Positive electrode material and preparation method thereof, positive electrode plate and secondary battery

By forming an oxygen vacancy defect metal oxide coating on the core surface of the lithium-rich positive electrode material, the problems of low discharge specific capacity, low first efficiency and poor cycle retention rate are solved, and high discharge specific capacity, high first efficiency and A positive electrode material with high cycle retention.

CN118919697APending Publication Date: 2024-11-08TIANJIN B&M SCI & TECH LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411198149.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Due to its unique anionic redox reaction, lithium-rich cathode materials have problems such as low discharge specific capacity, low first efficiency and poor cycle retention.

Method used

A positive electrode material is used, and its core comprises a material with a chemical formula of Li1.2-mNi0.8+m-q-xMnqQxO2, the Q element includes at least one of Co, Al and Zr, and the coating is an oxygen vacancies defective metal oxide, The cladding layer is formed through a two-step sintering process to improve the oxygen vacancies on the core surface and retain the integrity of the lattice oxygen skeleton.

Benefits of technology

The discharge specific capacity, first effect and cycle retention rate of the positive electrode material are improved, the lithium ion diffusion energy barrier is reduced, the lithium ion kinetic process is improved, the material stability is enhanced, the side reactions are suppressed, and the circulation performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919697A_ABST
    Figure CN118919697A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, and provides a positive electrode material and a preparation method thereof, a positive electrode plate and a secondary battery, the positive electrode material comprises an inner core and a coating layer coating at least part of the surface of the inner core; the inner core comprises a material with a chemical formula of Li (1.2-m) Ni (0.8 + m-q-xMnqQxO2, the element Q comprises at least one of Co, Al and Zr, m is more than or equal to 0 and less than or equal to 0.2, q is more than or equal to 0.5 and less than or equal to 1, and x is more than or equal to 0 and less than or equal to 0.3; and the material of the coating layer comprises an oxygen vacancy defect metal oxide. The lithium ion battery has the characteristics of high specific discharge capacity, high first efficiency, high cycle retention rate and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a positive electrode material and a preparation method thereof, a positive electrode sheet and a secondary battery. Background Art

[0002] Lithium-rich positive electrode materials refer to a type of material in which the molar ratio of lithium to all transition metals in the chemical formula is greater than 1. The nickel and cobalt content is low, and the main transition metals can be selected from elements with high crustal abundance such as manganese. Manganese is cheap, and lithium-rich positive electrode materials have cost advantages over other positive electrode materials. In addition, the theoretical specific capacity of lithium-rich positive electrode materials is above 300mAh / g, and the average discharge voltage is above 3.6V, which meets the needs of battery use. However, due to its unique anion redox reaction, lithium-rich positive electrode materials have problems such as low discharge specific capacity, low initial efficiency and poor cycle retention rate. Summary of the invention

[0003] Based on this, an embodiment of the present application provides a positive electrode material with high discharge specific capacity, high initial efficiency and high cycle retention rate, and a preparation method thereof, a positive electrode plate and a secondary battery.

[0004] In a first aspect, the present application provides a positive electrode material, the positive electrode material comprising a core and a coating layer coated on at least a portion of the surface of the core; the core comprises a chemical formula of Li 1.2-m Ni 0.8+m-q-x Mn q Q x O2 material, wherein the Q element includes at least one of Co, Al and Zr, 0≤m≤0.2, 0.5≤q≤1, 0≤x≤0.3; the material of the coating layer includes oxygen vacancy defect metal oxide.

[0005] In some embodiments, the positive electrode material satisfies: 25%≤O v1 / (O v1 +O L1 )≤50%, where O v1 is the peak area of ​​the characteristic peak where the oxygen vacancy is located in the O1s orbital fine spectrum in the XPS test spectrum of the positive electrode material; L1 It is the peak area of ​​the characteristic peak of lattice oxygen in the O1s orbital fine spectrum in the XPS test spectrum of the positive electrode material.

[0006] In some embodiments, the median binding energy of oxygen vacancies in the positive electrode material after charge correction is higher than the binding energy of a characteristic peak of lattice oxygen in the positive electrode material.

[0007] Optionally, the median value of oxygen vacancy binding energy of the positive electrode material after charge correction is 531eV~534eV, and the median value of lattice oxygen binding energy is 528eV~531eV.

[0008] In some embodiments, the oxygen vacancy defect metal oxide satisfies: 10%≤O v2 / (O v2 +O L2 )≤50%, where O v2 is the peak area of ​​the characteristic peak where the oxygen vacancy is located in the O1s orbital fine spectrum in the XPS test spectrum of the oxygen vacancy defect metal oxide; L2 It is the peak area of ​​the characteristic peak where lattice oxygen is located in the O1s orbital fine spectrum in the XPS test spectrum of the oxygen vacancy defect metal oxide.

[0009] In some embodiments, the charge-corrected median binding energy of the oxygen vacancy defective metal oxide is higher than the binding energy of the characteristic peak of lattice oxygen of the oxygen vacancy defective metal oxide.

[0010] Optionally, the median value of oxygen vacancy binding energy of the oxygen vacancy defect metal oxide after charge correction is 531eV~534eV, and the median value of lattice oxygen binding energy is 528eV~531eV.

[0011] In some embodiments, the crystal structure of the inner core comprises a layered α-NaFeO 2 structure.

[0012] Optionally, the core has a Li2MnO3 characteristic diffraction peak in the range of 20°~30°.

[0013] In some embodiments, the metal element in the oxygen vacancy defect metal oxide includes at least one of Ni, Co, Mn, Ti, Al, W, V, Mo, Ce, Fe, Cr, La and Zr.

