Positive electrode material, preparation method thereof and sodium ion battery
By introducing boron oxide and metal oxides such as Al, Y, Sc into the positive electrode material of sodium ion battery, the Na content and pH value are regulated, processing problems caused by high pH value are solved and the discharge performance of the battery is improved.
Patent Information
- Application Number
- CN202410966683.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
Smart Images

Figure CN118919679A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a positive electrode material and a preparation method thereof, and a sodium ion battery. Background Art
[0002] Sodium-ion batteries are secondary batteries that work similarly to lithium-ion batteries, relying mainly on the movement of sodium ions between the positive and negative electrodes. During the charge and discharge process, Na ions are inserted and removed back and forth between the two electrodes.
[0003] Sodium ion battery layered oxide is an important positive electrode material, which has a key impact on the performance of sodium ion batteries. The pH of sodium ion battery layered oxide positive electrode material is relatively high. During the slurry mixing process, high pH (>13) will cause the binder to fail, and then the slurry state will deteriorate, the viscosity will fluctuate greatly, and the coating process will be difficult to carry out. Therefore, the problem of lowering the pH of sodium ion battery layered oxide positive electrode material needs to be solved urgently.
[0004] In view of this, this invention is proposed. Summary of the invention
[0005] The first object of the present invention is to provide a positive electrode material having a low pH and improved processing performance of the positive electrode material.
[0006] The second object of the present invention is to provide a method for preparing a positive electrode material.
[0007] A third object of the present invention is to provide a sodium ion battery.
[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0009] The present invention provides a positive electrode material, the chemical formula of the positive electrode material is Na α Ni a Fe b Mn c Cu (1-a-b-c) O2·βBO 3 / 2 ·γMO 3 / 2 ; Wherein, 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1, 0.95≤α≤1.01, 0.001≤β≤0.005, 0.001≤γ≤0.01, and the M element is at least one of Al, Y and Sc.
[0010] Furthermore, the positive electrode material includes a layered oxide and a coating material attached to the surface of the layered oxide;
[0011] The layered oxide includes Na α Nia Fe b Mn c Cu (1-a-b-c) O2, where 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1;
[0012] The coating material includes boron oxide and an oxide containing an M element.
[0013] Further, the positive electrode material satisfies the following relationship: CS total value = 500 / (α+β+γ)+1 / β+1 / γ+50×(12-pH);
[0014] Wherein, the total CS value is 800-2500 ppm; pH is the pH value of the positive electrode material, pH <12.6.
[0015] Further, the positive electrode material satisfies the following relationship: 1≤C / S≤2;
[0016] In the formula, C is the content of carbon element in the positive electrode material, in ppm; S is the content of sulfur element in the positive electrode material, in ppm.
[0017] The present invention also provides a method for preparing the positive electrode material as described above, comprising the following steps:
[0018] Calcining the layered oxide, H3BO3 and the metal oxide to obtain the positive electrode material;
[0019] Wherein, the layered oxide includes Na α Ni a Fe b Mn c Cu (1-a-b-c) O2, wherein 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1, 0.95≤α≤1.01; the metal oxide comprises at least one of Al2O3, Y2O3 and Sc2O3.
[0020] Furthermore, the calcination includes: heating to 200-400° C. and calcining for 6-18 hours.
[0021] Furthermore, the method for preparing the layered oxide comprises:
[0022] After sintering the copper-nickel-iron-manganese quaternary precursor and the sodium source, the layered oxide is obtained;
[0023] or,
[0024] The layered oxide is obtained by sintering the nickel-iron-manganese ternary precursor, the copper source and the sodium source.
[0025] Furthermore, the average particle size of the copper-nickel-iron-manganese quaternary precursor and the nickel-iron-manganese ternary precursor are independently 2.5 to 8.5 μm, and the specific surface area is independently 10 to 30 m 2 / g.
[0026] Furthermore, the sintering includes: heating to 900-1000° C. and sintering for 8-24 hours.
[0027] The present invention also provides a sodium ion battery, comprising the positive electrode material as described above or the positive electrode material prepared by the method for preparing the positive electrode material as described above.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The positive electrode material provided by the present invention reduces the pH of the positive electrode material to less than 12.6 by adding B and at least one of Al, Y and Sc and regulating the relationship between the Na content, pH and the total CS value, thereby improving the processing performance of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 This is a SEM image of the positive electrode material prepared in Example 6 of the present invention.
