Sodium-ion battery positive electrode material as well as preparation method and application thereof
Through spray drying and sputtering sintering technology of sodium sources, iron-based sulfates and water-soluble carbon sources, sodium ion battery positive electrode materials with excellent cycling performance and high conductivity were prepared, and the problem of insufficient performance in the prior art was solved. It realizes efficient use of the battery.
Patent Information
- Application Number
- CN202410981428.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
AI Technical Summary
The cycling performance and first-time performance of the existing iron-based sulfate system sodium ion battery positive electrode material is poor, and the conductivity and stability are insufficient, which limits its application in sodium ion batteries.
After mixed spray drying of sodium source, iron-based sulfate and water-soluble carbon source, the sodium ion battery positive electrode material is formed by spray-drying technology, and the battery is prepared by combining conductive agents and binders to improve conductivity and stability.
It significantly improves the cycling performance and first-time efficiency of the positive electrode material of sodium ion battery, enhances the conductivity and ion transmission efficiency, and extends the service life of the battery.
Smart Images

Figure BDA0004956190940000121 
Figure BDA0004956190940000131
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a sodium ion battery positive electrode material and a preparation method and application thereof. Background Art
[0002] Currently, how to develop high voltage (>3.6V vs.Na + / Na), abundant resources, and long service life positive electrode materials to circumvent raw material and cost constraints have become the main research and development direction of sodium ion batteries.
[0003] In this type of research, the iron-based sulfate system is widely used due to its abundant resources, low price, and high working voltage (relative to Na + / Na is 3.8V) and is considered to be one of the promising positive electrode materials. However, the low conductivity and low stability of the iron-based sulfate system will seriously restrict its capacity. At present, the development and research of this positive electrode material at home and abroad mainly improves its conductivity by adding highly conductive inorganic carbon (carbon nanotubes, graphene, etc.) during the solid phase ball milling process, but the dispersion effect of inorganic carbon is greatly affected by the raw materials and experimental conditions, and its high cost will also weaken the market competitiveness of the positive electrode material.
[0004] However, many researchers have begun to try in-situ coating of organic carbon sources to obtain sodium ferric sulfate positive electrode materials. However, due to the inherent characteristics of sodium ferric sulfate materials (poor thermal stability), if the sintering temperature is too high, the sulfate ions will decompose, causing the collapse of the entire material structure. If the sintering temperature is too low, the solid phase diffusion rate will slow down, thereby greatly reducing the mass transfer rate, delaying the overall reaction process, hindering the carbonization of the carbon source, and reducing the ion transfer efficiency and conductivity. Summary of the invention
[0005] Therefore, the technical problem to be solved by the present invention is to overcome the poor cycle performance and initial performance of batteries containing sodium ion positive electrode materials made from iron-based sulfate in the prior art, thereby providing a sodium ion battery positive electrode material and its preparation method and application.
[0006] The first aspect of the present invention provides a method for preparing a positive electrode material for a sodium ion battery, wherein the preparation method specifically comprises the following steps:
[0007] S1, mixing a sodium source, an iron-based sulfate, a water-soluble carbon source and water and spray drying the mixture to obtain a precursor;
[0008] S2. Sputtering and sintering the precursor to obtain a positive electrode material for a sodium ion battery.
[0009] According to the present invention, the sodium source includes at least one of sodium sulfate, sodium hydroxide, sodium carbonate and sodium oxalate.
[0010] According to the present invention, the iron-based sulfate includes ferrous sulfate and / or ferric sulfate.
[0011] According to the present invention, the ferrous sulfate includes at least one of ferrous sulfate heptahydrate, ferrous sulfate pentahydrate, ferrous sulfate monohydrate, and anhydrous ferrous sulfate.
[0012] According to the present invention, the ferric sulfate includes ferric sulfate nonahydrate and / or anhydrous ferric sulfate.
[0013] According to the present invention, the water-soluble carbon source includes at least one of ascorbic acid, citric acid, glucose, sucrose, acetic acid, propionic acid and oxalic acid.
[0014] According to the present invention, the molar ratio of the sodium element in the sodium source to the iron element in the iron-based sulfate is 1:1-3.
[0015] According to the present invention, based on the total mass of the sodium source and the iron-based sulfate, the amount of the water-soluble carbon source is 2-30wt%, and the amount of water is 50-80wt%.