[0014] Optionally, the metal element in the oxygen vacancy defect metal oxide includes at least one of Ti, W, Ce and La.

[0015] In some embodiments, the mass proportion of the coating layer in the positive electrode material is 500ppm~20000ppm.

[0016] In some embodiments, the volume median particle size Dv50 of the positive electrode material is 2 μm to 15 μm.

[0017] In some embodiments, the positive electrode material includes secondary particles formed by aggregation of primary particles, and a volume median particle size Dv50 of the primary particles is 100 nm to 500 nm.

[0018] In some embodiments, the positive electrode material further includes a doping layer, the doping layer is located between the core and the coating layer, and the doping layer includes a chemical formula of Li 1.2-m Ni0.8+m-q-x-y Mn q Q x M y The material of O2, the M element includes the metal element contained in the oxygen vacancy defect metal oxide, 0<y≤0.01.

[0019] Optionally, the mass proportion of the doping layer in the positive electrode material is 500ppm~5000ppm.

[0020] In a second aspect, the present application provides a method for preparing a positive electrode material, the method for preparing a positive electrode material comprising:

[0021] A lithium source and a positive electrode material precursor are mixed to obtain a mixture, and the mixture is subjected to a first sintering to obtain a mixture containing a chemical formula of Li 1.2-m Ni 0.8+m-q-x Mn q Q x The core of the material of O2, wherein the Q element includes at least one of Co, Al and Zr, 0≤m≤0.2, 0.5≤q≤1, 0≤x≤0.3;

[0022] The inner core and the oxygen vacancy defect metal oxide are mixed, and after a second sintering, a coating layer containing the oxygen vacancy defect metal oxide is formed on at least a portion of the surface of the inner core to prepare the positive electrode material.

[0023] In some embodiments, the first sintering includes: performing a first sintering step and a second sintering step on the mixture in sequence.

[0024] Optionally, the first sintering step has a temperature of 400° C. to 600° C., a heating rate of 1.0° C. / min to 5.0° C. / min, a sintering time of 1 h to 10 h, and an oxygen-containing atmosphere.

[0025] Optionally, the second step sintering has a temperature of 600°C to 1000°C, a heating rate of 1.0°C / min to 5.0°C / min, a time of 6h to 20h, and an oxygen-containing atmosphere.

[0026] In some embodiments, the second sintering is performed at a temperature of 150° C. to 500° C., a heating rate of 1.0° C. / min to 5.0° C. / min, a time of 1 h to 10 h, and an oxygen volume fraction in the sintering atmosphere of 0% to 25%.

[0027] In a third aspect, the present application provides a positive electrode plate, comprising at least one of the positive electrode material as described in the first aspect and the positive electrode material prepared by the preparation method as described in the second aspect.

[0028] In a fourth aspect, the present application provides a secondary battery, comprising the positive electrode plate as described in the third aspect.

[0029] Compared with the traditional technology, this application has at least the following beneficial effects:

[0030] The positive electrode material of the present application forms a coating layer containing oxygen vacancy defective metal oxide on the surface of the inner core, which can inherit the oxygen vacancies in the oxygen vacancy defective metal oxide to the inner core surface, which is more conducive to increasing the oxygen vacancy content on the inner core surface, thereby solving the problem of oxygen loss in the inner core, while retaining the integrity of the oxygen skeleton inside the lattice, while retaining the anion redox capacity, improving the cycle performance and storage performance. Moreover, the introduction of oxygen vacancies can also reduce the lithium ion diffusion barrier, increase the lithium ion diffusion rate, and then promote the lithium ion kinetic process, improve the first effect and cycle performance. In addition, the surface of the positive electrode material of the present application has additional oxygen vacancies, which can improve the material stability, help to suppress the gas production during the formation, and also improve the cycle stability of the positive electrode material, suppress the occurrence of side reactions, and help to improve the cycle performance. The positive electrode material of the present application has the characteristics of high discharge specific capacity, high first efficiency and high cycle retention rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a SEM image of the positive electrode material prepared in Example 1 of the present application;

[0032] Figure 2 The positive electrode material in Example 1 of the present application, the positive electrode material in Comparative Example 2 and WO 2.72 XPS test spectrum. DETAILED DESCRIPTION

[0033] Below in conjunction with the embodiments and examples, the present application is further described in detail. These embodiments and examples are only used to illustrate the present application and are not used to limit the scope of the present application. The purpose of providing these embodiments and examples is to make the understanding of the disclosure of the present application more thorough and comprehensive. It should also be understood that the present application can be implemented in many different forms, and is not limited to the embodiments and examples described herein. Those skilled in the art can make various changes or modifications without violating the connotation of the present application, and the equivalent form obtained also falls within the protection scope of the present application. In addition, in the description below, a large number of specific details are given in order to provide a more comprehensive understanding of the present application. It should be understood that the present application can be implemented without one or more of these details.

[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0035] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.

[0036] In this application, the terms "first", "second", etc. in "the first aspect", "the second aspect", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0037] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0038] In the present application, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values ​​in the numerical interval is considered to be continuous, and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to an integer in the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints, which is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined. In other words, unless otherwise specified, the numerical range disclosed in the present application should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows for a broad range of quantitative intervals such as percentage intervals, ratio intervals, and ratio intervals.