[0032] Figure 2 This is a SEM image of the positive electrode material prepared in Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0033] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0034] In some embodiments of the present invention, a positive electrode material is provided, the chemical formula of the positive electrode material is Naα Ni a Fe b Mn c Cu (1-a-b-c) O2·βBO 3 / 2 ·γMO 3 / 2 ; Wherein, 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1, 0.95≤α≤1.01, 0.001≤β≤0.005, 0.001≤γ≤0.01, and the M element is at least one of Al, Y and Sc.
[0035] In some embodiments of the present invention, the value of β may be 0.001, 0.002, 0.003, 0.004, 0.005 or a range consisting of any two of them.
[0036] In some embodiments of the present invention, the value of γ may be 0.001, 0.002, 0.004, 0.006, 0.008, 0.01 or a range consisting of any two of them.
[0037] The positive electrode material of the present invention reduces the pH of the positive electrode material to less than 12.6 by adding a compound additive containing B and at least one of Al, Y and Sc, thereby improving the processing performance of the positive electrode material.
[0038] The positive electrode material of the present invention introduces a specific proportion of a B-containing compound and an Al / Y / Sc oxide into a layered oxide, wherein the B-containing compound plays an adhesion and coating role, while the Al / Y / Sc oxide plays a dispersion and isolation role. The present invention reduces the pH of the positive electrode material and improves the performance of the positive electrode material by introducing the above-mentioned specific components.
[0039] In the positive electrode material, the content of B element is high, the pH value of the positive electrode material is high, and the capacity of the battery prepared by using it is low; when only B or only Al / Y / Sc is added, the pH value of the positive electrode material is high, and the capacity of the battery prepared by using it is low or the discharge specific capacity is extremely poor. Therefore, only by adding B and Al / Y / Sc at the same time can a positive electrode material with excellent performance be obtained.
[0040] In some embodiments of the present invention, the positive electrode material includes a layered oxide and a coating material attached to the surface of the layered oxide;
[0041] Layered oxides include Na α Ni a Fe b Mn c Cu (1-a-b-c) O2, where 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1;
[0042] The coating material includes boron oxide and an oxide containing an M element.
[0043] In some embodiments of the present invention, the positive electrode material satisfies the following relationship:
[0044] CS total value=500 / (α+β+γ)+1 / β+1 / γ+50×(12-pH);
[0045] Wherein, the total CS value is 800-2500 ppm; pH is the pH value of the positive electrode material, pH <12.6.
[0046] The total CS value refers to the total content of carbon and sulfur in the positive electrode material. The error between the total CS value calculated by the above formula and the total CS value actually measured is ±500ppm.
[0047] In some embodiments of the present invention, the positive electrode material satisfies the following relationship:
[0048] 1≤C / S≤2;
[0049] Wherein, C is the carbon content in the positive electrode material, in ppm; S is the sulfur content in the positive electrode material, in ppm.
[0050] With the introduction of additives (containing B compounds and Al / Y / Sc oxides), the sintering difficulty is reduced, and the total CS value is at a low value, which can present a linear inverse relationship. The formula error ±500ppm is the deviation correction amount ignored by other coefficients, and the remaining numbers are the sintering difficulty coefficients. In addition, the reduction of the pH of the positive electrode material will also introduce a small amount of carbon elements, causing the total CS value to increase.
[0051] The carbon element in the positive electrode material comes from but is not limited to sodium carbonate, sodium bicarbonate, other raw material impurities, introduction of sintering atmosphere and air introduction during the preparation process, etc.; the sulfur element comes from but is not limited to raw materials such as precursors, Cu sources, sodium sources, additives, etc.
[0052] In some embodiments of the present invention, the positive electrode material is of O3 type.
[0053] In some embodiments of the present invention, the average particle size D50 of the positive electrode material is 5 to 20 μm; typically but not limitatively, for example, the average particle size D50 of the positive electrode material can be 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm or a range of any two thereof.