[0016] According to the present invention, the spray drying inlet temperature is 150-170°C, and the outlet temperature is 90-110°C.
[0017] According to the present invention, the sputtering uses a transition metal target, and the transition metal includes any one of Ni, Cu, and Zn.
[0018] In the present invention, when sputtering, vacuum is first drawn and then argon is introduced. The pressure range of the vacuum is 4×10 -4 -6×10 -4 Pa, the working pressure after the introduction of argon gas is 8-10Pa, the gas flow rate of the argon gas is 50-100sccm; the sputtering current is 100-500mA, and the voltage is 100-1200V; the sputtering time is 10-60min, preferably any one of 15min, 30min, and 45min.
[0019] According to the present invention, the sintering process includes: heating to 270-300°C at a rate of 2-5°C / min for the first stage sintering, the sintering time is 4-7h, and then heating to 350-400°C at a rate of 2-5°C / min for the second stage sintering, the sintering time is 12-24h.
[0020] The second aspect of the present invention protects a sodium ion battery positive electrode material prepared by the aforementioned preparation method.
[0021] A third aspect of the present invention protects a secondary battery, wherein the secondary battery comprises the aforementioned sodium ion battery positive electrode material.
[0022] The specific preparation method of the battery is as follows: the positive electrode material is evenly mixed with the conductive agent acetylene black and the binder PVDF in a mass ratio of 80:10:10, 1-methyl-2-pyrrolidone is added (the mass ratio of the positive electrode material to 1-methyl-2-pyrrolidone is 4:1) and ball milled for 1 hour, the slurry is evenly coated on the aluminum sheet, dried and pressed into a positive electrode sheet, a propylene carbonate (PC) solution containing 1-3 mol / L NaC1O4 is used as the electrolyte, and a metal sodium sheet is used as the negative electrode to assemble into a CR2032 button battery.
[0023] The technical solution of the present invention has the following advantages:
[0024] The present invention protects a method for preparing a positive electrode material for a sodium ion battery, wherein the preparation method specifically comprises the following steps: S1, mixing a sodium source, an iron-based sulfate, a water-soluble carbon source and water and spray-drying the mixture to obtain a precursor; S2, sputtering and sintering the precursor to obtain the positive electrode material for the sodium ion battery; in the present invention, the iron-based sulfate is used together with the water-soluble carbon source, which can improve the conductivity while maintaining good stability; the precursor is coated with the sputtering technology and then sintered, which can improve the material stability and enhance the ion transmission efficiency and conductivity; so that the battery containing the positive electrode material for the sodium ion battery finally obtained has excellent cycle performance, discharge specific capacity and first efficiency. DETAILED DESCRIPTION
[0025] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0026] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0027] Example 1
[0028] A method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0029] S1. Sodium sulfate, ferrous sulfate heptahydrate, ascorbic acid and water are mixed, wherein the molar ratio of the sodium element in the sodium sulfate to the iron element in the ferrous sulfate heptahydrate is 1:2, based on the total mass of the sodium sulfate and the ferrous sulfate heptahydrate, the amount of ascorbic acid is 10wt%, the amount of water is 60wt%, and spray drying is performed with an inlet temperature of 170°C and an outlet temperature of 90°C to obtain a precursor;
[0030] S2, using a direct current power supply in an argon atmosphere, a Ni target (purity: 99.995%, size: φ50.8×2mm) was coated on the precursor, and the pressure in the chamber was 6×10 -4 Pa, working pressure is 8Pa, sputtering gas is argon, gas flow rate is 80sccm, sputtering power is 150W, sputtering is 15min; the temperature is raised to 300℃ at a rate of 2℃ / min for the first stage sintering, and the sintering time is 4h; then the temperature is raised to 350℃ at a rate of 2℃ / min for the second stage sintering, and the sintering time is 24h to obtain the positive electrode material of sodium ion battery.
