M z O2, where 0.5≤n≤0.7;
[0040] S3: Put Na n Co 1-z M z O2 is dispersed in the lithium salt solution, mixed evenly in a ratio of Li to Na molar ratio ≥5, reacted in a reactor at 140-160°C for 22-26h, filtered, rinsed with deionized water, dried, and crushed to obtain Li x Na y Co 1- z M z O2 positive electrode active material;
[0041] S4: The nickel salt solution, the manganese salt solution, and the salt solution doped with element N are mixed evenly according to the molar ratio of Ni, Mn, and N being a: (2-ab): b to form a mixed solution, and then the mixed solution is mixed with the carbonate solution according to the molar ratio of (Ni+N+Mn) to carbonate ions being 1:2, and filtered to obtain Ni a Mn 2-a-b N b CO3 precipitation; then Ni a Mn 2-a-b N bThe CO3 precipitate is mixed evenly with the lithium salt to make the molar ratio of Li to (Ni+Mn+N) be (1.0-1.4): (1.8-2.2), and then sintered at 750-1000℃ for 8-12h to obtain LiNi a Mn 2-a-b N b O4 positive electrode active material;
[0042] S5: After mixing the materials prepared in step S3 and S4 according to a certain proportion, sintering at 700-800° C. for 5-8 hours, the composite positive electrode material is obtained.
[0043] In some embodiments, in step S1, the molar ratio of Co to M in the cobalt salt solution and the salt solution of the doping element M is (1-z):z, wherein 0≤z<0.02.
[0044] In some embodiments, in step S2, (Co 1-z M z )3O4 and Na2CO3 are mixed in a molar ratio of Na to Co of (0.5-0.7):(1-1.2).
[0045] In some embodiments, the lithium salt solution in step S3 includes but is not limited to lithium nitrate, lithium chloride, etc.
[0046] In some embodiments, the nickel salt solution in step S4 includes but is not limited to nickel chloride, nickel sulfate, nickel nitrate, etc.; the manganese salt solution includes but is not limited to manganese chloride, manganese sulfate, manganese nitrate, etc.; the salt solution doped with element N includes but is not limited to aluminum sulfate, magnesium sulfate, etc.
[0047] According to a third aspect of the present application, the present application provides a positive electrode sheet, comprising a positive electrode current collector and a positive electrode active material layer coated on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer comprises the above-mentioned composite positive electrode material.
[0048] According to the fourth aspect of the present application, the present application provides a secondary battery, including a battery cell formed by winding a negative electrode sheet, a positive electrode sheet and a separator, an electrolyte, and a shell that encapsulates the battery cell and the electrolyte, wherein the positive electrode sheet is the above-mentioned positive electrode sheet.
[0049] The negative electrode plate includes a negative electrode current collector and a negative electrode active material layer coated on at least one surface of the negative electrode current collector. The negative electrode active material layer may include but is not limited to one or more of graphite, soft carbon, hard carbon, carbon fiber, mesophase carbon microspheres, silicon-based materials, tin-based materials, lithium titanate or other metals that can form alloys with lithium. Among them, graphite can be selected from one or more of artificial graphite, natural graphite and modified graphite; silicon-based materials can be selected from one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, and silicon alloys; tin-based materials can be selected from one or more of elemental tin, tin oxide compounds, and tin alloys. The negative electrode current collector is usually a structure or part that collects current. The negative electrode current collector can be various materials in the art that are suitable for use as a negative electrode current collector for lithium-ion batteries. For example, the negative electrode current collector may include but is not limited to metal foil, and more specifically may include but is not limited to copper foil.
[0050] The separator can be any material suitable for lithium-ion battery separators in the art, for example, it can be a combination of one or more materials including but not limited to polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester and natural fibers.
[0051] The lithium-ion battery also includes an electrolyte, which includes an organic solvent, an electrolyte lithium salt and an additive. Among them, the electrolyte lithium salt can be LiPF6 and / or LiBOB used in high-temperature electrolytes; it can also be at least one of LiBF4, LiBOB, and LiPF6 used in low-temperature electrolytes; it can also be at least one of LiBF4, LiBOB, LiPF6, and LiTFSI used in anti-overcharge electrolytes; it can also be at least one of LiClO4, LiAsF6, LiCF3SO3, and LiN(CF3SO2)2. The organic solvent can be a cyclic carbonate, including PC and EC; it can also be a chain carbonate, including DFC, DMC, or EMC; it can also be a carboxylic acid ester, including MF, MA, EA, MP, etc. The additives include but are not limited to at least one of film-forming additives, conductive additives, flame retardant additives, anti-overcharge additives, additives for controlling the content of H2O and HF in the electrolyte, additives for improving low-temperature performance, and multifunctional additives.