[0054] In some embodiments of the present invention, a method for preparing the above-mentioned positive electrode material is also provided, comprising the following steps:
[0055] The layered oxide, H3BO3 and the metal oxide are calcined to obtain a positive electrode material;
[0056] Among them, oxides include Na α Ni a Fe b Mn c Cu (1-a-b-c) O2, wherein 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1, 0.95≤α≤1.01; the metal oxide includes at least one of Al2O3, Y2O3 and Sc2O3.
[0057] The invention prepares a positive electrode material with a lower pH value by calcining a layered oxide and an additive containing B, Al / Y / Sc at a low temperature.
[0058] H3BO3 has a relatively low melting point of only 170°C. It is also known as water glass and is an inorganic adhesive with excellent fire resistance. During the calcination process, the melting and reaction of H3BO3 will form a uniform coating layer on the surface of the layered oxide, but it will directly adhere to the particles, while the oxides of Al / Y / Sc will evenly adhere to the surface of the layered oxide, thereby increasing the distance between the particles, inhibiting the adhesion between the particles, and increasing the effective area of the B coating.
[0059] During the calcination process, the coating formed by H3BO3 prevents the sodium ions in the unstable positive electrode material from escaping, and also reduces the contact area between the positive electrode material and the outside world, thereby reducing the pH value of the material. In addition, during the battery cell slurrying process, the presence of the coating will eliminate the residual moisture in the environment in advance, preventing further reaction with the positive electrode material, and inhibiting the occurrence of slurry gelation.
[0060] In some embodiments of the present invention, calcination includes: heating to 200-400°C and calcining for 6-18h; typically but not limiting, for example, the calcination temperature can be 200°C, 250°C, 300°C, 350°C, 400°C or a range consisting of any two thereof; the calcination time can be 6h, 8h, 10h, 12h, 14h, 16h, 18h or a range consisting of any two thereof.
[0061] In some embodiments of the present invention, the heating rate during the calcination process is 1-10° C. / min.
[0062] In some embodiments of the present invention, calcination is performed under an oxygen-containing atmosphere; preferably an air atmosphere or an oxygen atmosphere.
[0063] In some embodiments of the present invention, after calcination, the process further comprises crushing; preferably, the crushing is performed to a particle size D50 of 5 to 20 μm.
[0064] In some embodiments of the present invention, the method for preparing the layered oxide comprises:
[0065] After sintering the copper-nickel-iron-manganese quaternary precursor and the sodium source, a layered oxide is obtained;
[0066] or,
[0067] After sintering the nickel-iron-manganese ternary precursor, the copper source and the sodium source, a layered oxide is obtained.
[0068] In some embodiments of the present invention, the copper-nickel-iron-manganese quaternary precursor includes Ni a Fe b Mn c Cu (1-a-b-c) (OH)2; wherein, 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1.
[0069] In some embodiments of the present invention, the nickel-iron-manganese ternary precursor includes Ni u Fe v Mn 1-u-v (OH)2; wherein, 0<u≤0.5, 0<v≤0.4.
[0070] In some embodiments of the present invention, the average particle size D50 of the copper-nickel-iron-manganese quaternary precursor and the nickel-iron-manganese ternary precursor are each independently 2.5 to 8.5 μm, and the specific surface area (BET) is each independently 10 to 30 m 2 / g; typically but not limiting, for example, the average particle size D50 of the copper-nickel-iron-manganese quaternary precursor and the nickel-iron-manganese ternary precursor can be 2.5μm, 3.5μm, 4.5μm, 5.5μm, 6.5μm, 7.5μm, 8.5μm or a range of any two thereof; the specific surface area (BET) can be 10m 2 / g, 15m 2 / g, 20m 2 / g, 25m 2 / g, 30m 2 / g or a range consisting of any two of them.
[0071] If the particle size of the copper-nickel-iron-manganese quaternary precursor and the nickel-iron-manganese ternary precursor is too small, the reaction activity is strong, the side reaction is high, and the corrosion in the preparation process is serious; if the particle size is too large, the reaction activity is low and it is difficult to sinter fully; if the specific surface area is too large, the reaction activity is strong, the adhesion is serious, and the yield is affected by the crushing of too fine powder; if the specific surface area is too small, the reaction activity is low and it is difficult to sinter fully.
