Triethylene diamine / vanadium pentoxide positive electrode material and preparation method and application thereof
Patent Information
- Application Number
- CN202411191567.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-08
AI Technical Summary
[0004]客体预嵌策略,现在比较普遍的是采用一种或多种金属阳离子嵌入五氧化二钒的水热法合成各类钒酸盐,该方法通常需要较长的反应时间,大概40小时左右,不利于这些正极材料的高效制备生产,而且电化学性能有待进一步提高
[0016] The present invention uses vanadium pentoxide as the main raw material and triethylenediamine as the pre-embedded guest to prepare the triethylenediamine/vanadium pentoxide positive electrode material. This method embeds the triethylenediamine into the pentoxide through microwave hydrothermal reaction. In the interlayer structure of vanadium oxide, the interlayer spacing of vanadium pentoxide is expanded. The vanadium pentoxide embedded in triethylenediamine shows an initial discharge specific capacity of 373mAh/g at a current density of 5A/g.
Smart Images

Figure CN118919696A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of battery positive electrode materials, and in particular to a triethylenediamine / vanadium pentoxide positive electrode material and a preparation method and application thereof. Background Art
[0002] In aqueous electrolytes, the standard potential of zinc metal is relatively low, and the electrochemical properties of zinc ions are stable, making zinc-ion batteries highly safe. In addition, the high ionic conductivity of aqueous electrolytes also helps to improve the power density of batteries. However, despite the many advantages of ZIBs, they still face many challenges in the selection and optimization of positive electrode materials.
[0003] Vanadium pentoxide (V2O5), as a transition metal oxide, is considered as one of the potential cathode materials for ZIBs due to its rich redox potential and multi-electron reaction characteristics. However, the inherent poor conductivity of V2O5 and the structural instability during repeated charge and discharge processes limit its performance and lifespan in practical applications. The guest pre-embedding strategy is an effective solution, which can alleviate the problems of poor conductivity and structural stability to a certain extent by embedding guest molecules or ions into the lattice of V2O5.
[0004] The guest pre-embedding strategy is now more common to use one or more metal cations to embed vanadium pentoxide into the hydrothermal method to synthesize various vanadates. This method usually requires a long reaction time, about 40 hours, which is not conducive to the efficient preparation and production of these positive electrode materials, and the electrochemical performance needs to be further improved. Summary of the invention
[0005] The purpose of the present invention is to address the above-mentioned deficiencies in the prior art and to provide a triethylenediamine / vanadium pentoxide positive electrode material and a preparation method and application thereof.
[0006] The invention discloses a method for preparing a triethylenediamine / vanadium pentoxide positive electrode material, comprising the following steps: mixing vanadium pentoxide with a triethylenediamine solution and subjecting the mixture to a microwave hydrothermal reaction; after the reaction is completed, washing, drying and grinding the reaction product to obtain the positive electrode material.
[0007] Furthermore, the microwave hydrothermal reaction temperature is 160-180°C and the time is 1-4h.
[0008] Furthermore, the concentration of the triethylenediamine solution is 0.1 mol / L.
[0009] Furthermore, the molar ratio of triethylenediamine to vanadium pentoxide is 0.2-1.
[0010] Furthermore, the centrifugal method was used for washing, and the number of washing times was 3 times.
[0011] Furthermore, the drying method is forced air drying, the drying temperature is 70-80° C., and the drying time is 10-12 hours.
[0012] A triethylenediamine / vanadium pentoxide positive electrode material prepared by the above-mentioned preparation method.
[0013] A positive electrode for an aqueous zinc ion battery is prepared by mixing the triethylenediamine / vanadium pentoxide positive electrode material with conductive carbon powder and a binder, adding a dispersant N-methylpyrrolidone, and magnetically stirring to obtain a slurry. The prepared slurry is evenly coated on a stainless steel mesh to construct the positive electrode for an aqueous zinc ion battery.
[0014] Furthermore, the mass ratio of the triethylenediamine / vanadium pentoxide positive electrode material to the conductive carbon powder and the binder is 7-5:2-1:1.
[0015] An aqueous zinc ion battery is provided. The aqueous zinc ion battery positive electrode, a glass fiber separator, an aqueous electrolyte and a zinc sheet negative electrode are assembled into an aqueous zinc ion battery, wherein the binder is polyvinylidene fluoride and the aqueous electrolyte is a 3 mol / L zinc trifluoromethanesulfonate solution.