[0052] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be further described in detail below in conjunction with specific implementation methods, but the implementation methods of the present invention are not limited thereto.
[0053] Example 1
[0054] (1) Preparation of composite positive electrode materials:
[0055] The present embodiment provides a composite positive electrode material, comprising a first positive electrode active material and a second positive electrode active material, wherein the first positive electrode active material comprises a P63mc crystalline positive electrode active material, and the second positive electrode active material comprises Crystalline positive electrode active material.
[0056] The method for preparing the composite positive electrode material comprises the following steps:
[0057] S1: Cobalt sulfate solution and aluminum sulfate solution were mixed evenly in a molar ratio of Co to Al of 0.99:0.01, and excess sodium carbonate solution was added, and the mixture was stirred and filtered to obtain a precipitate; the precipitate was sintered at 550°C for 10 hours to obtain (Co 0.99 Al 0.01 )3O4 powder;
[0058] S2:Co 0.99 Al 0.01 )3O4 and Na2CO3 were mixed evenly in a molar ratio of Na to Co of 0.7:1; Na was sintered at 950℃ for 48h to obtain 0.7 Co 0.99 Al 0.01 O2;
[0059] S3: Put Na 0.7 Co 0.99 Al 0.01 O2 was dispersed in lithium nitrate solution, mixed evenly in a molar ratio of Li to Na of 10:1, reacted in a reactor at 150°C for 24 hours, filtered, rinsed with deionized water, dried, and mechanically crushed (feed frequency was 33 Hz) to obtain Li with a Dv50 of 13 μm. 0.87 Na 0.13 Co 0.99 Al 0.01 O2 positive electrode active material;
[0060] S4: Nickel sulfate solution, manganese sulfate solution, and aluminum sulfate solution were mixed evenly according to the molar ratio of Ni, Mn, and Al of 0.5:1.49:0.01, and then (Ni+Al+Mn) and carbonate molar ratio of 1:2 were mixed with sodium carbonate solution, and Ni was fully precipitated and filtered to obtain 0.5 Mn 1.49 Al 0.01 CO3 precipitation; then mixed with lithium hydroxide in a molar ratio of Li: (Ni+Mn+Al) of 1.2:2, sintered at 750-1000°C for 10h, and mechanically crushed (feed frequency of 20Hz) to obtain LiNi with a Dv50 of 4μm 0.5 Mn 1.49 Al 0.01 O4 positive electrode active material;
[0061] S5: The materials prepared in step S3 and S4 are mixed in a mass ratio of 95:5, and sintered at 750° C. for 6 h to obtain the composite positive electrode material.
[0062] (2) Preparation of positive electrode
[0063] The positive electrode material obtained in the experiment, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) were fully stirred in an N-methyl methyl pyrrolidone solvent system at a mass ratio of 95.5:2.5:2. After being stirred evenly, a positive electrode slurry was obtained, and the slurry was coated on an Al foil, baked, rolled, and cut into strips to obtain a positive electrode sheet.
[0064] (3) Preparation of negative electrode sheet
[0065] Graphite, conductive agent carbon nanotubes, binder styrene butadiene rubber, and thickener sodium carboxymethyl cellulose were stirred and mixed in deionized water at a mass ratio of 97.2:1.2:0.8:0.8. After being mixed evenly, the negative electrode slurry was coated on Cu foil, baked, rolled, and cut into strips to obtain a negative electrode sheet.
[0066] (4) Preparation of diaphragm
[0067] Polyethylene (PE) polymer film is used as the isolation membrane.
[0068] (5) Preparation of electrolyte
[0069] An organic solution is obtained by mixing the following components and mass ratios: ethylene carbonate (EC): propyl propionate (PP): vinylene carbonate (VC): diethyl carbonate (DEC): propylene carbonate (PC) = 22:25:3:28:22; lithium salt LiPF6 is added to the organic solution, and the mass ratio of the added mass to the organic solution is 9.5:90.5; after mixing evenly, an electrolyte is obtained.