[0031] Example 2
[0032] A method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0033] S1. Sodium carbonate, ferrous sulfate pentahydrate, citric acid and water are mixed, wherein the molar ratio of the sodium element in the sodium carbonate to the iron element in the ferrous sulfate pentahydrate is 1:2, based on the total mass of the sodium carbonate and the ferrous sulfate pentahydrate, the amount of citric acid is 10wt%, the amount of water is 60wt%, and spray drying is performed with an inlet temperature of 170°C and an outlet temperature of 90°C to obtain a precursor;
[0034] S2, using a direct current power supply in an argon atmosphere, a Ni target (purity: 99.995%, size: φ50.8×2mm) was coated on the precursor, and the pressure in the chamber was 6×10 -4 Pa, working pressure is 8Pa, sputtering gas is argon, gas flow rate is 80sccm, sputtering power is 150W, sputtering is 15min; the temperature is raised to 300℃ at a rate of 2℃ / min for the first stage sintering, and the sintering time is 4h; then the temperature is raised to 350℃ at a rate of 2℃ / min for the second stage sintering, and the sintering time is 24h to obtain the positive electrode material of sodium ion battery.
[0035] Example 3
[0036] A method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0037] S1. Sodium sulfate, anhydrous ferric sulfate, ascorbic acid and water are mixed, wherein the molar ratio of the sodium element in the sodium sulfate to the iron element in the anhydrous ferric sulfate is 1:2, based on the total mass of the sodium sulfate and the anhydrous ferric sulfate, the amount of ascorbic acid is 10wt%, the amount of water is 60wt%, and spray drying is performed, the inlet temperature is 170°C, and the outlet temperature is 90°C, to obtain a precursor;
[0038] S2, using a direct current power supply in an argon atmosphere, a Ni target (purity: 99.995%, size: φ50.8×2mm) was coated on the precursor, and the pressure in the chamber was 6×10 -4 Pa, working pressure is 8Pa, sputtering gas is argon, gas flow rate is 80sccm, sputtering power is 150W, sputtering is 15min; the temperature is raised to 300℃ at a rate of 2℃ / min for the first stage sintering, and the sintering time is 4h; then the temperature is raised to 350℃ at a rate of 2℃ / min for the second stage sintering, and the sintering time is 24h to obtain the positive electrode material of sodium ion battery.
[0039] Example 4
[0040] A method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0041] S1. Sodium sulfate, ferrous sulfate heptahydrate, ascorbic acid and water are mixed, wherein the molar ratio of the sodium element in the sodium sulfate to the iron element in the ferrous sulfate heptahydrate is 1:3, based on the total mass of the sodium sulfate and the ferrous sulfate heptahydrate, the amount of ascorbic acid is 15wt%, the amount of water is 55wt%, and spray drying is performed with an inlet temperature of 170°C and an outlet temperature of 90°C to obtain a precursor;
[0042] S2, using a direct current power supply in an argon atmosphere, a Ni target (purity: 99.995%, size: φ50.8×2mm) was coated on the precursor, and the pressure in the chamber was 6×10 -4 Pa, working pressure is 8Pa, sputtering gas is argon, gas flow rate is 80sccm, sputtering power is 150W, sputtering is 15min; the temperature is raised to 300℃ at a rate of 2℃ / min for the first stage sintering, and the sintering time is 4h; then the temperature is raised to 350℃ at a rate of 2℃ / min for the second stage sintering, and the sintering time is 24h to obtain the positive electrode material of sodium ion battery.
[0043] Example 5
[0044] A method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0045] S1. Sodium sulfate, ferrous sulfate heptahydrate, ascorbic acid and water are mixed, wherein the molar ratio of the sodium element in the sodium sulfate to the iron element in the ferrous sulfate heptahydrate is 1:2.5, based on the total mass of the sodium sulfate and the ferrous sulfate heptahydrate, the amount of ascorbic acid is 10wt%, the amount of water is 60wt%, and spray drying is performed with an inlet temperature of 170°C and an outlet temperature of 90°C to obtain a precursor;
[0046] S2, using a direct current power supply in an argon atmosphere, a Ni target (purity: 99.995%, size: φ50.8×2mm) was coated on the precursor, and the pressure in the chamber was 6×10 -4 Pa, working pressure is 8Pa, sputtering gas is argon, gas flow rate is 80sccm, sputtering power is 150W, sputtering is 15min; the temperature is raised to 300℃ at a rate of 2℃ / min for the first stage sintering, and the sintering time is 4h; then the temperature is raised to 350℃ at a rate of 2℃ / min for the second stage sintering, and the sintering time is 24h to obtain the positive electrode material of sodium ion battery.
