Positive electrode material, positive electrode plate, sodium ion battery and preparation method and application of sodium ion battery
By using a positive electrode material with the chemical formula of NanMn1-x-y-zMxZnyLizO2 in sodium ion batteries, a stable O3-phase structure is formed by doping active and inactive elements, the O3-type layered transition metal oxide in sodium ion batteries is solved. In the 2-4V voltage range, the balance between high capacity and long cycle life is achieved.
Patent Information
- Application Number
- CN202311344550.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-17
- Publication Date
- 2024-11-08
AI Technical Summary
In sodium ion batteries, the O3 layered transition metal oxide positive electrode material has a low content in the voltage range of 2 to 4V and has poor cycle stability, making it difficult to have high capacity and long cycle life within this voltage range.
Using the positive electrode material with the chemical formula NanMn1-x-y-zMxZnyLizO2, M is at least one of Cu2+, Ni2+, Cr2+, Fe3+ and Co2+, by doping the active element and the inactive elements Li and Zn on the Mn side. , forming an O3 phase structure to ensure that the Zn element is at point Wyckoff 3b and the Li element is at point Wyckoff 4c, and the orderly distribution is achieved to stabilize the lattice and suppress unfavorable phase transition and oxygen evolution.
The capacity and cycle stability of the positive electrode material in the voltage range of 2 to 4V are improved, high specific capacity and long cycle life are ensured, and cost is reduced.
Smart Images

Figure CN118919709A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of methods or devices for directly converting chemical energy into electrical energy, and more specifically, to a positive electrode material, a positive electrode sheet, a sodium ion battery, and a preparation method and application thereof. Background Art
[0002] With the rapid advancement of automobile electrification, the huge demand for lithium-ion power batteries has led to an imbalance in the supply and demand of lithium resources and high prices. On the other hand, there is an urgent need to develop sustainable energy sources such as photovoltaics and wind power. In order to reduce the phenomenon of wind and light abandonment, it is urgent to configure energy storage batteries. Given that lithium-ion batteries currently dominate energy storage batteries, the rapid development of the energy storage industry has further aggravated the consumption of lithium resources. Therefore, it is imperative to develop new energy storage batteries based on non-lithium-ion batteries.
[0003] Compared with lithium-ion batteries, sodium-ion batteries have the advantages of low cost, abundant resources, good safety, and environmental friendliness, and are more suitable for large-scale energy storage. For sodium-ion batteries, the key factor restricting their performance is the positive electrode material. At present, the substances suitable for positive electrode materials of sodium-ion batteries mainly include oxides, fluorides, sulfides, phosphates and pyrophosphates, among which layered transition metal oxides have the advantages of high capacity, good rate performance, and long cycle life, and are more suitable for positive electrode materials of sodium-ion batteries.
[0004] Layered transition metal oxide materials can be divided into P2 type and O3 type according to their crystal structure. Compared with P2 type, O3 type layered transition metal oxides can store more Na + , has a higher reversible specific capacity within the same voltage range, that is, its capacity can be increased by increasing the charge and discharge voltage; but in the existing electrolyte system, when the charge and discharge voltage of O3-type layered transition metal oxide reaches 4.1V or above, the high voltage will not only decompose the electrolyte, but also cause the layered transition metal oxide to easily undergo irreversible phase transformation, causing lattice distortion and lattice oxygen loss, thereby causing its reversible specific capacity to decay rapidly and the cycle life to be significantly reduced; although the structural distortion of the positive electrode material can be suppressed to a certain extent by reducing the charge and discharge voltage (reducing the voltage range to 2-4V) to improve its cycle stability, the capacity of the positive electrode material within this voltage range is difficult to exceed 145mAh / g. Therefore, there is an urgent need for a positive electrode material with both high capacity and cycle stability within a voltage of 2-4V. Summary of the invention
[0005] The present invention aims to overcome the defects and shortcomings of existing sodium ion battery layered transition metal oxide positive electrode materials, such as low capacity and poor cycle stability within a voltage range of 2 to 4V, and to provide a positive electrode material.
[0006] Another object of the present invention is to provide a method for preparing a positive electrode material.
[0007] Another object of the present invention is to provide an application of a positive electrode material in a sodium ion battery.