[0016] The invention uses vanadium pentoxide as a main raw material and triethylenediamine as a pre-embedded guest to prepare a triethylenediamine / vanadium pentoxide positive electrode material. The method embeds triethylenediamine into the interlayer structure of vanadium pentoxide through a microwave hydrothermal reaction, so that the interlayer spacing of vanadium pentoxide is expanded. The vanadium pentoxide embedded in triethylenediamine exhibits an initial discharge specific capacity of 373 mAh / g at a current density of 5 A / g.
[0017] The present invention greatly shortens the hydrothermal reaction time through microwave hydrothermal reaction and makes the prepared positive electrode material have good uniformity. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The full spectrum of the X-ray electron spectrum (XPS) of the positive electrode material powder obtained in Example 1;
[0019] Figure 2 The scanning electron microscope (SEM) image and elemental mapping (EDS) image of the positive electrode material powder obtained in Example 1;
[0020] Figure 3 The electron diffraction pattern of the positive electrode material powder obtained in Example 1 under a transmission electron microscope (TEM);
[0021] Figure 4a X-ray diffraction (XRD) diagram of the positive electrode material powder obtained in Examples 1-4;
[0022] Figure 4bX-ray diffraction (XRD) diagram of the positive electrode material powder obtained in Examples 5-8;
[0023] Figure 5a The cycle comparison diagram of the positive electrode materials prepared in Examples 1 to 3 for aqueous zinc ion batteries at a current density of 5 A / g;
[0024] Figure 5b This is a cycle comparison diagram of the positive electrode material prepared in Example 4 for aqueous zinc ion batteries at a current density of 5 A / g;
[0025] Figure 5c The cycle comparison diagram of the positive electrode material prepared in Example 5-8 for aqueous zinc ion battery at a current density of 5A / g;
[0026] Figure 6a A comparison chart of the rate performance of the positive electrode materials prepared in Examples 1 to 3 for aqueous zinc ion batteries at a current density of 0.1 to 5 A / g;
[0027] Figure 6b This is a comparison chart of the rate performance of the positive electrode material prepared in Example 4 for aqueous zinc ion batteries at a current density of 0.1 to 5 A / g;
[0028] Figure 6c A comparison chart of the rate performance of the positive electrode materials prepared in Examples 5 to 8 for aqueous zinc ion batteries at a current density of 0.1 to 5 A / g;
[0029] Figure 7 The cyclic voltammetry curve of the positive electrode material prepared in Example 1 for aqueous zinc ion battery at a scan rate of 0.1 mV / s. DETAILED DESCRIPTION
[0030] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.
[0031] Example 1
[0032] 0.18g of vanadium pentoxide, 2mL of pre-prepared triethylenediamine solution with a concentration of 0.1mol / L and 38mL of deionized water were added to a microwave reactor in sequence, and microwave heating was performed for 1 hour at a temperature of 180°C. After the reaction was completed, the reaction product was cooled to 40°C, washed with deionized water three times, dried by air drying, and then ground to obtain a vanadium pentoxide positive electrode material embedded with triethylenediamine molecules.
[0033] Example 2
[0034] 0.18 g of vanadium pentoxide, 5 mL of pre-prepared 0.1 mol / L triethylenediamine solution and 35 mL of deionized water were added to a microwave reactor in sequence, and microwave heating was performed for 1 hour at a temperature of 180°C. After the reaction was completed, the reaction product was cooled to 40°C, washed with deionized water three times, dried by air drying, and then ground to obtain a vanadium pentoxide cathode material embedded with triethylenediamine molecules.
[0035] Example 3
[0036] 0.18 g of vanadium pentoxide, 10 mL of a pre-prepared 0.1 mol / L triethylenediamine solution and 30 mL of deionized water were added to a microwave reactor in sequence, and microwave heating was performed for 1 hour at a temperature of 180°C. After the reaction was completed, the reaction product was cooled to 40°C, washed with deionized water three times, dried by a forced air drying method, and then ground to obtain a vanadium pentoxide cathode material embedded with triethylenediamine molecules.
[0037] Example 4
[0038] 0.18 g of vanadium pentoxide, 0.5 mL of a pre-prepared 0.1 mol / L triethylenediamine solution, and 39.5 mL of deionized water were added to a microwave reactor in sequence, and microwave heating was performed for 1 hour at a temperature of 180° C. After the reaction was completed, the reaction product was cooled to 40° C., washed with deionized water three times, dried by a forced air drying method, and then ground to obtain a vanadium pentoxide positive electrode material in which triethylenediamine molecules were embedded.
[0039] Example 5
[0040] 0.18g of vanadium pentoxide, 2mL of pre-prepared triethylenediamine solution with a concentration of 0.1mol / L and 38mL of deionized water were added to a microwave reactor in sequence, and microwave heating was performed for 4 hours at a temperature of 180°C. After the reaction was completed, the reaction product was cooled to 40°C, washed with deionized water three times, dried by air drying, and then ground to obtain a vanadium pentoxide positive electrode material embedded with triethylenediamine molecules.