[0047] Example 6
[0048] A method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0049] S1. Sodium sulfate, ferrous sulfate heptahydrate, ascorbic acid and water are mixed, wherein the molar ratio of the sodium element in the sodium sulfate to the iron element in the ferrous sulfate heptahydrate is 1:2, based on the total mass of the sodium sulfate and the ferrous sulfate heptahydrate, the amount of ascorbic acid is 30wt%, the amount of water is 60wt%, and spray drying is performed with an inlet temperature of 170°C and an outlet temperature of 90°C to obtain a precursor;
[0050] S2, using a direct current power supply in an argon atmosphere, a Ni target (purity: 99.995%, size: φ50.8×2mm) was coated on the precursor, and the pressure in the chamber was 6×10 -4 Pa, working pressure is 8Pa, sputtering gas is argon, gas flow rate is 80sccm, sputtering power is 150W, sputtering is 15min; the temperature is raised to 300℃ at a rate of 2℃ / min for the first stage sintering, and the sintering time is 4h; then the temperature is raised to 350℃ at a rate of 2℃ / min for the second stage sintering, and the sintering time is 24h to obtain the positive electrode material of sodium ion battery.
[0051] Example 7
[0052] A method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0053] S1. Sodium sulfate, ferrous sulfate heptahydrate, ascorbic acid and water are mixed, wherein the molar ratio of the iron element in the sodium sulfate to the iron element in the ferrous sulfate heptahydrate is 1:2, based on the total mass of the sodium sulfate and the ferrous sulfate heptahydrate, the amount of ascorbic acid is 10wt%, the amount of water is 60wt%, and spray drying is performed with an inlet temperature of 170°C and an outlet temperature of 90°C to obtain a precursor;
[0054] S2, using a DC power supply in an argon atmosphere, a Zn target (purity: 99.995%, size: φ50.8×2mm) was coated on the precursor, and the pressure in the chamber was 6×10 -4 Pa, working pressure is 8Pa, sputtering gas is argon, gas flow rate is 80sccm, sputtering power is 150W, sputtering is 15min; the temperature is raised to 300℃ at a rate of 2℃ / min for the first stage sintering, and the sintering time is 4h; then the temperature is raised to 350℃ at a rate of 2℃ / min for the second stage sintering, and the sintering time is 24h to obtain the positive electrode material of sodium ion battery.
[0055] Example 8
[0056] A method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0057] S1. Sodium sulfate, ferrous sulfate heptahydrate, ascorbic acid and water are mixed, wherein the molar ratio of the sodium element in the sodium sulfate to the iron element in the ferrous sulfate heptahydrate is 1:2, based on the total mass of the sodium sulfate and the ferrous sulfate heptahydrate, the amount of ascorbic acid is 10wt%, the amount of water is 60wt%, and spray drying is performed with an inlet temperature of 170°C and an outlet temperature of 90°C to obtain a precursor;
[0058] S2, using a direct current power supply in an argon atmosphere, a Ni target (purity: 99.995%, size: φ50.8×2mm) was coated on the precursor, and the pressure in the chamber was 6×10 -4 Pa, working pressure is 8Pa, sputtering gas is argon, gas flow rate is 80sccm, sputtering power is 150W, sputtering is 15min; heating to 270℃ at a rate of 5℃ / min for the first stage sintering, and the sintering time is 4h; then heating to 350℃ at a rate of 2℃ / min for the second stage sintering, and the sintering time is 24h to obtain the positive electrode material for sodium ion battery.
[0059] Example 9
[0060] A method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0061] S1. Sodium sulfate, ferrous sulfate heptahydrate, ascorbic acid and water are mixed, wherein the molar ratio of the sodium element in the sodium sulfate to the iron element in the ferrous sulfate heptahydrate is 1:2, based on the total mass of the sodium sulfate and the ferrous sulfate heptahydrate, the amount of ascorbic acid is 10wt%, the amount of water is 60wt%, and spray drying is performed with an inlet temperature of 170°C and an outlet temperature of 90°C to obtain a precursor;
[0062] S2, using a direct current power supply in an argon atmosphere, a Ni target (purity: 99.995%, size: φ50.8×2mm) was coated on the precursor, and the pressure in the chamber was 6×10 -4 Pa, working pressure is 8Pa, sputtering gas is argon, gas flow rate is 80sccm, sputtering power is 150W, sputtering is 15min; heating to 300℃ at a rate of 2℃ / min for the first stage sintering, and the sintering time is 4h; then heating to 400℃ at a rate of 3℃ / min for the second stage sintering, and the sintering time is 24h to obtain the positive electrode material for sodium ion battery.