[0008] Another object of the present invention is to provide a positive electrode sheet comprising the positive electrode material.
[0009] Another object of the present invention is to provide a sodium ion battery comprising the above-mentioned positive electrode material.
[0010] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0011] The present invention protects a positive electrode material, which is in an O3 phase (a crystal structure of face-centered cubic stacking) and has a chemical formula of Na n Mn 1-x-y-z M x Zn y Li z O 2 ; M is Cu 2+ 、Ni 2+ Cr 2+ , Fe 3+ and Co 2+ At least one of;
[0012] Among them, 0.5≤x≤0.6, 0.05≤y≤0.1, 0.005≤z≤0.05, 0.9≤n≤1.1, and x, y, z, n satisfy the principle of electrical neutrality in terms of numerical value;
[0013] The Na n Mn 1-x-y-z M x Zn y Li z O 2 All Zn elements in 2+ Located at Wyckoff 3b point, all Li elements are Li + Located at Wyckoff 4c point.
[0014] The positive electrode material of the present invention is in O3 phase, and the core material uses Mn as the basic framework. The capacity is provided by doping the active element M on the Mn side. The synergistic doping of the inactive elements Li and Zn and their coupling effect promote the oxidation / reduction reaction of the active element, thereby improving the capacity of the positive electrode material and inhibiting the adverse phase change during the charge and discharge process, thereby achieving a good balance between the capacity and cycle life of the positive electrode material.
[0015] Li and Zn in the positive electrode material of the present invention are inactive elements and play a supporting role. + and Zn2+ Orderly distribution and coordinated doping can stabilize the lattice and inhibit oxygen evolution, and in turn promote the random distribution of Mn / M elements, thereby improving the oxidation / reduction reaction of M and inhibiting unfavorable phase transitions. The lack of any doping is not conducive to the improvement of the overall performance of the positive electrode material. 2+ Co-doping and Li + and Zn 2+ Orderly distribution makes Li + Located at Wyckoff 4c point, in LiO 4 Li in tetrahedron + Not easy to diffuse to Na + , which can effectively inhibit the MnO 6 / MO 6 A distorted, stable lattice of an octahedron.
[0016] It should also be noted that the above-mentioned M elements will change valence during the charging and discharging process, that is, Cu is +2 or +3, Ni is +2, +3 or +4, Cr is +2 or +3, Fe is +2 or +3, and Co is +2 or +3; Na and Li are both +1, and Mn is +4.
[0017] Specifically, the Na n Mn 1-x-y-z M x Zn y Li z O 2 The Zn and Li elements in the lattice are distributed in an orderly and gradient manner, and their content in the lattice gradually decreases from the outside to the inside.
[0018] The study found that when Zn is not added or Li + and Zn 2+ Random distribution (i.e. not all Zn elements are in the form of Zn 2+ Located at the Wyckoff 3b point, not all Li elements are Li + At Wyckoff 4c, Li + Located in LiO 6 The 3b position of the octahedron is not conducive to stabilizing the surface lattice (especially when charged to a high voltage); while the gradient doping of Li and Zn can be beneficial to stabilizing the surface lattice, effectively inhibiting lattice distortion and oxygen evolution, and effectively inhibiting the corrosion of the positive electrode material by the electrolyte, thereby making the positive electrode material have a high specific capacity and a long cycle life, and the gradient doping is also beneficial to reducing costs.
[0019] Specifically, the Na n Mn 1-x-y-z M x Zn y Li z O2 The Mn and M elements in the lattice are randomly distributed. When Mn and M are arranged in order, it is not conducive to stabilizing the lattice and will inhibit the gradient doping and orderly distribution of Li and Zn.
[0020] Preferably, the positive electrode material is a single crystal structure, and the particle size D50 is 4 to 8 μm.
[0021] Preferably, the M is Cu 2+ 、Ni 2+ Cr 2+ , Fe 3+ and Co 2+ More preferably, M is Cu 2+ 、Ni 2+ Cr 2+ , Fe 3+ and Co 2+ At least two of them and one of them is Ni, and the molar ratio of Ni to (M+Mn) is (0.23-0.29):1.
