Graphene-based conductive agent and preparation method and application thereof

Through the preparation of graphene-based conductive agents, the gas phase intercalation and heat treatment technology of graphene and metal chloride are used to solve the problem of insufficient conductivity of the positive electrode material of ion battery, and the effect of high energy density and long cycle life is achieved.

CN118919726APending Publication Date: 2024-11-08ANHUI UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410994249.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The poor conductivity of the existing ion battery positive electrode materials leads to insufficient charge and discharge performance and cycle life, which cannot meet the needs of high energy density and long cycle life.

Method used

By using the preparation method of graphene-based conductive agent, a graphene-based group with excellent conductivity is formed by gas intercalation of multi-layer graphene and metal chloride under a protective atmosphere, and then mixed with a phosphorus source and lithium source and heat treatment. Conductive agent, used to increase the specific capacity of the positive electrode material.

Benefits of technology

The conductivity and cycle stability of lithium-ion batteries are significantly improved, and the specific capacity of lithium iron phosphate positive electrode is improved to reach 178mAh/g. This method is simple, low-cost and suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919726A_ABST
    Figure CN118919726A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of ion batteries, in particular to a graphene-based conductive agent and a preparation method and application thereof. The preparation method comprises the following steps: preparing a multilayer graphene intercalation compound from graphene and metal chloride through gas phase intercalation; and combining the multi-layer graphene intercalation compound with a lithium source and a phosphorus source through a high-temperature solid-phase method to prepare the graphene-based lithium ion battery positive electrode conductive agent with specific capacity. In the process, lithium iron phosphate nanoparticles or clusters are synthesized and fully filled among graphene sheet layers, so that the interlayer spacing of the graphene is effectively enlarged, further stacking of the graphene is prevented, and the conductivity of the positive electrode material of the ion battery is improved. Moreover, when the graphene-based conductive agent prepared by the invention is used for the lithium ion battery, the actual specific capacity of the lithium iron phosphate positive electrode material can reach 178mAh / g, the theoretical capacity 170mAh / g of the current lithium iron phosphate positive electrode is broken through, and the specific capacity of the lithium iron phosphate positive electrode material is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ion batteries, and in particular to a graphene-based ion conductive agent and a preparation method and application thereof. Background Art

[0002] With the rapid development of electric vehicles and mobile electronic devices, people have higher and higher requirements for the energy density of ion batteries. In recent years, the rapid development of the global economy has led to a continuous increase in energy demand. The development of secondary batteries with high energy density, long cycle life, high safety, green environmental protection and low cost is of great significance in the field of new energy.

[0003] As a common energy storage device, the energy storage principle of ion batteries is that metal ions are embedded / de-embedded in the positive and negative electrode materials, accompanied by the transmission of electrons in the external circuit. Taking lithium-ion batteries as an example, the positive electrode materials of lithium batteries mainly include lithium iron phosphate, lithium manganese oxide, lithium cobalt oxide, ternary materials, etc. Lithium ions are in the lattice of the positive electrode material. Under normal charging and discharging conditions, the positive electrode material gains and loses electrons while embedding and de-embedding lithium ions. Therefore, in order to exert its performance, its ion and electron transmission channels must be guaranteed. However, the positive electrode materials currently used have poor conductivity, and good charge and discharge performance cannot be achieved by relying solely on the conductivity of the positive electrode material itself. Therefore, a certain amount of conductive agent is usually added when preparing ion battery pole pieces to improve the battery's rate and cycle performance. Summary of the invention

[0004] The purpose of the present invention is to provide a graphene-based conductive agent and a preparation method and application thereof, to provide a conductive agent with excellent conductive properties, and to improve the specific capacity of positive electrode materials.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] A method for preparing a graphene-based conductive agent comprises the following steps:

[0007] The multilayer graphene and the metal chloride are intercalated in a gas phase under a protective atmosphere to obtain a multilayer graphene intercalation compound;

[0008] mixing the multilayer graphene intercalation compound, a phosphorus source and a lithium source to obtain a mixed material;

[0009] The mixed material is heat-treated to obtain the graphene-based conductive agent.

[0010] Optionally, the metal chloride comprises at least one of anhydrous aluminum chloride, anhydrous cupric chloride, anhydrous ferric chloride, anhydrous sodium chloride, anhydrous cobalt chloride, anhydrous nickel chloride and anhydrous potassium chloride; and the mass ratio of the multilayer graphene to the metal chloride is 1:1 to 20.