[0039] All documents mentioned in this application are cited as references in this application, just as each document is cited as reference separately. Unless they conflict with the application purpose and / or technical solution of this application, the cited documents involved in this application are cited with all contents and all purposes. When the cited documents are involved in this application, the definitions of relevant technical features, terms, nouns, phrases, etc. in the cited documents are also cited. When the cited documents are involved in this application, the examples and preferred methods of the cited relevant technical features can also be incorporated into this application as references, but are limited to the implementation of this application. It should be understood that when the cited content conflicts with the description in this application, the present application shall prevail or be modified adaptively according to the description of this application.

[0040] In traditional technology, lithium-rich cathode materials are modified by high-valent element doping, liquid phase treatment, and surface inert layer coating. For example, metal oxides and conductive polymers are co-coated on the surface of lithium-rich cathode materials through a two-step hydrothermal method to improve cycle performance. However, surface inert layer coating will reduce the proportion of active substances and increase impedance, affecting the cycle performance and initial efficiency of the battery.

[0041] In a first aspect, the present application provides a positive electrode material, the positive electrode material comprising a core and a coating layer coated on at least a portion of the surface of the core; the core comprises a chemical formula of Li 1.2-m Ni 0.8+m-q-x Mn q Q x O2 material, wherein the Q element includes at least one of Co, Al and Zr, 0≤m≤0.2, 0.5≤q≤1, 0≤x≤0.3; the material of the coating layer includes oxygen vacancy defect metal oxide.

[0042] The positive electrode material of the present application forms a coating layer containing oxygen vacancy defective metal oxide on the surface of the inner core, which can inherit the oxygen vacancies in the oxygen vacancy defective metal oxide to the inner core surface, which is more conducive to increasing the oxygen vacancy content on the inner core surface, thereby solving the problem of oxygen loss in the inner core, while retaining the integrity of the oxygen skeleton inside the lattice, while retaining the anion redox capacity, improving the cycle performance and storage performance. Moreover, the introduction of oxygen vacancies can also reduce the lithium ion diffusion barrier, increase the lithium ion diffusion rate, and then promote the lithium ion kinetic process, improve the first effect and cycle performance. In addition, the surface of the positive electrode material of the present application has additional oxygen vacancies, which can improve the material stability, help to suppress the gas production during the formation, and also improve the cycle stability of the positive electrode material, suppress the occurrence of side reactions, and help to improve the cycle performance. The positive electrode material of the present application has the characteristics of high discharge specific capacity, high first efficiency and high cycle retention rate.

[0043] Wherein, m includes but is not limited to: 0, 0.02, 0.04, 0.06, 0.08, 0.10, 0.12, 0.14, 0.16, 0.18 or 0.20. q includes but is not limited to: 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95 or 1.00. x includes but is not limited to: 0, 0.03, 0.06, 0.09, 0.12, 0.15, 0.18, 0.21, 0.24, 0.27 or 0.30.

[0044] It is understood that oxygen vacancy defect metal oxide refers to the oxygen atom in the metal oxide lattice that is separated and causes oxygen deficiency to form vacancies. p-zIt is represented by, where M represents the metal element in the metal oxide, and the p value represents the ratio of the oxidation state of the M element to the oxygen element. For example, when the M element is W and the oxidation state of W is +6, p is 3. The z value represents the ratio of oxygen atom vacancies, 0<z≤p. Oxygen vacancy defect metal oxides can be WO 2.72 or La3Li7Zr2O 12 For example, oxygen vacancies in oxygen vacancy defect metal oxides can be formed by sintering in a reducing atmosphere, heating with a metal element, or treating with an acidic substance. Compared with directly forming oxygen vacancies on the positive electrode material, there are more optional processes.

[0045] In some embodiments, the positive electrode material satisfies: 25%≤O v1 / (O v1 +O L1 )≤50%, for example, it can be 25%, 26%, 28%, 30%, 32%, 34%, 36%, 38%, 40%, 42%, 44%, 46%, 48% or 50%. v1 is the peak area of ​​the characteristic peak where the oxygen vacancy is located in the O1s orbital fine spectrum in the XPS test spectrum of the positive electrode material; L1 It is the peak area of ​​the characteristic peak of lattice oxygen in the O1s orbital fine spectrum in the XPS test spectrum of the positive electrode material.

[0046] The positive electrode material of the present application has the above oxygen vacancy content, and has a higher oxygen vacancy content than the lithium-rich positive electrode material, and has the advantages of high initial efficiency, good cycle stability, and low gas production.

[0047] In some embodiments, the charge-corrected median binding energy of oxygen vacancies in the positive electrode material is higher than the binding energy of a characteristic peak of lattice oxygen in the positive electrode material.

[0048] Optionally, the charge-corrected oxygen vacancy binding energy median of the cathode material is 531eV-534eV, and the lattice oxygen binding energy median is 528eV-531eV. It is understandable that in the XPS test, the binding energy of the cathode material will appear in the form of a peak on the spectrum, and the median of the peak is the median binding energy.

[0049] In some embodiments, the oxygen vacancy defect metal oxide satisfies: 10%≤O v2 / (O v2 +O L2 )≤50%, for example, it can be 10%, 14%, 18%, 22%, 26%, 30%, 34%, 38%, 42%, 46% or 50%. v2 is the peak area of ​​the characteristic peak where the oxygen vacancy is located in the O1s orbital fine spectrum in the XPS test spectrum of the oxygen vacancy defect metal oxide;L2 It is the peak area of ​​the characteristic peak where lattice oxygen is located in the O1s orbital fine spectrum in the XPS test spectrum of the oxygen vacancy defect metal oxide.

[0050] The oxygen vacancy defect metal oxide of the present application has the above oxygen vacancy content, and the positive electrode material has high initial efficiency, good cycle stability and low gas production.