[0022] Cu, Ni, Cr, Fe, and Co are electrochemically active elements that can provide capacity by changing valence. When M is a combination of multiple elements (≥2) mentioned above, their successive oxidation / reduction reactions can effectively inhibit adverse phase changes and promote each other's oxidation / reduction reactions, thereby providing capacity and increasing the structural stability of the positive electrode material, inhibiting adverse phase changes and Jahn-Teller distortion during charge and discharge, and improving the cycle stability of the positive electrode material.
[0023] The present invention also protects a method for preparing the above-mentioned positive electrode material, comprising the following steps:
[0024] S1. mixing and co-precipitating a manganese-containing compound and a compound containing an M element to obtain a precursor;
[0025] S2. The precursor in S1 is mixed evenly with a sodium-containing compound, a lithium-containing compound and a zinc-containing compound, and subjected to a high-temperature solid-phase reaction to obtain a positive electrode material;
[0026] Wherein, the M element in S1 is at least one of Cu, Ni, Cr, Fe and Co.
[0027] Specifically, the temperature of the high temperature solid phase reaction is 650-1000°C, and the time is 10-20 hours. Optionally, the temperature of the high temperature solid phase reaction is 900-1000°C, preferably 900-930°C.
[0028] Optionally, the precursor is at least one of hydroxide, carbonate and oxalate.
[0029] Optionally, the sodium-containing compound is at least one of sodium carbonate, sodium acetate and sodium oxalate; the zinc-containing compound is at least one of zinc acetate, zinc oxalate, zinc carbonate and zinc oxide; the lithium-containing compound is at least one of lithium acetate, lithium oxalate, lithium carbonate and lithium hydroxide.
[0030] The use of the above-mentioned positive electrode material in a sodium ion battery is also within the protection scope of the present invention.
[0031] The present invention also protects a positive electrode sheet, comprising a current collector and a positive electrode active material layer disposed on at least one side of the current collector, wherein the positive electrode active material layer comprises the positive electrode material.
[0032] The present invention also protects a sodium ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator located between the positive electrode sheet and the negative electrode sheet, and an electrolyte, wherein the positive electrode sheet comprises the above-mentioned positive electrode material.
[0033] Compared with the prior art, the present invention has the following beneficial technical effects:
[0034] The positive electrode material of the present invention is in O3 phase, the core material uses Mn as the basic framework, and the capacity is provided by doping the active element M on the Mn side, while Li and Zn are orderly distributed in the lattice, and the synergistic doping of the inactive elements Li and Zn and their coupling effect are utilized to promote the oxidation / reduction reaction of the active element M, inhibit the adverse phase change during the charge and discharge process, thereby improving the capacity and cycle stability of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is the XRD diagram of the positive electrode material in Example 1.
[0036] Figure 2 This is the SEM image of the positive electrode material in Example 1.
[0037] Figure 3 This is a charge and discharge curve diagram of the positive electrode material in Example 1.
[0038] Figure 4 This is a cycle life diagram of the positive electrode material in Example 1.
[0039] Figure 5 This is the charge and discharge curve of the positive electrode material in Comparative Example 1.
[0040] Figure 6 This is the charge and discharge curve of the positive electrode material in Comparative Example 2. DETAILED DESCRIPTION
[0041] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0042] Example 1
[0043] A positive electrode material with the chemical formula Na 0.93 [Mn 0.40 Fe 0.28 Ni 0.24 Zn 0.07 Li 0.01 ]O 2 .
[0044] The above positive electrode material can be prepared by the following preparation method:
[0045] S1. According to the stoichiometric ratio of the positive electrode material, Mn was prepared by coprecipitation method. 0.40 Fe 0.28 Ni 0.24 (OH) 1.84 Precursor;
[0046] S2. Add Mn in S1 0.40 Fe 0.28 Ni 0.24 (OH) 1.84 Precursor (Mn in the precursor is +2) and Na 2 CO 3 , Li 2 CO 3 The mixture was ball-milled with ZnO to obtain Na 0.93 [Mn 0.40 Fe 0.28 Ni 0.24 Zn 0.07 Li 0.01 ]O 2 .