[0072] In some embodiments of the present invention, the copper-nickel-iron-manganese quaternary precursor and the nickel-iron-manganese ternary precursor contain impurity elements; the impurity elements include at least one of Na, S, Ca, Mg, Al, Zn, Co and Li; the content of each impurity element is <5000ppm.
[0073] In some embodiments of the present invention, the sodium source includes but is not limited to Na2CO3 and / or NaHCO3.
[0074] In some embodiments of the present invention, the copper source includes, but is not limited to, CuO.
[0075] In some embodiments of the present invention, sintering includes: heating to 900-1000°C and sintering for 8-24h; typically but not limitatively, for example, the sintering temperature can be 900°C, 950°C, 1000°C or a range consisting of any two thereof; the sintering time can be 8h, 15h, 20h, 24h or a range consisting of any two thereof.
[0076] In some embodiments of the present invention, the heating rate during the sintering process is 1-10° C. / min.
[0077] In some embodiments of the present invention, sintering is performed in an oxygen-containing atmosphere, preferably an air atmosphere or an oxygen atmosphere.
[0078] In some embodiments of the present invention, after sintering, the process further comprises crushing; preferably, the crushing is performed to a particle size D50 of 5 to 20 μm.
[0079] In some embodiments of the present invention, a sodium ion battery is also provided, comprising the above-mentioned positive electrode material or the positive electrode material prepared by the above-mentioned method for preparing the positive electrode material.
[0080] The positive electrode material of the present invention is used in a sodium ion battery to improve the discharge specific capacity and specific capacity range of the sodium ion battery.
[0081] Example 1
[0082] The chemical formula of the positive electrode material provided in this embodiment is:
[0083] Na α Cu 0.1 Mn 0.25 Ni 0.15 Fe 0.5 O2·0.004BO 3 / 2 0.008AlO 3 / 2 ;
[0084] The specific preparation method comprises the following steps:
[0085] Weigh 1.652 kg of Na2CO3 (purity 99.72%), 0.291 kg of NaHCO3 (purity 99.68%) and 4 kg of spherical precursor Cu 0.1 Mn 0.25 Ni 0.15 Fe 0.5 (OH)2(particle size D 50 The BET specific surface area is 7.5 μm and 15.63 m 2 / g), after high-speed mixing, the temperature was raised to 900°C at a rate of 2°C / min in an oxygen atmosphere for sintering for 15h, and then the material was crushed to a particle size D50 of 14.7μm;
[0086] 8.611 g of H3BO3 (purity of 99.21%) and 80.132 g of Al2O3 (purity of 99.12%) were added to the above-mentioned crushed material and mixed at high speed. The temperature was raised to 400°C at a rate of 3°C / min in an air atmosphere and calcined for 15 hours. After crushing, a positive electrode material with a particle size D50 of 14.6 μm was obtained, which was recorded as B1.
[0087] Example 2
[0088] The chemical formula of the positive electrode material provided in this embodiment is:
[0089] Na α Cu 0.01 Mn 0.45 Ni 0.44 Fe 0.1 O2 0.005BO 3 / 2 0.01YO 3 / 2 ;
[0090] The specific preparation method comprises the following steps:
[0091] Weigh 1.836 kg of Na2CO3 (purity 99.72%) and 4 kg of spherical precursor Cu 0.01 Mn 0.45 Ni 0.44 Fe 0.1 (OH)2(particle size D 50 The BET specific surface area is 18.62 m 2 / g) after high-speed mixing, the temperature was raised to 1000°C at a rate of 3°C / min in an air atmosphere for sintering for 18h, and then the material was crushed to a particle size D50 of 8.1μm;
[0092] To the above-mentioned crushed material, add 10.768g of H3BO3 (purity of 99.21%) and 39.357g of Y2O3 (purity of 99.13%) and mix at high speed. In an air atmosphere, heat to 400°C at a rate of 2°C / min and calcine for 15h. After crushing, a positive electrode material with a particle size D50 of 8.2μm is obtained, which is recorded as B2.