[0070] (6) Preparation of batteries
[0071] The positive electrode sheet, the isolation film, and the negative electrode sheet are stacked in order and wound to obtain an electrode assembly; the electrode assembly is placed in a packaging shell, an electrolyte is injected into the packaging shell and the packaging is performed to finally obtain a lithium-ion battery.
[0072] Example 2
[0073] Different from Example 1, the feeding frequency of mechanical crushing in step S3 of this example was adjusted from 33 Hz to 25 Hz, and Li with a Dv50 of 5 μm was prepared. 0.87 Na 0.13 Co 0.99 Al 0.01 O2 positive electrode material.
[0074] The rest is the same as Example 1 and will not be described again here.
[0075] Example 3
[0076] Different from Example 1, the feeding frequency of mechanical crushing in step S3 of this example was adjusted from 33 Hz to 38 Hz, and Li with a Dv50 of 20 μm was prepared. 0.87 Na 0.13 Co 0.99 Al 0.01 O2 positive electrode material.
[0077] The rest is the same as Example 1 and will not be described again here.
[0078] Example 4
[0079] Different from Example 1, the feeding frequency of mechanical crushing in step S4 of this example is adjusted from 20 Hz to 28 Hz, and LiNi with a Dv50 of 10 μm is prepared. 0.5 Mn 1.49 Al 0.01 O4 positive electrode material.
[0080] The rest is the same as Example 1 and will not be described again here.
[0081] Example 5
[0082] Different from Example 1, the feeding frequency of mechanical crushing in step S4 of this example is adjusted from 20 Hz to 15 Hz, and LiNi with a Dv50 of 1 μm is prepared. 0.5 Mn 1.49 Al 0.01 O4 positive electrode material.
[0083] The rest is the same as Example 1 and will not be described again here.
[0084] Example 6
[0085] Different from Example 1, in step S5 of this embodiment, Li 0.87 Na 0.13 Co 0.99 Al 0.01 O2 cathode materials and LiNi 0.5 Mn 1.49 Al 0.01 The mass ratio of O4 positive electrode material is 1:1.
[0086] The rest is the same as Example 1 and will not be described again here.
[0087] Example 7
[0088] Different from Example 1, in step S5 of this embodiment, Li0.87 Na 0.13 Co 0.99 Al 0.01 O2 cathode materials and LiNi 0.5 Mn 1.49 Al 0.01 The mass ratio of O4 positive electrode material is 99:1.
[0089] The rest is the same as Example 1 and will not be described again here.
[0090] Comparative Example 1
[0091] Different from Example 1, the preparation method of the positive electrode material of this comparative example includes the following steps:
[0092] S1: Cobalt sulfate solution and aluminum sulfate were mixed evenly in a molar ratio of Co to Al of 0.99:0.01, and excess sodium carbonate solution was added, stirred and filtered to obtain a precipitate; the precipitate was sintered at 550°C for 10 hours to obtain (Co 0.99 Al 0.01 )3O4 powder.
[0093] S2:Co 0.99 Al 0.01 )3O4 and Na2CO3 were mixed evenly according to the molar ratio of Na to Co of 0.7:1; Na2CO3 with P63mc structure was obtained by sintering at 950℃ for 48h. 0.7 Co 0.99 Al 0.01 O2.
[0094] S3: Put Na 0.7 Co 0.99 Al 0.01 O2 was dispersed in lithium nitrate solution, mixed evenly in a molar ratio of Li to Na of 10:1, reacted in a reactor at 150°C for 24 hours, filtered, rinsed with deionized water, dried, and mechanically crushed to obtain Li with a Dv50 of 13 μm. 0.87 Na 0.13 Co 0.99 Al 0.01 O2 positive electrode material.
[0095] S4: Li prepared in step 3 0.87 Na 0.13 Co 0.99 Al 0.01 The O2 positive electrode material is sintered at 750° C. for 6 hours to obtain the positive electrode material.
[0096] The rest is the same as Example 1 and will not be described again here.
[0097] Comparative Example 2
[0098] Different from Example 1, the preparation method of the positive electrode material of this comparative example includes the following steps:
[0099] S1: Nickel sulfate solution, manganese sulfate solution, and aluminum sulfate solution were mixed evenly according to the molar ratio of Ni, Mn, and Al of 0.5:1.49:0.01, and then mixed with sodium carbonate solution according to the molar ratio of (Ni+Al+Mn) to carbonate of 1:2, and fully precipitated and filtered to obtain Ni 0.5 Mn 1.49 Al 0.01 CO3 precipitation; then mixed with lithium hydroxide in a molar ratio of Li: (Ni+Mn+Al) of 1.2:2, sintered at 750-1000℃ for 10h, and mechanically crushed to obtain LiNi with a Dv50 of 4μm 0.5 Mn 1.49 Al 0.01 O4 positive electrode material.