[0047] The above positive electrode material was tested and the obtained XRD spectrum was as follows Figure 1 As shown, it can be seen that the positive electrode material is in O3 phase, and the XRD spectrum analysis confirms that Zn 2+ All located at Wyckoff 3b point, Li + All are located at the Wyckoff 4c point; at the same time, through SEM analysis, it can be found that the particle size D50 of the positive electrode material is 4 to 8 μm (such as Figure 2 As shown), the cross section (section) of the above-mentioned positive electrode material was subjected to energy spectrum line scanning and surface scanning analysis, and it was found that Mn, Fe, and Ni were randomly distributed in the lattice, and the content of Li and Zn in the lattice gradually decreased from the outside to the inside, showing an orderly, gradient distribution.
[0048] Example 2
[0049] A positive electrode material with the chemical formula Na 0.94 [Mn 0.40 Fe 0.28 Ni 0.24 Zn 0.06 Li 0.02 ]O 2 .
[0050] The above positive electrode material can be prepared by the following preparation method:
[0051] S1. According to the stoichiometric ratio of the positive electrode material, Mn was prepared by coprecipitation method. 0.40 Fe 0.28 Ni 0.24 (OH) 1.84 Precursor;
[0052] S2. Add Mn in S1 0.40 Fe 0.28 Ni 0.24 (OH) 1.84 The precursor was mixed with sodium acetate, lithium acetate and ZnO by ball milling (ball milling speed was 350 rpm / min, ball milling time was 15 h), and then calcined at 930 ° C for 15 h in air atmosphere to obtain Na 0.94 [Mn 0.40 Fe 0.28 Ni 0.24 Zn 0.06 Li 0.02 ]O 2 .
[0053] After testing, the properties of the positive electrode material are similar to those of the positive electrode material in Example 1, presenting an O3 phase with a particle size D50 of 4 to 8 μm; and the XRD spectrum analysis determined that Zn 2+ All located at Wyckoff 3b point, Li + All of them are located at the Wyckoff 4c point; the cross-section of the above-mentioned positive electrode material is subjected to energy spectrum line scanning and surface scanning analysis, Mn, Fe, and Ni are randomly distributed in the lattice, and the content of Li and Zn in the lattice gradually decreases from the outside to the inside, showing an orderly, gradient distribution.
[0054] Example 3
[0055] A positive electrode material with the chemical formula Na 0.95 [Mn 0.39 Fe 0.28 Ni 0.25 Zn 0.07 Li 0.01 ]O 2 .
[0056] The above positive electrode material can be prepared by the following preparation method:
[0057] S1. According to the stoichiometric ratio of the positive electrode material, Mn was prepared by coprecipitation method. 0.39 Fe 0.28 Ni 0.25 (CO 3 ) 0.92 Precursor;
[0058] S2. Add Mn in S1 0.39 Fe 0.28 Ni 0.25 (CO 3 ) 0.92 Precursor and sodium oxalate, Li 2 CO 3 The mixture was mixed with zinc acetate by ball milling (the ball milling speed was 350 rpm / min and the ball milling time was 15 h), and then calcined at 930 ° C for 15 h in an air atmosphere to obtain Na 0.95 [Mn 0.39 Fe 0.28 Ni 0.25 Zn 0.07 Li 0.01 ]O 2 .
[0059] After testing, the properties of the positive electrode material are similar to those of the positive electrode material in Example 1, presenting an O3 phase with a particle size D50 of 4 to 8 μm; and the XRD spectrum analysis determined that Zn 2+ All located at Wyckoff 3b point, Li + All of them are located at the Wyckoff 4c point; the cross-section of the above-mentioned positive electrode material is subjected to energy spectrum line scanning and surface scanning analysis, Mn, Fe, and Ni are randomly distributed in the lattice, and the content of Li and Zn in the lattice gradually decreases from the outside to the inside, showing an orderly, gradient distribution.
[0060] Example 4
[0061] A positive electrode material with the chemical formula Na 0.93 [Mn 0.39 Fe 0.30 Ni 0.23 Zn 0.07 Li 0.01 ]O 2 .
[0062] The above positive electrode material can be prepared by the following preparation method:
[0063] S1. According to the stoichiometric ratio of the positive electrode material, Mn was prepared by coprecipitation method. 0.39 Fe 0.30 Ni 0.23 (C2 O 4 ) 0.92 Precursor;
[0064] S2. Add Mn in S1 0.39 Fe 0.30 Ni 0.23 (C 2 O 4 ) 0.92 Precursor and Na 2 CO 3 , Li 2 CO 3 The mixture was mixed with zinc acetate by ball milling (the ball milling speed was 350 rpm / min and the ball milling time was 15 h), and then calcined at 930 ° C for 15 h in an air atmosphere to obtain Na 0.93 [Mn 0.39 Fe 0.30 Ni 0.23 Zn 0.07 Li 0.01 ]O 2 .