[0041] Example 6
[0042] 0.18 g of vanadium pentoxide, 5 mL of pre-prepared 0.1 mol / L triethylenediamine solution and 35 mL of deionized water were added to a microwave reactor in sequence, and microwave heating was performed for 4 hours at a temperature of 180°C. After the reaction was completed, the reaction product was cooled to 40°C, washed with deionized water three times, dried by air drying, and then ground to obtain a vanadium pentoxide cathode material embedded with triethylenediamine molecules.
[0043] Example 7
[0044] 0.18 g of vanadium pentoxide, 10 mL of a pre-prepared 0.1 mol / L triethylenediamine solution and 30 mL of deionized water were added to a microwave reactor in sequence, and microwave heating was performed for 4 hours at a temperature of 180°C. After the reaction was completed, the reaction product was cooled to 40°C, washed with deionized water three times, dried by a forced air drying method, and then ground to obtain a vanadium pentoxide cathode material embedded with triethylenediamine molecules.
[0045] Example 8
[0046] 0.18 g of vanadium pentoxide, 0.5 mL of a pre-prepared 0.1 mol / L triethylenediamine solution, and 39.5 mL of deionized water were added to a microwave reactor in sequence, and microwave heating was performed for 4 hours at a temperature of 180°C. After the reaction was completed, the reaction product was cooled to 40°C, washed with deionized water three times, dried by a forced air drying method, and then ground to obtain a vanadium pentoxide cathode material in which triethylenediamine molecules were embedded.
[0047] Assembled into aqueous zinc ion button battery
[0048] The above positive electrode materials are mixed with conductive carbon powder and binder at a mass ratio of 7:2:1, and the dispersant is N-methylpyrrolidone. The prepared slurry is evenly coated on a stainless steel mesh to construct an aqueous zinc ion battery positive electrode by magnetic stirring for 12 hours, and then the aqueous zinc ion battery positive electrode, glass fiber separator, aqueous electrolyte, and zinc sheet negative electrode are assembled into an aqueous zinc ion button battery. The binder is polyvinylidene fluoride, and the aqueous electrolyte is a 3 mol / L zinc trifluoromethanesulfonate solution.
[0049] SEM and EDS testing:
[0050] Figure 1 The morphology and element mapping of the positive electrode material obtained in Example 1 under a scanning electron microscope are shown. In the figure, elements such as carbon, nitrogen, oxygen, and vanadium are evenly distributed, indicating the successful embedding of triethylenediamine molecules.
[0051] XPS Test:
[0052] The chemical element composition of the positive electrode material obtained in Example 1 was analyzed by XPS. Figure 2 As shown, the characteristic peaks of carbon, nitrogen, oxygen, vanadium and other elements clearly appear in the spectrum, verifying Figure 1 conclusion.
[0053] TEM test:
[0054] In order to explore whether the embedding of triethylenediamine molecules affects the crystal structure of vanadium pentoxide, the microstructure of the positive electrode material prepared in Example 1 was observed using a transmission electron microscope. Figure 3This is an electron diffraction pattern of the positive electrode material powder obtained in Example 1 under a projection electron microscope. The diffraction rings in the figure correspond to the (201), (401) and (710) crystal planes of the original vanadium pentoxide, but the diffraction rings of other crystal planes of vanadium pentoxide are not obvious, indicating that the embedding of triethylenediamine molecules has a certain influence on the crystal structure of vanadium pentoxide.
[0055] XRD test:
[0056] In order to further explore the crystal structure of vanadium pentoxide embedded in triethylenediamine molecules, XRD tests were performed on the positive electrode material powders prepared in Examples 1-8. Figure 4a and Figure 4b The X-ray diffraction diagram of the positive electrode material powder obtained in Example 1-8 shows that when the amount of triethylenediamine added increases, the embedding of triethylenediamine molecules expands the interlayer spacing of the (001) crystal plane of vanadium pentoxide. Generally, the interlayer spacing corresponding to the (001) crystal plane of vanadium pentoxide is After calculation, the main peak interlayer spacing of the positive electrode materials prepared in Examples 1-4, i.e., the interlayer spacing of the (001) crystal plane, is The main peak interlayer distances of the positive electrode materials obtained in Examples 5-8 are That is, the interlayer distance of Example 1 is the largest. This means that the interlayers of vanadium pentoxide embedded in triethylenediamine molecules can accommodate more zinc ions, thereby providing more capacity.