[0063] Comparative Example 1
[0064] A method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0065] S1. Sodium sulfate, anhydrous ferric phosphate, ascorbic acid and water are mixed, wherein the molar ratio of the sodium element in the sodium sulfate to the iron element in the anhydrous ferric phosphate is 1:2, based on the total mass of the sodium sulfate and the anhydrous ferric phosphate, the amount of ascorbic acid is 10wt%, the amount of water is 60wt%, and spray drying is performed with an inlet temperature of 170°C and an outlet temperature of 90°C to obtain a precursor;
[0066] S2, using a direct current power supply in an argon atmosphere, a Ni target (purity: 99.995%, size: φ50.8×2mm) was coated on the precursor, and the pressure in the chamber was 6×10 -4 Pa, working pressure is 8Pa, sputtering gas is argon, gas flow rate is 80sccm, sputtering power is 150W, sputtering is 15min; the temperature is raised to 300℃ at a rate of 2℃ / min for the first stage sintering, and the sintering time is 4h; then the temperature is raised to 350℃ at a rate of 2℃ / min for the second stage sintering, and the sintering time is 24h to obtain the positive electrode material of sodium ion battery.
[0067] Comparative Example 2
[0068] A method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0069] S1, sodium sulfate, ascorbic acid and water are mixed, wherein the amount of ascorbic acid is 10wt% and the amount of water is 60wt% based on the mass of sodium sulfate, and spray drying is performed with an inlet temperature of 170° C. and an outlet temperature of 90° C. to obtain a precursor;
[0070] S2, using a direct current power supply in an argon atmosphere, a Ni target (purity: 99.995%, size: φ50.8×2mm) was coated on the precursor, and the pressure in the chamber was 6×10 -4Pa, working pressure is 8Pa, sputtering gas is argon, gas flow rate is 80sccm, sputtering power is 150W, sputtering is 15min; the temperature is raised to 300℃ at a rate of 2℃ / min for the first stage sintering, and the sintering time is 4h; then the temperature is raised to 350℃ at a rate of 2℃ / min for the second stage sintering, and the sintering time is 24h to obtain the positive electrode material of sodium ion battery.
[0071] Comparative Example 3
[0072] A method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0073] S1. Sodium sulfate, ferrous sulfate heptahydrate, carbon nanotubes and water are mixed, wherein the molar ratio of the sodium element in the sodium sulfate to the iron element in the ferrous sulfate heptahydrate is 1:2, based on the total mass of the sodium sulfate and the ferrous sulfate heptahydrate, the amount of the carbon nanotubes is 10wt%, the amount of water is 60wt%, and spray drying is performed with an inlet temperature of 170°C and an outlet temperature of 90°C to obtain a precursor;
[0074] S2, using a direct current power supply in an argon atmosphere, a Ni target (purity: 99.995%, size: φ50.8×2mm) was coated on the precursor, and the pressure in the chamber was 6×10 -4 Pa, working pressure is 8Pa, sputtering gas is argon, gas flow rate is 80sccm, sputtering power is 150W, sputtering is 15min; the temperature is raised to 300℃ at a rate of 2℃ / min for the first stage sintering, and the sintering time is 4h; then the temperature is raised to 350℃ at a rate of 2℃ / min for the second stage sintering, and the sintering time is 24h to obtain the positive electrode material of sodium ion battery.
[0075] Comparative Example 4
[0076] A method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0077] S1. Sodium sulfate, ferrous sulfate heptahydrate, ascorbic acid and water are mixed, wherein the molar ratio of the sodium element in the sodium sulfate to the iron element in the ferrous sulfate heptahydrate is 1:2, based on the total mass of the sodium sulfate and the ferrous sulfate heptahydrate, the amount of ascorbic acid is 10wt%, the amount of water is 60wt%, and spray drying is performed with an inlet temperature of 170°C and an outlet temperature of 90°C to obtain a precursor;
[0078] S2. The obtained precursor is heated to 300°C at a rate of 2°C / min for the first stage sintering, and the sintering time is 4 hours; then the temperature is raised to 350°C at a rate of 2°C / min for the second stage sintering, and the sintering time is 24 hours to obtain the positive electrode material for the sodium ion battery.