[0065] After testing, the properties of the positive electrode material are similar to those of the positive electrode material in Example 1, presenting an O3 phase with a particle size D50 of 4 to 8 μm; and the XRD spectrum analysis determined that Zn 2+ All located at Wyckoff 3b point, Li + All of them are located at the Wyckoff 4c point; the cross-section of the above-mentioned positive electrode material is subjected to energy spectrum line scanning and surface scanning analysis, Mn, Fe, and Ni are randomly distributed in the lattice, and the content of Li and Zn in the lattice gradually decreases from the outside to the inside, showing an orderly, gradient distribution.
[0066] Example 5
[0067] A positive electrode material with the chemical formula Na 0.95 [Mn 0.39 Fe 0.28 Cu 0.01 Ni 0.24 Zn 0.07 Li 0.01 ]O 2 .
[0068] The above positive electrode material can be prepared by the following preparation method:
[0069] S1. According to the stoichiometric ratio of the positive electrode material, Mn was obtained by coprecipitation method. 0.39 Fe 0.28 Cu 0.01 Ni 0.24 (OH) 1.84 Precursor;
[0070] S2. Add Mn in S1 0.39 Fe 0.28 Cu 0.01 Ni 0.24 (OH) 1.84 Precursor and Na 2 CO 3 , Li 2 CO 3 The mixture was mixed with zinc acetate by ball milling (the ball milling speed was 350 rpm / min and the ball milling time was 15 h), and then calcined at 930 ° C for 15 h in an air atmosphere to obtain Na 0.95 [Mn 0.39 Fe 0.28 Cu 0.01 Ni 0.24 Zn 0.07 Li 0.01 ]O 2 .
[0071] After testing, the properties of the positive electrode material are similar to those of the positive electrode material in Example 1, presenting an O3 phase with a particle size D50 of 4 to 8 μm; and the XRD spectrum analysis determined that Zn 2+ All located at Wyckoff 3b point, Li + All of them are located at the Wyckoff 4c point; the cross-section of the above-mentioned positive electrode material is subjected to energy spectrum line scanning and surface scanning analysis, Mn, Fe, and Ni are randomly distributed in the lattice, and the content of Li and Zn in the lattice gradually decreases from the outside to the inside, showing an orderly, gradient distribution.
[0072] Example 6
[0073] A positive electrode material with the chemical formula Na 0.95 [Mn 0.39 Fe 0.27 Co 0.01 Ni 0.25 Zn 0.07 Li 0.01 ]O 2 .
[0074] The above positive electrode material can be prepared by the following preparation method:
[0075] S1. According to the stoichiometric ratio of the positive electrode material, Mn was prepared by coprecipitation method. 0.39 Fe 0.27 Co 0.01 Ni 0.25 (CO 3 ) 0.92 Precursor;
[0076] S2. Add Mn in S1 0.39 Fe0.27 Co 0.01 Ni 0.25 (CO 3 ) 0.92 Precursor and Na 2 CO 3 , Li 2 CO 3 The mixture was mixed with zinc acetate by ball milling (the ball milling speed was 350 rpm / min and the ball milling time was 15 h), and then calcined at 930 ° C for 15 h in an air atmosphere to obtain Na 0.95 [Mn 0.39 Fe 0.27 Co 0.01 Ni 0.25 Zn 0.07 Li 0.01 ]O 2 .
[0077] After testing, the properties of the positive electrode material are similar to those of the positive electrode material in Example 1, presenting an O3 phase with a particle size D50 of 4 to 8 μm; and the XRD spectrum analysis determined that Zn 2+ All located at Wyckoff 3b point, Li + All of them are located at the Wyckoff 4c point; the cross-section of the above-mentioned positive electrode material is subjected to energy spectrum line scanning and surface scanning analysis, Mn, Fe, and Ni are randomly distributed in the lattice, and the content of Li and Zn in the lattice gradually decreases from the outside to the inside, showing an orderly, gradient distribution.