[0057] Electrochemical testing
[0058] Long cycle test:
[0059] Using a BlueDian electrochemical workstation, a long cycle test was performed on an aqueous zinc ion button cell assembled with the positive electrode material prepared in the above embodiment at a current density of 5A / g. Figure 5a As shown, Examples 1 to 3 all exhibit good cycle stability, and Example 1 has the highest discharge specific capacity. Figure 5b The long cycle test of Example 4 is tested, as Figure 5b As shown in the figure, its capacity gradually increases in the first 500 cycles, indicating that the material is in an unactivated state at the beginning; when the capacity reaches the peak, it can only remain stable for a period of time, and then the capacity begins to decrease. This phenomenon is similar to the performance of vanadium pentoxide directly as a positive electrode material, that is, a small amount of triethylenediamine molecules embedded cannot improve the cycle stability of vanadium pentoxide. Figure 5c As shown in the cycle diagram of Examples 4-6 under high current density, the difference from Examples 1-3 is that the reaction time is changed from 1 hour to 4 hours. It can be found that although the cycle stability of Examples 5-8 is good during 1500 cycles, the initial capacity decreases and the overall capacity is less than that of Examples 1-4.
[0060] Rate performance test:
[0061] Using a BlueDian electrochemical workstation, the rate performance test of the aqueous zinc ion button cell assembled with the positive electrode material prepared in the above embodiment was carried out at a current density of 0.1 to 5 A / g. Figure 6a and 6b As shown, at each current density, Example 1 exhibits the highest discharge specific capacity.
[0062] Figure 6c The positive electrode materials prepared in Examples 5 to 8 are used in aqueous zinc ion batteries for rate performance comparison at current densities of 0.1 to 5 A / g. It can be seen that Examples 5-8 also have good rate performance. At the same current density, the capacity of Examples 1-4 is higher than that of Examples 5-8.
[0063] Cyclic voltammetry test:
[0064] Using a Chenhua electrochemical workstation, the positive electrode material prepared in Example 1 was subjected to a cyclic voltammetry test at a scan rate of 0.1 mV / s. Figure 7 is the cyclic voltammetry curve of Example 1, from Figure 7 It can be seen that the first three cyclic voltammetry curves of Example 1 almost completely overlap, indicating that the positive electrode material prepared in Example 1 has good reversibility.
[0065] For matters not mentioned above, the prior art applies.
[0066] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a triethylenediamine / vanadium pentoxide positive electrode material, characterized in that: The following steps are involved: The vanadium pentoxide and triethylenediamine solution are mixed and then subjected to microwave hydrothermal reaction. After the reaction is completed, the reaction product is washed, dried and ground to obtain the triethylenediamine / vanadium pentoxide positive electrode material.
2. The preparation method according to claim 1, characterized in that The microwave hydrothermal reaction temperature is 160-180°C and the time is 1-4h.
3. The preparation method according to claim 1, characterized in that: The concentration of triethylenediamine solution is 0.1 mol / L.
4. The preparation method according to claim 1, characterized in that: The molar ratio of triethylenediamine to vanadium pentoxide is 0.2-1.
5. The preparation method according to claim 1, characterized in that: The centrifugal method was used for washing, and the number of washing times was 3 times.
6. The preparation method according to claim 1, characterized in that: The drying method is air drying, the drying temperature is 70-80°C, and the drying time is 10-12 hours.
7. A triethylenediamine / vanadium pentoxide positive electrode material prepared by the preparation method according to any one of claims 1 to 6.
8. An aqueous zinc ion battery positive electrode, characterized in that: The triethylenediamine / vanadium pentoxide positive electrode material as claimed in claim 7 is mixed with conductive carbon powder and a binder, and a dispersant N-methylpyrrolidone is added, and a slurry is obtained by magnetic stirring. The prepared slurry is evenly coated on a stainless steel mesh to construct an aqueous zinc ion battery positive electrode.
9. The aqueous zinc ion battery positive electrode according to claim 8, characterized in that: The mass ratio of the triethylenediamine / vanadium pentoxide positive electrode material to the conductive carbon powder and the binder is 7-5:2-1:
1.
10. An aqueous zinc ion battery, characterized in that: The aqueous zinc ion battery positive electrode, glass fiber separator, aqueous electrolyte, and zinc sheet negative electrode as described in claim 8 are assembled into an aqueous zinc ion battery, wherein the binder is polyvinylidene fluoride and the aqueous electrolyte is a 3 mol / L zinc trifluoromethanesulfonate solution.
Citation Information
Cited By
Vanadium oxide positive electrode intercalation layer for battery and preparation method of vanadium oxide positive electrode intercalation layer
CN119673939A