[0051] In some embodiments, the charge-corrected median binding energy of the oxygen vacancy defective metal oxide is higher than the binding energy of the characteristic peak of lattice oxygen of the oxygen vacancy defective metal oxide.

[0052] Optionally, the median value of oxygen vacancy binding energy of the oxygen vacancy defect metal oxide after charge correction is 531eV~534eV, and the median value of lattice oxygen binding energy is 528eV~531eV.

[0053] In some embodiments, the crystal structure of the core comprises a layered α-NaFeO2 structure. The core has a characteristic diffraction peak of Li2MnO3 in the range of 20° to 30°.

[0054] In some embodiments, the metal element in the oxygen vacancy defect metal oxide includes at least one of Ni, Co, Mn, Ti, Al, W, V, Mo, Ce, Fe, Cr, La and Zr. Optionally, the metal element in the oxygen vacancy defect metal oxide includes at least one of Ti, W, Ce and La. The present application selects metal elements with high valence and short bond length, which can enhance the bond energy of the covalent bond between the transition metal and the lattice oxygen and increase the stability of oxygen.

[0055] In some embodiments, the mass proportion of the coating layer in the positive electrode material is 500ppm~20000ppm, for example, it can be 500ppm, 1000ppm, 2000ppm, 4000ppm, 6000ppm, 8000ppm, 10000ppm, 12000ppm, 14000ppm, 16000ppm, 18000ppm or 20000ppm. The quality of the coating layer in the positive electrode material selected in the present application as above can improve the first effect and cycle stability of the positive electrode material and reduce gas production.

[0056] In some embodiments, the volume median particle size Dv50 of the positive electrode material is 2 μm to 15 μm, for example, it can be 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm or 15 μm.

[0057] In some embodiments, the morphology of the cathode material includes particles with spherical and spherical-like morphologies.

[0058] In some embodiments, the positive electrode material includes secondary particles formed by aggregation of primary particles, and the volume median particle size Dv50 of the primary particles is 100nm~500nm, for example, it can be 100nm, 140nm, 180nm, 220nm, 260nm, 300nm, 340nm, 380nm, 420nm, 460nm or 500nm.

[0059] In some embodiments, the positive electrode material further includes a doping layer, the doping layer is located between the core and the coating layer, and the doping layer contains a chemical formula of Li 1.2-m Ni 0.8+m-q-x-y Mn q Q x M y The material of O2, the M element includes the metal element contained in the oxygen vacancy defect metal oxide, 0<y≤0.01.

[0060] In the present application, a doping layer is formed between the coating layer and the core. The doping elements of the doping layer include metal elements in oxygen vacancy defect metal oxides, which can enhance the covalent bond energy between the transition metal and the lattice oxygen, provide a transition for the coating layer, and enhance the coating effect.

[0061] Wherein, y includes but is not limited to: 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.007, 0.008, 0.009 or 0.010.

[0062] It can be understood that in the present application, the doping layer can be formed separately, or it can be formed by the coating element penetrating into the surface of the inner core when the coating layer is formed.

[0063] Optionally, the mass proportion of the doping layer in the positive electrode material is 500ppm~5000ppm, for example, it can be 500ppm, 1000ppm, 1500ppm, 2000ppm, 2500ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm or 5000ppm.

[0064] The second aspect of the present application provides a method for preparing a positive electrode material, the method for preparing a positive electrode material comprising:

[0065] A lithium source and a positive electrode material precursor are mixed to obtain a mixture, and the mixture is subjected to a first sintering to obtain a mixture containing a chemical formula of Li 1.2-m Ni 0.8+m-q-x Mn q Q x The core of the material of O2, wherein the Q element includes at least one of Co, Al and Zr, 0≤m≤0.2, 0.5≤q≤1, 0≤x≤0.3;

[0066] The inner core and the oxygen vacancy defect metal oxide are mixed, and after a second sintering, a coating layer containing the oxygen vacancy defect metal oxide is formed on at least a portion of the surface of the inner core to prepare the positive electrode material.

[0067] In the preparation process of this application, a full solid-phase in-situ inheritance coating process is adopted, and a defective metal oxide rich in oxygen vacancies is directly coated on the surface of the inner core, which can not only inherit the oxygen vacancies in the defective oxide to the surface of the inner core, but also is more conducive to increasing the oxygen vacancy content on the surface of the positive electrode material, and can inhibit the loss of oxygen on the surface of the positive electrode material through oxygen vacancies; and effectively retain the oxygen vacancy structure of the defective metal oxide, which can reduce the complexity of the process; compared with the indirect synthesis coating process, it avoids the problem of spontaneous recombination of defective metal oxides during annealing and sintering, causing oxygen vacancy loss. In addition, the introduction of oxygen vacancies can also reduce the lithium ion diffusion barrier, increase the lithium ion diffusion rate, and then promote the lithium ion kinetic process, and improve the first effect and cycle performance.

[0068] In some embodiments, the molar ratio between the positive electrode material precursor and the lithium element in the lithium source is 1:(1.04~1.56), for example, it can be 1:1.04, 1:1.10, 1:1.15, 1:1.20, 1:1.25, 1:1.30, 1:1.35, 1:1.40, 1:1.45, 1:1.50, 1:1.55 or 1:1.56.

[0069] In some embodiments, the chemical formula of the positive electrode material precursor is Ni a Mn b Q c (OH)2, wherein Q includes at least one of Co, Al and Zr, 0≤a≤0.5, 0.5≤b≤1, 0≤c≤0.3, a+b+c=1. Wherein, a includes but is not limited to: 0, 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.45 or 0.50. b includes but is not limited to: 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95 or 1.00. c includes but is not limited to: 0, 0.03, 0.06, 0.09, 0.12, 0.15, 0.18, 0.21, 0.24, 0.27 or 0.30.