[0079] Test Case
[0080] The specific preparation method of the battery is as follows: the positive electrode material is evenly mixed with the conductive agent acetylene black and the binder PVDF in a mass ratio of 80:10:10, 1-methyl-2-pyrrolidone is added (the mass ratio of the positive electrode material to 1-methyl-2-pyrrolidone is 4:1) and ball milled for 1 hour, the slurry is evenly coated on the aluminum sheet, dried and pressed into a positive electrode sheet, a propylene carbonate (PC) solution containing 1 mol / L NaC1O4 is used as the electrolyte, a metal sodium sheet is used as the negative electrode, and assembled into a 2032 button battery.
[0081] Use Siken test system to conduct electrical performance test;
[0082] The battery was first charged to 4.5V at a constant current with a charge rate of 0.1C, and the charge capacity was recorded. Then, the battery was first discharged to 2.0V at a discharge rate of 0.1C, and the discharge capacity was recorded.
[0083] First 0.1C discharge specific capacity = 0.1C first discharge capacity / mass × 100%;
[0084] First efficiency = 0.1C first discharge capacity / 0.1C first charge capacity × 100%;
[0085] Charge to 4.5V at a constant current of 1C, and then discharge to 2.0V at a discharge rate of 1C, repeat 50 times, test the discharge capacity at the first cycle and the discharge capacity at the 50th cycle, and calculate the capacity retention rate;
[0086] 1C@50 cycles capacity retention rate = discharge capacity at the 50th cycle / discharge capacity at the 1st cycle × 100%;
[0087] The batteries prepared in the embodiments and comparative examples were tested, as shown in Table 1.
[0088] Table 1
[0089]
[0090]
[0091] The present invention uses iron-based sulfate together with a water-soluble carbon source, which can improve the conductivity while maintaining good stability; the precursor is coated with a sputtering technique and then sintered, which can improve the material stability while enhancing the ion transmission efficiency and conductivity; the battery containing the sodium ion battery positive electrode material finally prepared has excellent cycle performance, discharge specific capacity and first efficiency.
[0092] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A method for preparing a positive electrode material for a sodium ion battery, characterized in that: The specific steps of the preparation method include: S1, mixing a sodium source, an iron-based sulfate, a water-soluble carbon source and water and spray drying the mixture to obtain a precursor; S2. Sputtering and sintering the precursor to obtain a positive electrode material for a sodium ion battery.
2. The preparation method according to claim 1, characterized in that: The iron-based sulfate includes ferrous sulfate and / or ferric sulfate; Optionally, the ferrous sulfate includes at least one of ferrous sulfate heptahydrate, ferrous sulfate pentahydrate, ferrous sulfate monohydrate, and anhydrous ferrous sulfate; Optionally, the ferric sulfate includes ferric sulfate nonahydrate and / or anhydrous ferric sulfate.
3. The preparation method according to claim 1 or 2, characterized in that: The water-soluble carbon source includes at least one of ascorbic acid, citric acid, glucose, sucrose, acetic acid, propionic acid, and oxalic acid.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The sodium source includes at least one of sodium sulfate, sodium hydroxide, sodium carbonate and sodium oxalate; And / or, the molar ratio of the sodium element in the sodium source to the iron element in the iron-based sulfate is 1:1-3.
5. The preparation method according to any one of claims 1 to 4, characterized in that: Based on the total mass of the sodium source and the iron-based sulfate, the amount of the water-soluble carbon source is 2-30wt%, and the amount of water is 50-80wt%.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The spray drying inlet temperature is 150-170°C, and the outlet temperature is 90-110°C.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The sputtering uses a transition metal target, and the transition metal includes any one of Ni, Cu, and Zn.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The sintering process includes: heating to 270-300°C at a rate of 2-5°C / min for first-stage sintering, the sintering time is 4-7h, and then heating to 350-400°C at a rate of 2-5°C / min for second-stage sintering, the sintering time is 12-24h.
9. A sodium ion battery positive electrode material obtained by the preparation method according to any one of claims 1 to 8.
10. A secondary battery, characterized in that: The secondary battery comprises the sodium ion battery positive electrode material according to claim 9.