[0093] Example 3
[0094] The chemical formula of the positive electrode material provided in this embodiment is:
[0095] Na α Cu 0.03 Mn 0.34 Ni 0.31 Fe 0.32 O2·0.002BO 3 / 2 0.0005AlO 3 / 2 0.001YO 3 / 2 ;
[0096] The specific preparation method comprises the following steps:
[0097] Weigh 1.838 kg of Na2CO3 (purity 99.72%) and 4 kg of spherical precursor Cu 0.03 Mn 0.34 Ni 0.31 Fe 0.32 (OH)2(particle size D 50 The BET specific surface area is 19.54 m 2 / g) after high-speed mixing, the temperature was raised to 980°C at a rate of 3°C / min in an air atmosphere for sintering for 10 h, and then the material was crushed to a particle size D50 of 9.5 μm;
[0098] To the above-mentioned crushed material, add 4.312g of H3BO3 (purity of 99.21%), 0.890g of Al2O3 (purity of 99.12%) and 3.940g of Y2O3 (purity of 99.13%) and mix at high speed. In an air atmosphere, heat to 400°C at a rate of 3°C / min and calcine for 6h to obtain a positive electrode material with a particle size D50 of 9.6μm, recorded as B3.
[0099] Example 4
[0100] The chemical formula of the positive electrode material provided in this embodiment is:
[0101] Na α Cu 0.05 Mn 0.49 Ni 0.44 Fe 0.02 O2·0.002BO3 / 2 0.001YO 3 / 2 0.0005ScO 3 / 2 ;
[0102] The specific preparation method comprises the following steps:
[0103] Weigh 1.832 kg of Na2CO3 (purity 99.72%) and 4 kg of spherical precursor Cu 0.05 Mn 0.49 Ni 0.44 Fe 0.02 (OH)2(particle size D 50 The BET specific surface area is 22.48 m 2 / g) after high-speed mixing, the temperature was raised to 1000°C at a rate of 3°C / min in an air atmosphere for sintering for 18h, and then the material was crushed to a particle size D50 of 6.8μm;
[0104] To the above-mentioned crushed material, add 4.297g of H3BO3 (purity of 99.21%), 3.926g of Y2O3 (purity of 99.13%) and 1.199g of Sc2O3 (purity of 99.12%) and mix at high speed. In an air atmosphere, heat to 350°C at a rate of 10°C / min and calcine for 18h. After crushing, a positive electrode material with a particle size D50 of 7.1μm is obtained, which is recorded as B4.
[0105] Example 5
[0106] The chemical formula of the positive electrode material provided in this embodiment is:
[0107] Na α Cu 0.07 Mn 0.4 Ni 0.33 Fe 0.2 O2·0.002BO 3 / 2 0.0015YO 3 / 2 ;
[0108] The specific preparation method comprises the following steps:
[0109] Weigh 2.907 kg of NaHCO3 (purity 99.68%) and 4 kg of spherical precursor Cu 0.07 Mn 0.4 Ni 0.33 Fe 0.2 (OH)2(particle size D 50 The BET specific surface area is 4.7 μm and 18.62 m 2 / g) after high-speed mixing, the temperature was raised to 990°C at a rate of 3°C / min in an air atmosphere for sintering for 15h, and then the material was crushed to a particle size D50 of 5.4μm;
[0110] To the above-mentioned crushed material, add 4.300g of H3BO3 (purity of 99.21%) and 5.894g of Y2O3 (purity of 99.13%) and mix at high speed. Under an oxygen atmosphere, heat to 400°C at a rate of 8°C / min and calcine for 10 hours. After crushing, a positive electrode material with a particle size D50 of 5.6μm is obtained, which is recorded as B5.
[0111] Example 6
[0112] The chemical formula of the positive electrode material provided in this embodiment is:
[0113] Na α Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2·0.003BO 3 / 2 0.003AlO 3 / 2 ;
[0114] The specific preparation method comprises the following steps:
[0115] Weigh 1.832 kg of Na2CO3 (purity 99.72%) and 4 kg of spherical precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2(particle size D 50 The BET specific surface area is 6.7 μm and 13.41 m 2 / g) after high-speed mixing, the temperature was raised to 960°C at a rate of 3°C / min in an air atmosphere for sintering for 15h, and then the material was crushed to a particle size D50 of 10.1μm;
[0116] To the above-mentioned crushed material, add 6.447g of H3BO3 (purity 99.21%) and 5.320g of Al2O3 (purity 99.12%) and mix at high speed. In an air atmosphere, heat to 350°C at a rate of 5°C / min and calcine for 12h. After crushing, a positive electrode material with a particle size D50 of 10.2μm is obtained, which is recorded as B6.