[0070] In some embodiments, the lithium source includes lithium carbonate, lithium hydroxide, lithium sulfate, lithium acetate, or lithium oxalate.

[0071] In some embodiments, the mass of the oxygen vacancy defect metal oxide is 500ppm~20000ppm of the core mass, for example, it can be 500ppm, 1000ppm, 2000ppm, 4000ppm, 6000ppm, 8000ppm, 10000ppm, 12000ppm, 14000ppm, 16000ppm, 18000ppm or 20000ppm.

[0072] In some embodiments, the first sintering includes: performing a first sintering step and a second sintering step on the mixture in sequence.

[0073] In some embodiments, the temperature of the first sintering step is 400°C to 600°C, for example, it can be 400°C, 420°C, 440°C, 460°C, 480°C, 500°C, 520°C, 540°C, 560°C, 580°C or 600°C.

[0074] In some embodiments, the heating rate of the first sintering step is 1.0°C / min~5.0°C / min, for example, it can be 1.0°C / min, 1.5°C / min, 2.0°C / min, 2.5°C / min, 3.0°C / min, 3.5°C / min, 4.0°C / min, 4.5°C / min or 5.0°C / min.

[0075] In some embodiments, the first sintering time is 1 h to 10 h, for example, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h or 10 h.

[0076] In some embodiments, the first sintering atmosphere is an oxygen-containing atmosphere. Optionally, the oxygen volume content in the first sintering atmosphere is ≥ 70%.

[0077] In some embodiments, the temperature of the second sintering step is 600°C to 1000°C, for example, it can be 600°C, 640°C, 680°C, 720°C, 760°C, 800°C, 840°C, 880°C, 920°C, 960°C or 1000°C.

[0078] In some embodiments, the heating rate of the second sintering step is 1.0°C / min~5.0°C / min, for example, it can be 1.0°C / min, 1.5°C / min, 2.0°C / min, 2.5°C / min, 3.0°C / min, 3.5°C / min, 4.0°C / min, 4.5°C / min or 5.0°C / min.

[0079] In some embodiments, the second sintering time is 6 h to 20 h, for example, 6 h, 8 h, 10 h, 12 h, 14 h, 16 h, 18 h or 20 h.

[0080] In some embodiments, the atmosphere of the second sintering step is an oxygen-containing atmosphere. Optionally, the volume content of oxygen in the atmosphere of the second sintering step is ≥ 70%.

[0081] In some embodiments, the second sintering temperature is 150° C. to 500° C., for example, 150° C., 180° C., 210° C., 240° C., 270° C., 300° C., 330° C., 360° C., 390° C., 420° C., 450° C., 480° C. or 500° C. The second sintering temperature is selected as above in the present application to protect the oxygen vacancy defect metal oxide while ensuring the coating effect and reduce the recombination of the oxygen vacancy defect metal oxide.

[0082] In some embodiments, the heating rate of the second sintering is 1.0°C / min to 5.0°C / min, for example, 1.0°C / min, 1.5°C / min, 2.0°C / min, 2.5°C / min, 3.0°C / min, 3.5°C / min, 4.0°C / min, 4.5°C / min or 5.0°C / min.

[0083] In some embodiments, the second sintering time is 1 hour to 10 hours, for example, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours or 10 hours. The present application selects the second sintering time as above to effectively ensure the coating effect and avoid a large amount of lattice oxygen loss in the core caused by long-term sintering, resulting in irreversible phase change.

[0084] In some embodiments, the oxygen volume fraction in the atmosphere of the second sintering is 0% to 25%, for example, 0%, 2%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24% or 25%. Optionally, an oxygen-free atmosphere is used during the second sintering process.

[0085] The present application selects the volume fraction of oxygen in the second sintering as above. The low oxygen content in the atmosphere can protect the oxygen vacancies in the defective metal oxides. If the oxygen content is relatively high, it is easy to cause the defective metal oxides to oxidize, resulting in a large loss of oxygen vacancies in the defective metal oxides, affecting the coating effect.

[0086] Exemplarily, a method for preparing the above-mentioned positive electrode material is provided, comprising the following steps:

[0087] A lithium source and a cathode material precursor are mixed to obtain a mixture, wherein the molar ratio of the cathode material precursor to the lithium element in the lithium source is 1:(1.04-1.56), and the mixture is heated to 400-600°C at a heating rate of 1.0°C / min-5.0°C / min in an oxygen-containing atmosphere (oxygen volume content ≥21%), and sintered for 1h-10h; then, the mixture is heated to 600-1000°C at a heating rate of 1.0°C / min-5.0°C / min in an oxygen-containing atmosphere (oxygen volume content ≥21%), and sintered for 6h-20h to obtain a mixture containing a chemical formula of Li 1.2-m Ni 0.8+m-q-x Mn q Q x The core of the material of O2, wherein the Q element includes at least one of Co, Al and Zr, 0≤m≤0.2, 0.5≤q≤1, 0≤x≤0.3;

[0088] The inner core and an oxygen vacancy defect metal oxide are mixed, wherein the mass of the oxygen vacancy defect metal oxide is 500ppm~20000ppm of the mass of the inner core. In an atmosphere with an oxygen volume fraction of 0%~25%, the temperature is increased to 150℃~500℃ at a heating rate of 1.0℃ / min~5.0℃ / min. After sintering for 1h~10h, the oxygen vacancy defect metal oxide forms a coating layer on at least a portion of the surface of the inner core, thereby preparing the positive electrode material.