[0078] Comparative Example 1
[0079] A positive electrode material having the chemical formula Na[Mn 0.40 Fe 0.28 Ni 0.24 Li 0.08 ]O 2 .
[0080] The above positive electrode material can be prepared by the following preparation method:
[0081] S1. According to the stoichiometric ratio of the positive electrode material, Mn was prepared by coprecipitation method. 0.40 Fe 0.28 Ni 0.24 (OH) 1.84 Precursor;
[0082] S2. Add Mn in S1 0.40 Fe 0.28 Ni 0.24 (OH) 1.84 Precursor and Na 2 CO 3 and Li 2 CO3 The mixture was mixed by ball milling (the ball milling speed was 350 rpm / min and the ball milling time was 15 h), and then calcined at 930 °C for 15 h in an air atmosphere to obtain Na[Mn 0.40 Fe 0.28 Ni 0.24 Li 0.08 ]O 2 .
[0083] The above positive electrode material is not doped with Zn, and Zn is partially replaced by Li. According to XRD spectrum analysis, Li + Located at Wyckoff 3b point.
[0084] Comparative Example 2
[0085] A positive electrode material with the chemical formula Na 0.92 [Mn 0.40 Fe 0.28 Ni 0.24 Zn 0.08 ]O 2 .
[0086] The above positive electrode material can be prepared by the following preparation method:
[0087] S1. According to the stoichiometric ratio of the positive electrode material, Mn was prepared by coprecipitation method. 0.40 Fe 0.28 Ni 0.24 (OH) 1.84 Precursor;
[0088] S2. Add Mn in S1 0.40 Fe 0.28 Ni 0.24 (OH) 1.84 Precursor and Na 2 CO 3 The mixture was ball-milled with ZnO to obtain Na 0.92 [Mn 0.40 Fe 0.28 Ni 0.24 Zn 0.08 ]O 2 .
[0089] The above positive electrode material is not doped with Li, and a portion of Li is replaced by Zn.
[0090] Comparative Example 3
[0091] A positive electrode material with the chemical formula Na 0.99 [Mn 0.51 Ni 0.41Zn 0.07 Li 0.01 ]O 2 .
[0092] The preparation method of the above positive electrode material is the same as that of Example 1. The positive electrode material is not doped with Fe, and the Fe part is replaced by Ni and Mn. The energy spectrum line scanning and surface scanning analysis of the cross section (cross section) of the positive electrode material show that the distribution of Ni and Mn elements is locally ordered.
[0093] Comparative Example 4
[0094] A positive electrode material with the chemical formula Na 0.93 [Mn 0.40 Fe 0.28 Ni 0.24 Mg 0.07 Li 0.01 ]O 2 .
[0095] The preparation method of the above positive electrode material is the same as that of Example 1. The positive electrode material is not doped with Zn, and Zn is partially replaced by Mg. The cross-section (cross section) of the positive electrode material is subjected to energy spectrum line scanning and surface scanning analysis. The content of Li and Mg in the lattice gradually decreases from the outside to the inside, showing a random, gradient distribution. According to XRD spectrum analysis, Mg 2+ Located at Wyckoff 3b, Li + Located at Wyckoff 3b point.
[0096] Comparative Example 5
[0097] A positive electrode material with the chemical formula Na 0.93 [Mn 0.40 Fe 0.28 Ni 0.24 Zn 0.07 K 0.01 ]O 2 .
[0098] The preparation method of the positive electrode material is the same as that of Example 1. The positive electrode material is not doped with Li, and Li is partially replaced by K. The cross-section (cross section) of the positive electrode material is subjected to energy spectrum line scanning and surface scanning analysis. The content of K and Zn in the lattice is uniformly distributed and randomly distributed. The XRD spectrum analysis shows that Zn 2+ Located at Wyckoff 3b point, K + Located at Wyckoff 3b point.
[0099] Comparative Example 6
[0100] A positive electrode material with the chemical formula Na 0.90 [Mn 0.40 Fe 0.28 Cu 0.24Zn 0.07 Li 0.01 ]O 2 .