[0117] Example 7
[0118] The chemical formula of the positive electrode material provided in this embodiment is:
[0119] Na α Cu 0.11 Mn0.33 Ni 0.22 Fe 0.34 O2 0.001BO 3 / 2 0.0015ScO 3 / 2 ;
[0120] The specific preparation method comprises the following steps:
[0121] Weigh 1.999 kg of Na2CO3 (purity 99.72%), 310.986 g of CuO (purity 95.34%, D50 = 12.4 μm) and 4 kg of spherical precursor Mn 0.37 Ni 0.25 Fe 0.38 (OH)2(particle size D 50 The BET specific surface area is 4.5 μm and 12.74 m 2 / g) after high-speed mixing, the temperature was raised to 980°C at a rate of 5°C / min in an air atmosphere for sintering for 24h, and then the material was crushed to a particle size D50 of 9.8μm;
[0122] To the above-mentioned crushed material, add 2.344 g of H3BO3 (purity of 99.21%) and 3.925 g of Sc2O3 (purity of 99.12%) and mix at high speed. In an air atmosphere, heat to 300°C at a rate of 5°C / min and calcine for 12 hours. After crushing, a positive electrode material with a particle size D50 of 9.8μm is obtained, which is recorded as B7.
[0123] Comparative Example 1
[0124] The chemical formula of the positive electrode material provided in this comparative example is:
[0125] Na α Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2 0.006BO 3 / 2 0.006AlO 3 / 2 ;
[0126] The specific preparation method comprises the following steps:
[0127] Weigh 1.832 kg of Na2CO3 (purity 99.72%) and 4 kg of spherical precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2(particle size D 50 The BET specific surface area is 6.7 μm and 13.41 m 2 / g) were mixed at high speed, and then heated to 960°C at a rate of 3°C / min in an air atmosphere for sintering for 15h, and then the material was crushed to a particle size D50 of 9.8μm;
[0128] 12.894 g of H3BO3 (purity of 99.21%) and 10.640 g of Al2O3 (purity of 99.12%) were added to the above-mentioned crushed material and mixed at high speed. The temperature was raised to 300°C at a rate of 3°C / min in an air atmosphere and calcined for 10 hours. After crushing, a positive electrode material with a particle size D50 of 9.7 μm was obtained, which was recorded as A1.
[0129] Comparative Example 2
[0130] The chemical formula of the positive electrode material provided in this comparative example is:
[0131] Na α Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2·0.003BO 3 / 2 ;
[0132] The specific preparation method comprises the following steps:
[0133] Weigh 1.832 kg of Na2CO3 (purity 99.72%) and 4 kg of spherical precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2(particle size D 50 The BET specific surface area is 6.7 μm and 13.41 m 2 / g) after high-speed mixing, the temperature was raised to 960°C at a rate of 3°C / min in an air atmosphere for sintering for 15h, and then the material was crushed to a particle size D50 of 9.6μm;
[0134] 6.447 g of H3BO3 (purity of 99.21%) was added to the above-mentioned crushed material and mixed at high speed. The temperature was raised to 300°C at a rate of 3°C / min in an air atmosphere and calcined for 10 hours. After crushing, a positive electrode material with a particle size D50 of 9.5 μm was obtained, which was recorded as A2.
[0135] Comparative Example 3
[0136] The chemical formula of the positive electrode material provided in this comparative example is:
[0137] Na α Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34O2·0.003BO 3 / 2 0.003CoO 3 / 2 ;
[0138] The specific preparation method comprises the following steps:
[0139] Weigh 1.832 kg of Na2CO3 (purity 99.72%) and 4 kg of spherical precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2(particle size D 50 The BET specific surface area is 6.7 μm and 13.41 m 2 / g) after high-speed mixing, the temperature was raised to 960°C at a rate of 3°C / min in an air atmosphere for sintering for 15h, and then the material was crushed to a particle size D50 of 10.2μm;
[0140] 12.894 g of H3BO3 (purity of 99.21%) and 8.652 g of Co2O3 (purity of 99.15%) were added to the above-mentioned crushed material and mixed at high speed. The temperature was raised to 300°C at a rate of 3°C / min in an air atmosphere and calcined for 10 hours. After crushing, a positive electrode material with a particle size D50 of 10.3 μm was obtained, which was recorded as A3.