[0089] A third aspect of the present application provides a positive electrode plate, comprising at least one of the positive electrode material as described in the first aspect and the positive electrode material prepared by the preparation method as described in the second aspect.

[0090] The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material, a conductive agent and a binder. The positive electrode active material comprises at least one of the positive electrode material or the positive electrode material prepared by the preparation method, and the conductive agent and the binder may be conductive agents and binders commonly used in the technical field.

[0091] A fourth aspect of the present application provides a secondary battery, comprising the positive electrode sheet as described in the third aspect.

[0092] The above-mentioned secondary battery may, for example, include the above-mentioned positive electrode sheet, negative electrode sheet, electrolyte and diaphragm of the present application. The diaphragm is arranged between the positive electrode sheet and the negative electrode sheet, and mainly plays the role of preventing the positive and negative electrodes from short-circuiting, while allowing active ions to pass through. The electrolyte plays the role of conducting active ions between the positive electrode sheet and the negative electrode sheet. During the charging and discharging process of the secondary battery, the active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The present application has no special restrictions on the negative electrode sheet, electrolyte and diaphragm, and the negative electrode sheet, electrolyte and diaphragm prepared by the preparation method commonly used in the technical field, or the negative electrode sheet, electrolyte and diaphragm commonly used in the art can be used. Optionally, the above-mentioned secondary battery includes a lithium-ion battery.

[0093] Furthermore, another embodiment of the present application also provides an electrical device, including the above-mentioned battery of the present application.

[0094] The above-mentioned electrical devices may include any equipment or devices that use secondary batteries as driving sources, such as mobile phones, laptop computers, electric vehicles, ships, satellites, energy storage devices, smart home appliances, etc., but are not limited thereto.

[0095] The embodiments of the present application will be described in detail below in conjunction with examples. It should be understood that these examples are only used to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are preferably referred to the guidance provided in the present application, and can also be based on the experimental manual or normal conditions in this area, can also be based on the conditions recommended by the manufacturer, or refer to experimental methods known in the art.

[0096] Example 1

[0097] S1, 1000g of Ni 0.35 Mn 0.65 (OH)2 and 593g of LiOH were mixed to obtain a mixture, the mixture was heated to 500°C at a heating rate of 3.0°C / min in an air atmosphere, and sintered for 6h; then the mixture was heated to 900°C at a heating rate of 3.0°C / min in an air atmosphere, and sintered for 15h, and then the sintered product was crushed and passed through a 325-mesh sieve to obtain a mixture containing a chemical formula of Li 1.16 Ni 0.294 Mn 0.546 The core of the material of O2;

[0098] S2, weighing the core and oxygen vacancy defect metal oxide WO 2.72The mass of the oxygen vacancy defect metal oxide is 2000ppm of the mass of the core. The mixture is ball-milled at 25Hz for 5h in a nitrogen atmosphere. Then, the temperature is raised to 300℃ at a heating rate of 3.0℃ / min in a nitrogen atmosphere. After sintering for 5h, a coating layer is formed on the surface of the core. The sintered product is cooled in the furnace, crushed, and passed through a 325-mesh sieve to obtain the positive electrode material Li 1.16 Ni 0.294 Mn 0.546 O2@WO 2.72 , Figure 1 This is the SEM image of the positive electrode material.

[0099] Example 2

[0100] S1, 1000g of Ni 0.35 Mn 0.65 (OH)2 and 593g of LiOH were mixed to obtain a mixture, the mixture was heated to 500°C at a heating rate of 3.0°C / min in an air atmosphere, and sintered for 6h; then the mixture was heated to 900°C at a heating rate of 3.0°C / min in an air atmosphere, and sintered for 15h, and then the sintered product was crushed and passed through a 325-mesh sieve to obtain a mixture containing a chemical formula of Li 1.16 Ni 0.294 Mn 0.546 The core of the material of O2;

[0101] S2, weighing the core and oxygen vacancy defect metal oxide CeO 1.9 The mass of the oxygen vacancy defect metal oxide is 2500ppm of the mass of the core. After mixing in a nitrogen atmosphere, the temperature is raised to 300°C at a rate of 3.0°C / min. After sintering for 5 hours, a coating layer is formed on the surface of the core. The sintered product is cooled in the furnace, crushed, and passed through a 325-mesh sieve to prepare the positive electrode material Li 1.16 Ni 0.294 Mn 0.546 O2@CeO 1.9 .

[0102] Example 3

[0103] S1, 1000g of Ni 0.35 Mn 0.65 (OH)2 and 593g of LiOH were mixed to obtain a mixture, the mixture was heated to 500°C at a heating rate of 3.0°C / min in an air atmosphere, and sintered for 6h; then the mixture was heated to 900°C at a heating rate of 3.0°C / min in an air atmosphere, and sintered for 15h, and then the sintered product was crushed and passed through a 325-mesh sieve to obtain a mixture containing a chemical formula of Li 1.16 Ni 0.294 Mn 0.546 The core of the material of O2;

[0104] S2, weigh the core and oxygen vacancy defect metal oxide LLZO (La3Li7Zr2O 12 ), the mass of the oxygen vacancy defect metal oxide is 3000ppm of the mass of the core, and the mixture is ball-milled at 25Hz for 5h in an argon atmosphere, and then heated to 400℃ at a heating rate of 3.0℃ / min in an argon atmosphere, and a coating layer is formed on the surface of the core after sintering for 5h. The sintered product is cooled in the furnace, crushed, and passed through a 325-mesh sieve to obtain the positive electrode material Li 1.16 Ni 0.294 Mn 0.546 O2@LLZO.