[0101] The preparation method of the above positive electrode material is the same as that of Example 1. The positive electrode material is not doped with Ni, and Ni is partially replaced by Cu. The cross-section (cross section) of the positive electrode material is subjected to energy spectrum line scanning and surface scanning analysis, and the distribution of Cu, Fe, and Mn elements is locally orderly; the XRD spectrum analysis shows that Zn 2+ All located at Wyckoff 3b point, Li + Part of it is located at Wyckoff 3b point.
[0102] Comparative Example 7
[0103] A positive electrode material with the chemical formula Na 0.96 [Mn 0.40 Fe 0.28 Ni 0.19 Zn 0.09 Li 0.04 ]O 2 .
[0104] The preparation method of the above positive electrode material is the same as that of Example 1. Compared with the positive electrode material in Example 1, the ratio of Zn to Li is increased and the ratio of Ni is reduced. According to XRD spectrum analysis, Li + Not all of them are located at Wyckoff 4c point, and some of them are located at Wyckoff 3b point.
[0105] Comparative Example 8
[0106] A positive electrode material with the chemical formula Na 0.93 [Mn 0.40 Fe 0.28 Ni 0.24 Zn 0.07 Li 0.01 ]O 2 .
[0107] The above positive electrode material can be prepared by the following preparation method:
[0108] According to the stoichiometric ratio of the positive electrode material, Na 2 CO 3 , Mn 3 O 4 , Fe 2 O 3 , NiO, ZnO and Li 2 CO 3 The mixture was evenly mixed by ball milling (the ball milling speed was 350 rpm / min and the ball milling time was 15 h), and then calcined at 930 ° C for 15 h in an air atmosphere to obtain Na0.93 [Mn 0.40 Fe 0.28 Ni 0.24 Zn 0.07 Li 0.01 ]O 2 .
[0109] Through the XRD pattern analysis of the above positive electrode materials, it was determined that Zn 2+ Located at Wyckoff 3b, Li + Not all of them are located at the Wyckoff 4c point, and some are located at the Wyckoff 3b point. At the same time, energy spectrum line scanning and surface scanning analysis are performed on the cut surface (cross section) of the positive electrode material. Zn and Li in the positive electrode material are uniformly and randomly distributed in the lattice.
[0110] Performance Testing
[0111] The positive electrode materials in Examples 1 to 6 and Comparative Examples 1 to 8 were respectively made into positive electrode sheets. At the same time, metallic sodium was used as the negative electrode sheet, glass fiber was used as the separator, and 1M NaPF 6 The propylene carbonate (PC) / ethyl methyl carbonate (EMC) solution was used as the electrolyte, and 4% of the weight of the above electrolyte was added with fluorinated ethylene carbonate (FEC), and a button cell was assembled for charge and discharge tests. The current density was 15 mA / g (0.1C), the voltage range was 2 to 4 V, and the material was cycled 100 times at 1C. The test results are shown in Tables 1 and Figures 3 to 6 As shown:
[0112] Table 1 Capacity of positive electrode materials in various embodiments and comparative examples and capacity retention rate after 100 cycles
[0113]
[0114] It can be seen from the test results in Table 1 that the sodium ion battery assembled with the positive electrode sheet made of the positive electrode material of the present invention has a capacity of 152.1-156.1 mAh / g under the conditions of voltage of 2-4V and 0.1C, and the capacity retention rate after 100 charge and discharge cycles reaches 87%-90%, indicating that the positive electrode material of the present invention has both high capacity and excellent cycle stability. At the same time, from the test results of Example 1 and Comparative Example 1, Comparative Example 2, Comparative Example 4 and Comparative Example 5, it can be found that the capacity and cycle stability of the positive electrode material can be effectively improved by orderly and coordinated doping of Li and Zn; from the test results of Example 1 and Comparative Example 8, it can be found that the capacity and cycle stability of the positive electrode material can be further improved by gradient doping of Li and Zn. It can be concluded from the test results of Examples 1 to 6 and Comparative Example 3 that when M contains more than two active elements, the capacity and cycle stability of the product can be effectively improved due to the synergistic effect of the doping elements, so that the maximum capacity of the positive electrode material between 2 and 4 V can reach 156.1 mAh / g, and the capacity retention rate after 100 cycles can reach 90%; It can be concluded from the test results of Examples 1 to 6 and Comparative Examples 6 to 7 that when M contains Ni and the Ni content is strictly controlled, the positive electrode material has a higher specific capacity and a longer cycle life.