[0100] S2: LiNi prepared in step 1 0.5 Mn 1.49 Al 0.01 The O4 positive electrode material is sintered at 750° C. for 6 hours to obtain the positive electrode material.
[0101] The rest is the same as Example 1 and will not be described again here.
[0102] Comparative Example 3
[0103] Different from Example 1, the feeding frequency of mechanical crushing in step S3 of this comparative example was adjusted from 33 Hz to 44 Hz, and Li 0.87 Na 0.13 Co 0.99 Al 0.01 O2 positive electrode material.
[0104] The rest is the same as Example 1 and will not be described again here.
[0105] Comparative Example 4
[0106] Different from Example 1, the feeding frequency of mechanical crushing in step S4 of this comparative example was adjusted from 20 Hz to 35 Hz, and LiNi with a Dv50 of 15 μm was prepared. 0.5 Mn 1.49 Al 0.01 O4 positive electrode material.
[0107] The rest is the same as Example 1 and will not be described again here.
[0108] Comparative Example 5
[0109] Different from Example 1, in step S5 of this comparative example, Li0.87 Na 0.13 Co 0.99 Al 0.01 O2 cathode materials and LiNi 0.5 Mn 1.49 Al 0.01 The mass ratio of O4 positive electrode material is 1:2.
[0110] The rest is the same as Example 1 and will not be described again here.
[0111] Performance Testing
[0112] The positive electrode materials obtained in the above-mentioned Examples 1-7 and Comparative Examples 1-5 were used in lithium-ion button batteries, and the gram capacity test was carried out at 25°C, the charge and discharge conditions were 0.1C, and the charge and discharge range was 3.0V-4.60V; the 100cls cycle test was carried out at 45°C, the charge and discharge conditions were 1.0C, and the charge and discharge range was 3.0V-4.60V; the low-temperature discharge test was carried out at -10°C, the charge and discharge conditions were 0.1C, and the charge and discharge range was 3.0V-4.60V. The test results are shown in Table 1 below.
[0113] Table 1
[0114]
[0115]
[0116] From the data in Table 1 above, it can be seen that the positive electrode material Li 0.87 Na 0.13 Co 0.99 Al 0.01 O2 has high gram capacity, good cycle stability, and weak low temperature performance. Crystalline positive electrode material LiNi 0.5 Mn 1.49 Al 0.01 O4 has good low temperature performance and low gram capacity.
[0117] From the data comparison of Examples 1-5, it can be seen that when Li 0.87 Na 0.13 Co 0.99 Al 0.01 When the O2 particle size increases, the specific capacity of the composite material decreases slightly, the cycle performance improves, and the low temperature performance decreases; when LiNi 0.5 Mn 1.49 Al 0.01 When the O4 particle size becomes larger, the specific capacity of the composite material decreases, the low-temperature discharge decreases, and the cycle performance is slightly improved.
[0118] From the data comparison of Examples 1, 6-7, it can be seen that the positive electrode material Li0.87 Na 0.13 Co 0.99 Al 0.01 O2 and Crystalline positive electrode material LiNi 0.5 Mn 1.49 Al 0.01 When the mass ratio of O4 decreases, the specific capacity of the composite material is greatly reduced. In summary, the composite material prepared in Example 1 has high specific capacity, long cycle and good low temperature performance.
[0119] From the data comparison of Example 1 and Comparative Examples 1-2, it can be seen that the positive electrode material containing only P63mc crystal has poor low temperature performance. The crystalline positive electrode material has a small specific capacity and poor cycle performance.
[0120] In summary, the present invention designs a positive electrode material comprising P63mc crystalline phase and Composite positive electrode material of crystalline positive electrode material. Under high voltage, the P63mc crystalline positive electrode material has a unique coplanar connection of LiO6 octahedron and CoO6 octahedron, and only the slip of the CoO2 layer and the arrangement of Li vacancies occur, thus avoiding the cycle attenuation caused by irreversible capacity loss; The positive electrode material with a crystalline structure has a three-dimensional lithium ion diffusion channel, and lithium ions can be quickly released under high voltage, improving the low-temperature discharge performance of the composite material. The particle size design and proportion optimization of the crystalline positive electrode material can enable the composite material to have both cycle performance and low-temperature performance at high voltage.