[0105] Example 4

[0106] The positive electrode material is prepared according to the method of Example 1, except that the sintering temperature in step S2 is 550°C.

[0107] Example 5

[0108] The positive electrode material is prepared according to the method of Example 1, except that the volume fraction of oxygen in the sintering atmosphere in step S2 is 25%.

[0109] Example 6

[0110] The positive electrode material is prepared according to the method of Example 1, except that the volume fraction of oxygen in the sintering atmosphere in step S2 is 35%.

[0111] Comparative Example 1

[0112] The positive electrode material was prepared according to the method of Example 1, except that WO 2.72 Replace with an equal mass of WO3.

[0113] Comparative Example 2

[0114] Directly adopt the Li prepared in step S1 of Example 1 1.16 Ni 0.294 Mn 0.546 As positive electrode material.

[0115] The components of the positive electrode materials prepared in each embodiment and each comparative example were measured using an ICP-OES (inductively coupled plasma atomic emission spectrometer).

[0116] XPS characterization was performed on the positive electrode materials and oxygen vacancy defect metal oxides prepared in each embodiment and each comparative example, and the O v1 / (O v1 +O L1 ) and O L1 / (O v1 +O L1), and O in oxygen vacancy defect metal oxides v2 / (O v2 +O L2 ), the test results of the median lattice oxygen binding energy and the median oxygen vacancy binding energy are shown in Table 1. v1 / (O v1 +O L1 ), O L1 / (O v1 +O L1 ) and O v2 / (O v2 +O L2 ) are shown in Table 2. The test results of Example 1, Comparative Example 2 and WO 2.72 The XPS test spectrum is as follows Figure 2 shown.

[0117] Table 1

[0118]

[0119] Table 2

[0120]

[0121] Note: In Tables 1 and 2, the metal oxide used in Comparative Example 1 has no oxygen vacancy defect value, and Comparative Example 2 is not coated, so there is no test result, which is represented by “ / ”.

[0122] The positive electrode materials prepared in the above examples and comparative examples are assembled into a battery, specifically comprising:

[0123] The specific preparation process is as follows: the positive electrode material, acetylene black conductive agent, and polyvinylidene fluoride binder are mixed uniformly in a mass ratio of 8:1:1, and an appropriate amount of N-methylpyrrolidone is added as a dispersant to mix and slurry; then the obtained slurry is evenly coated on the copper foil, vacuum dried at 120°C for 12h, and then cut into discs as positive electrode sheets, and the active material loading is 10mg / cm 2 ;

[0124] In a glove box with an argon atmosphere (oxygen content ≤ 0.1 ppm, water content ≤ 0.1 ppm), a button half-cell was assembled; the above-mentioned positive electrode sheet, negative metal lithium sheet, and electrolyte lithium hexafluorophosphate (dissolved in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1) were assembled into a CR2032 button cell to obtain a button half-cell for testing.

[0125] The electrochemical performance of the battery prepared above is tested, and the testing method includes:

[0126] Discharge specific capacity and first effect test: the test conditions are 0.1C, 2.8V~4.6V.

[0127] Cycle retention rate test: Test conditions are 0.33C, 2.8V~4.6V.

[0128] The test results are shown in Table 3.

[0129] Table 3

[0130]

[0131] From Table 1 and Table 2, we can see that:

[0132] (1) Compared with Example 4, it can be seen that the present application adjusts the coating temperature of the oxygen vacancy defect metal oxide to inhibit surface reconstruction and thus avoid the deterioration of the first effect and cycle performance.

[0133] (2) Compared with Examples 5-6, it can be seen that the present application adjusts the oxygen content of the atmosphere during the coating process, which can protect the oxygen vacancies in the coating layer, enhance the lithium ion kinetics, and improve the first effect and cycle.

[0134] (3) Compared with Comparative Examples 1-2, it can be seen that the positive electrode material of the present application forms a coating layer containing oxygen vacancy defect metal oxide on the surface of the inner core, which can inherit the oxygen vacancies in the oxygen vacancy defect metal oxide to the inner core surface, which is more conducive to increasing the oxygen vacancy content on the inner core surface, thereby solving the problem of oxygen loss in the inner core, while retaining the integrity of the oxygen skeleton inside the lattice, while retaining the anion redox capacity, improving the cycle performance and storage performance. Moreover, the introduction of oxygen vacancies can also reduce the lithium ion diffusion energy barrier, increase the lithium ion diffusion rate, and then promote the lithium ion kinetic process, improve the first efficiency and cycle performance. In addition, the surface of the positive electrode material of the present application has additional oxygen vacancies, which can improve the material stability, help to suppress the gas production during the formation, and also improve the cycle stability of the positive electrode material, suppress the occurrence of side reactions, and help to improve the cycle performance. The positive electrode material of the present application has the characteristics of high first efficiency, low gas production, high lithium ion kinetics and high cycle retention rate.

[0135] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0136] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the application. It should be noted that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.

Claims

1. A positive electrode material, characterized in that: The positive electrode material comprises a core and a coating layer coated on at least a portion of the surface of the core; the core comprises a chemical formula of Li 1.2-m Ni 0.8+m-q-x Mn q Q x O2 material, wherein the Q element includes at least one of Co, Al and Zr, 0≤m≤0.2, 0.5≤q≤1, 0≤x≤0.3; the material of the coating layer includes oxygen vacancy defect metal oxide.