[0115] Figure 3 , Figure 5 and Figure 6 The charge and discharge curves of the positive electrode materials in Example 1, Comparative Example 1 and Comparative Example 2 are respectively. It can be seen that the charge and discharge curve of the positive electrode material in Example 1 is smooth without steps; the charge and discharge curve of the positive electrode material in Comparative Example 1 is not smooth, and there is a step near 2.8V; the charge and discharge curve of the positive electrode material in Comparative Example 2 is not smooth, and there is also a step near 2.8V, indicating that there are irreversible, unfavorable phase changes and Mn 3+ The Jahn-Teller effect. Figure 4 It can be found that the positive electrode material in Example 1 has excellent cycle stability.
[0116] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A positive electrode material, It is characterized in that The positive electrode material is in the O3 phase, and its general chemical formula is Na n Mn 1-x-y- z M x Zn y Li z O 2 ; M is Cu 2+ 、Ni 2+ Cr 2+ , Fe 3+ and Co 2+ At least one of; Among them, 0.5≤x≤0.6, 0.05≤y≤0.1, 0.005≤z≤0.05, 0.9≤n≤1.1, and x, y, z, n satisfy the principle of electrical neutrality in terms of numerical value; The Na n Mn 1-x-y-z M x Zn y Li z O 2 All Zn elements in 2+ Located at Wyckoff 3b point, all Li elements are Li + Located at Wyckoff 4c point.
2. The positive electrode material according to claim 1, It is characterized in that The Na n Mn 1-x-y-z M x Zn y Li z O 2 The Mn and M elements in the lattice are randomly distributed.
3. The positive electrode material according to claim 1, It is characterized in that The positive electrode material is a single crystal structure.
4. The positive electrode material according to claim 3, It is characterized in that The particle size D50 of the positive electrode material is 4 to 8 μm.
5. The positive electrode material according to claim 1, It is characterized in that The M is Cu 2+ 、Ni 2+ Cr 2+ , Fe 3+ and Co 2+ At least two of the .
6. The positive electrode material according to claim 5, It is characterized in that The M is Cu 2+ 、Ni 2+ Cr 2+ , Fe 3+ and Co 2+ At least two of the above, and one of them is Ni.
7. The positive electrode material according to claim 6, It is characterized in that The molar ratio of Ni to (M+Mn) is (0.23-0.29):
1.
8. A method for preparing the positive electrode material according to any one of claims 1 to 7, It is characterized in that The following steps are involved: S1. mixing and co-precipitating a manganese-containing compound and a compound containing an M element to obtain a precursor; S2. The precursor in S1 is mixed evenly with a sodium-containing compound, a lithium-containing compound and a zinc-containing compound, and subjected to a high-temperature solid-phase reaction to obtain a positive electrode material; Wherein, the M element in S1 is at least one of Cu, Ni, Cr, Fe and Co.
9. The preparation method according to claim 8, It is characterized in that The temperature of the high temperature solid phase reaction is 650-1000° C. and the time is 10-20 hours.
10. The preparation method according to claim 8, It is characterized in that The precursor is at least one of hydroxide, carbonate and oxalate.
11. The preparation method according to claim 8, It is characterized in that The sodium-containing compound is at least one of sodium carbonate, sodium acetate and sodium oxalate; The zinc-containing compound is at least one of zinc acetate, zinc oxalate, zinc carbonate and zinc oxide; The lithium-containing compound is at least one of lithium acetate, lithium oxalate, lithium carbonate and lithium hydroxide.
12. Use of the positive electrode material according to any one of claims 1 to 7 in a sodium ion battery.
13. A positive electrode sheet, comprising a current collector and a positive electrode active material layer disposed on at least one side of the current collector, It is characterized in that The positive electrode active material layer comprises the positive electrode material according to any one of claims 1 to 7.
14. A sodium ion battery comprising a positive electrode sheet, a negative electrode sheet, a separator between the positive electrode sheet and the negative electrode sheet, and an electrolyte, It is characterized in that The positive electrode sheet comprises the positive electrode material according to any one of claims 1 to 7.
Citation Information
Cited By
Negative electrode based on phase-change material modified zinc powder, preparation method of negative electrode and aqueous zinc ion battery
CN122246039A