[0141] Comparative Example 4
[0142] The chemical formula of the positive electrode material provided in this comparative example is:
[0143] Na α Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2·0.003AlO 3 / 2 ;
[0144] The specific preparation method comprises the following steps:
[0145] Weigh 1.832 kg of Na2CO3 (purity 99.72%) and 4 kg of spherical precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2(particle size D 50 The BET specific surface area is 6.7 μm and 13.41 m 2 / g) after high-speed mixing, the temperature was raised to 960°C at a rate of 3°C / min in an air atmosphere for sintering for 15h, and then the material was crushed to a particle size of D50 = 9.9μm;
[0146] 5.320 g of Al2O3 (purity of 99.12%) was added to the above-mentioned crushed material and mixed at high speed. The temperature was raised to 300°C at a rate of 3°C / min in an air atmosphere and calcined for 10 hours. After crushing, a positive electrode material with a particle size D50 of 9.8 μm was obtained, which was recorded as A4.
[0147] Test example
[0148] The positive electrode materials of Example 6 and Comparative Example 3 were tested by scanning electron microscope, and the results are as follows: Figure 1 and Figure 2 shown.
[0149] from Figure 1 This is the morphology of the positive electrode material of Example 6, with distinct and smooth particles, relatively dispersed distribution, and no obvious particle adhesion; Figure 2 This is the morphology of the positive electrode material of Comparative Example 3. The particles are severely adhered to each other and the surface is rough, which is caused by high pH and poor air stability.
[0150] The parameters of the positive electrode materials of Examples 1 to 7 and Comparative Examples 1 to 4 were tested, and the results are shown in Table 1.
[0151] The test method for the Na content (α) in the positive electrode material is: using Avio-550PE inductively coupled plasma (ICP-OES), the main element dilution factor is 1:10000, the additive and impurity element dilution factor is 1:100, and the test wavelength is Na-238.2nm.
[0152] The pH test method is: use a Mettler Toledo FE-28 pH meter, calibrate the pH points to 6.86, 9.18, and 12.45, weigh 2±0.001g of sample, dissolve it in 40ml of pure water at 25°C, stir for 10 minutes, let it stand for 5 minutes, and read the value with a calibrated pH meter.
[0153] In Table 1, the total CS value refers to the total content of carbon and sulfur in the positive electrode material; C refers to the content of carbon in the positive electrode material, and S refers to the content of sulfur in the positive electrode material.
[0154] Total CS value (calculated value) = 500 / (α+β+γ)+1 / β+1 / γ+50×(12-pH);
[0155] The CS total value (test value) test value is measured by a CS tester; a high-frequency infrared carbon-sulfur analyzer CS-2800G is used to test the carbon content and the carbon content in the positive electrode material. The test parameters include: weighing 0.2g±0.001g of the standard sample, 0.5g±0.001g of the test sample, and a heating temperature of 2000-4000°C; based on the test results, the sum of the C element and the S element content, i.e., the CS total value (test value), can be calculated.
[0156] Table 1
[0157]
[0158] The positive electrode materials of Examples 1 to 7 and Comparative Examples 1 to 4 were respectively used as positive electrode active materials to assemble button-type batteries. The performance of each battery was tested, and the results are shown in Table 2.
[0159] A method for preparing a button cell comprises the following steps:
[0160] The positive electrode active material, SP and PVDF were mixed in a mass ratio of 90:5:5, and NMP was added to make a viscous glue solution, which was coated on an aluminum foil and baked in a vacuum drying oven at 120°C for 12 h to obtain a positive electrode sheet. A 2032 button cell was assembled in an Ar protective glove box using a metal sodium sheet as the counter electrode, glass fiber (Waterman) as the separator, and 1 mol / LNaPF6 EC / DMC=1:1 (Alfa) as the electrolyte.
[0161] Test method: Test the battery in the voltage range of 2.5-4.0V, cycle at 0.1C for 3 weeks, and record the average discharge capacity, discharge capacity extreme value and first efficiency of 5 batteries at 0.1C in the first 3 weeks.