2. The positive electrode material according to claim 1, characterized in that The positive electrode material satisfies at least one of the following conditions: (1) The positive electrode material meets the following requirements: 25% ≤ O v1 / (O v1 +O L1 )≤50%, where O v1 is the peak area of ​​the characteristic peak where the oxygen vacancy is located in the O1s orbital fine spectrum in the XPS test spectrum of the positive electrode material; L1 The peak area of ​​the characteristic peak of lattice oxygen in the O1s orbital fine spectrum in the XPS test spectrum of the positive electrode material; (2) The median binding energy of oxygen vacancies in the positive electrode material after charge correction is higher than the binding energy of the characteristic peak of lattice oxygen in the positive electrode material; optionally, the median binding energy of oxygen vacancies in the positive electrode material after charge correction is 531 eV~534 eV, and the median binding energy of lattice oxygen is 528 eV~531 eV.

3. The positive electrode material according to claim 1, characterized in that The oxygen vacancy defect metal oxide satisfies at least one of the following conditions: (1) The oxygen vacancy defect metal oxide satisfies: 10%≤O v2 / (O v2 +O L2 )≤50%, where O v2 is the peak area of ​​the characteristic peak where the oxygen vacancy is located in the O1s orbital fine spectrum in the XPS test spectrum of the oxygen vacancy defect metal oxide; L2 is the peak area of ​​the characteristic peak of lattice oxygen in the O1s orbital fine spectrum in the XPS test spectrum of the oxygen vacancy defect metal oxide; (2) The median value of the oxygen vacancy binding energy of the oxygen vacancy defect metal oxide after charge correction is higher than the binding energy of the characteristic peak of lattice oxygen of the oxygen vacancy defect metal oxide; optionally, the median value of the oxygen vacancy binding energy of the oxygen vacancy defect metal oxide after charge correction is 531eV~534eV, and the median value of the lattice oxygen binding energy is 528eV~531eV.

4. The positive electrode material according to claim 1, characterized in that The positive electrode material also satisfies at least one of the following conditions: (1) The crystal structure of the core includes a layered α-NaFeO2 structure; optionally, the core has a characteristic diffraction peak of Li2MnO3 in the range of 20° to 30°; (2) The metal element in the oxygen vacancy defect metal oxide includes at least one of Ni, Co, Mn, Ti, Al, W, V, Mo, Ce, Fe, Cr, La and Zr; optionally, the metal element in the oxygen vacancy defect metal oxide includes at least one of Ti, W, Ce and La.

5. The positive electrode material according to claim 1, characterized in that The positive electrode material also satisfies at least one of the following conditions: (1) The mass proportion of the coating layer in the positive electrode material is 500ppm~20000ppm; (2) The volume median particle size Dv50 of the positive electrode material is 2 μm to 15 μm; (3) The positive electrode material includes secondary particles formed by aggregation of primary particles, and the volume median particle size Dv50 of the primary particles is 100 nm to 500 nm.

6. The positive electrode material according to any one of claims 1 to 5, characterized in that The positive electrode material further includes a doping layer, wherein the doping layer is located between the core and the coating layer, and the doping layer includes a chemical formula of Li 1.2-m Ni 0.8+m-q-x- y Mn q Q x M y O2 material, M element includes the metal element contained in the oxygen vacancy defect metal oxide, 0<y≤0.01; Optionally, the mass proportion of the doping layer in the positive electrode material is 500ppm~5000ppm.

7. A method for preparing a positive electrode material, characterized in that: The preparation method of the positive electrode material comprises: A lithium source and a positive electrode material precursor are mixed to obtain a mixture, and the mixture is subjected to a first sintering to obtain a mixture containing a chemical formula of Li 1.2-m Ni 0.8+m-q-x Mn q Q x The core of the material of O2, wherein the Q element includes at least one of Co, Al and Zr, 0≤m≤0.2, 0.5≤q≤1, 0≤x≤0.3; The inner core and the oxygen vacancy defect metal oxide are mixed, and after a second sintering, a coating layer containing the oxygen vacancy defect metal oxide is formed on at least a portion of the surface of the inner core to prepare the positive electrode material.

8. The preparation method according to claim 7, characterized in that: The preparation method satisfies at least one of the following conditions: (1) The first sintering comprises: performing a first sintering step and a second sintering step on the mixture in sequence; Optionally, the first step of sintering is performed at a temperature of 400°C to 600°C, a heating rate of 1.0°C / min to 5.0°C / min, a time of 1h to 10h, and an oxygen-containing atmosphere; Optionally, the second step sintering temperature is 600°C to 1000°C, the heating rate is 1.0°C / min to 5.0°C / min, the time is 6h to 20h, and the atmosphere is an oxygen-containing atmosphere; (2) The temperature of the second sintering is 150°C~500°C, the heating rate is 1.0°C / min~5.0°C / min, the time is 1h~10h, and the volume fraction of oxygen in the sintering atmosphere is 0%~25%.

9. A positive electrode sheet, characterized in that: The invention comprises at least one of the positive electrode material described in any one of claims 1 to 6 and the positive electrode material prepared by the preparation method described in claim 7 or 8.

10. A secondary battery, characterized in that: Including the positive electrode sheet as described in claim 9.

Citation Information

Cited By

  • Positive plate as well as electrochemical device and electronic equipment comprising positive plate

    CN119742319A

  • Positive electrode sheet, and electrochemical device and electronic device containing same

    CN119742319B

  • Lithium-ion battery, positive electrode active material and preparation method therefor, and electric device

    WO2026157921A1