[0121] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A composite positive electrode material, characterized in that: The invention comprises a first positive electrode active material and a second positive electrode active material, wherein the first positive electrode active material comprises a P63mc crystalline positive electrode active material, and the second positive electrode active material comprises Crystalline positive electrode active material; The XRD diffraction spectrum of the composite positive electrode material contains at least three diffraction peaks in the range of 17.8° to 22°; wherein, there is a first diffraction peak in the range of 17.8° to 18.3°, with a peak intensity of I1; there are a second diffraction peak and a third diffraction peak in the range of 18.3° to 19.0°, with peak intensities of I2 and I3 respectively; the diffraction peak intensities I1, I2 and I3 satisfy the relationship: I2 / I1≥2, I3 / I1≥2, 0.5≤I3 / I2≤2.
2. A composite positive electrode material according to claim 1, characterized in that: The average particle size of the first positive electrode active material is D1, and the average particle size of the second positive electrode active material is D2; The value range of D1 is: 5 μm≤D1≤20 μm; the value range of D2 is: 1 μm≤D2≤10 μm.
3. A composite positive electrode material according to claim 1, characterized in that: The chemical formula of the composite positive electrode material is: LiNi a Mn 2-a-b N b O4@Li x Na y Co 1-z M z O2, wherein M and N include at least one of Al, Mg, Ti, La, Y, Zn, Ni, Mn, Co, V, and Si elements; wherein 0≤a≤0.6, 0≤b<0.02; 0.7≤x<1, 0.01<y<0.1, 0≤z<0.
02.
4. A composite positive electrode material according to claim 3, characterized in that: The first positive electrode active material is Li x Na y Co 1-z M z O2, the second positive electrode active material is LiNi a Mn 2-a-b N b O4.
5. A composite positive electrode material according to claim 1, characterized in that: The mass of the first positive electrode active material is m1, and the mass of the second positive electrode active material is m2, wherein m1 and m2 satisfy the relationship: 0<m2 / m1≤1.
6. A method for preparing a composite positive electrode material according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1: Evenly mix the cobalt salt solution and the salt solution of the doping element M, add an excess of the precipitant solution, stir and filter to obtain a precipitate; The precipitate is sintered at 400℃~600℃ for 6~12h to obtain (Co 1-z M z )3O4 powder; S2:Co 1-z M z )3O4 and sodium salt are mixed uniformly; sintered at 800℃~1100℃ for 45~52h to obtain Na2O4 with P63mc crystal structure n Co 1-z M z O2, where 0.5≤n≤0.7; S3: Put Na n Co 1-z M z O2 is dispersed in the lithium salt solution, mixed evenly in a ratio of Li to Na molar ratio ≥5, reacted in a reactor at 140-160°C for 22-26h, filtered, rinsed with deionized water, dried, and crushed to obtain Li x Na y Co 1-z M z O2 positive electrode active material; S4: The nickel salt solution, the manganese salt solution, and the salt solution doped with element N are mixed evenly according to the molar ratio of Ni, Mn, and N being a: (2-ab): b to form a mixed solution, and then the mixed solution is mixed with the carbonate solution according to the molar ratio of (Ni+N+Mn) to carbonate ions being 1:2, and filtered to obtain Ni a Mn 2-a-b N b CO3 precipitation; then Ni a Mn 2-a-b N b The CO3 precipitate is mixed evenly with the lithium salt to make the molar ratio of Li to (Ni+Mn+N) be (1.0-1.4): (1.8-2.2), and then sintered at 750-1000℃ for 8-12h to obtain LiNi a Mn 2-a-b N b O4 positive electrode active material; S5: After mixing the materials prepared in step S3 and S4 according to a certain proportion, sintering at 700-800° C. for 5-8 hours, the composite positive electrode material is obtained.
7. The method for preparing a composite positive electrode material according to claim 6, characterized in that: In step S1, the molar ratio of Co to M in the cobalt salt solution and the salt solution of the doping element M is (1-z):z, wherein 0≤z<0.
02.
8. The method for preparing a composite positive electrode material according to claim 6, characterized in that: In step S2, (Co 1- z M z )3O4 and Na2CO3 are mixed in a molar ratio of Na to Co of (0.5-0.7):(1-1.2).
9. A positive electrode sheet, characterized in that: The composite positive electrode material comprises the composite positive electrode material according to any one of claims 1 to 5.