[0162] Table 2
[0163] First effect (%) 0.1C discharge specific capacity (mAh / g) Very poor specific capacity (mAh / g) Example 1 91.32 132.43 2.74 Example 2 91.46 136.63 2.15 Example 3 91.14 135.12 2.72 Example 4 91.03 137.47 2.67 Example 5 92.34 134.48 2.33 Example 6 91.23 132.25 2.28 Example 7 92.34 131.71 2.59 Comparative Example 1 89.93 120.35 3.24 Comparative Example 2 89.76 123.26 3.11 Comparative Example 3 89.89 120.41 3.53 Comparative Example 4 87.31 129.29 6.75
[0164] It can be seen from Table 1 and Table 2 that, in comparison between Comparative Example 1 and Example 2, the higher the content of element B in the positive electrode material, the lower the buckling capacity obtained.
[0165] Comparing Comparative Example 2 with Example 6, when only B is added to the positive electrode material without introducing a trivalent metal element, the resulting charge capacity is low.
[0166] Comparing Comparative Example 4 with Example 6, the difference in discharge capacity when only the limited trivalent metal element is added without introducing B is very large.
[0167] Comparing Example 3 with Example 6, when other trivalent metal elements are added to the positive electrode material, the resulting charge capacity is low.
[0168] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A positive electrode material, characterized in that: The chemical formula of the positive electrode material is Na α Ni a Fe b Mn c Cu (1-a-b-c) O2·βBO 3 / 2 ·γMO 3 / 2 ; Wherein, 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1, 0.95≤α≤1.01, 0.001≤β≤0.005, 0.001≤γ≤0.01, and the M element is at least one of Al, Y and Sc.
2. The positive electrode material according to claim 1, characterized in that The positive electrode material includes a layered oxide and a coating material attached to the surface of the layered oxide; The layered oxide includes Na α Ni a Fe b Mn c Cu (1-a-b-c) O2, where 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1; The coating material includes boron oxide and an oxide containing an M element.
3. The positive electrode material according to claim 1, characterized in that The positive electrode material satisfies the following relationship: CS total value = 500 / (α+β+γ)+1 / β+1 / γ+50×(12-pH); Wherein, the total CS value is 800-2500 ppm; pH is the pH value of the positive electrode material, pH <12.
6.
4. The positive electrode material according to claim 1, characterized in that The positive electrode material satisfies the following relationship: 1≤C / S≤2; In the formula, C is the content of carbon element in the positive electrode material, in ppm; S is the content of sulfur element in the positive electrode material, in ppm.
5. The method for preparing the positive electrode material according to any one of claims 1 to 4, characterized in that: The steps include: Calcining the layered oxide, H3BO3 and the metal oxide to obtain the positive electrode material; Wherein, the layered oxide includes Na α Ni a Fe b Mn c Cu (1-a-b-c) O2, wherein 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1, 0.95≤α≤1.01; the metal oxide comprises at least one of Al2O3, Y2O3 and Sc2O3.
6. The method for preparing the positive electrode material according to claim 5, characterized in that: The calcination comprises: heating to 200-400° C. and calcining for 6-18 hours.
7. The method for preparing the positive electrode material according to claim 5, characterized in that: The method for preparing the layered oxide comprises: After sintering the copper-nickel-iron-manganese quaternary precursor and the sodium source, the layered oxide is obtained; or, The layered oxide is obtained by sintering the nickel-iron-manganese ternary precursor, the copper source and the sodium source.
8. The method for preparing the positive electrode material according to claim 7, characterized in that: The average particle size of the copper-nickel-iron-manganese quaternary precursor and the nickel-iron-manganese ternary precursor are independently 2.5 to 8.5 μm, and the specific surface area is independently 10 to 30 m 2 / g.
9. The method for preparing the positive electrode material according to claim 7, characterized in that: The sintering comprises: heating to 900-1000° C. and sintering for 8-24 hours.
10. A sodium ion battery, characterized in that: The invention comprises the positive electrode material according to any one of claims 1 to 4 or the positive electrode material prepared by the preparation method of the positive electrode material according to any one of claims 5 to 9.