[0011] Optionally, the protective atmosphere contains at least one of nitrogen, argon and helium; the temperature of the gas phase intercalation is 300-500°C, and the time is 5-24 hours; the phosphorus source contains at least one of H3PO4 and NH4H2PO4; the lithium source contains at least one of LiOH, LiH2PO4, Li2CO3 and LiNO3; the molar ratio of the multilayer graphene intercalation compound, the phosphorus source and the lithium source is 1-3:1-3:1-3; the mixed material also contains a carbon source.

[0012] Optionally, the carbon source comprises at least one of glucose, PEG12000, sucrose and polypyrrole; the mass of the carbon source is 0 to 20% of the total mass of the graphene intercalation compound, the phosphorus source and the lithium source.

[0013] Optionally, before the heat treatment, the mixed material is ball-milled; the ball-milling medium comprises at least one of stainless steel balls, agate balls, zirconium oxide balls, aluminum oxide balls and silicon carbide balls; the mass ratio of the ball-milling medium to the mixed material is 15 to 200:1; the ball-milling speed is 50 to 580 rpm, and the time is 0.5 to 72 h.

[0014] Optionally, the heating rate of the heat treatment is 2 to 10°C / min, the temperature is 600 to 800°C, and the time is 2 to 24h.

[0015] The invention provides a graphene-based conductive agent prepared by the preparation method.

[0016] The present invention also provides application of the graphene-based conductive agent in an ion battery.

[0017] Optionally, the ion battery is a lithium ion battery, a sodium ion battery, a zinc ion battery or a potassium ion battery.

[0018] Optionally, when the graphene-based conductive agent is used in an ion battery, the graphene-based conductive agent, active material, binder and solvent are mixed to obtain a positive electrode slurry, and the positive electrode slurry is coated on a positive electrode foil to obtain an ion battery positive electrode material;

[0019] The active material comprises lithium iron phosphate or NCM811, the binder comprises PVDF, PTFE or PVA, and the solvent comprises at least one of N-methylpyrrolidone, water, ethanol and isopropanol; the mass ratio of the graphene-based conductive agent, the active material and the binder is 1 to 4:6 to 8:1.

[0020] The present invention successfully synthesizes a graphene-based conductive agent with a self-contained specific capacity in two steps by ferric chloride vapor intercalation and high-temperature solid-phase method. In this process, the graphene used is a mechanically exfoliated multilayer graphene with an ultra-low defect density. Its unique two-dimensional sheet structure and the delocalized large π bond in the entire sheet make it show the thinnest and softest structural characteristics and excellent electrical conductivity; anhydrous metal chloride vapor intercalation multilayer graphene can effectively expand the interlayer spacing of graphene and prepare multilayer graphene intercalation compounds; then the multilayer graphene intercalation compounds are combined with lithium sources, phosphorus sources, and carbon sources by a high-temperature solid-phase method to prepare a graphene-based ion battery positive electrode conductive agent with a self-contained specific capacity. This process will synthesize lithium iron phosphate nanoparticles and clusters, which can be better combined with active materials in ion batteries to reduce contact resistance, and lithium iron phosphate nanoparticles and clusters are fully filled between graphene sheets, preventing further stacking of graphene, and improving the electrical conductivity of the lithium ion battery positive electrode conductive agent, thereby showing excellent electrochemical performance. Not only that, preventing graphene stacking can form highly conductive graphene sheets, which help electron migration during charging and discharging, thereby increasing the capacity of ion batteries and improving the specific capacity of lithium iron phosphate positive electrodes.

[0021] The graphene-based conductive agent prepared by the present invention has excellent wettability to electrolyte and strong liquid retention capacity; and the graphene-based conductive agent has a regular stacking structure (in which the electrochemically active material is sandwiched by many graphene sheets), and when used as a lithium-ion battery, it provides a buffer matrix for volume changes during lithiation. The presence of lithium iron phosphate distributed between the layers expands the distance between the graphene sheets, which allows lithium ions to diffuse rapidly inside and outside the material, and the mutual coupling allows the specific capacity of the lithium iron phosphate positive electrode to be significantly improved to 178 mAh / g.

[0022] The graphene-based conductive agent prepared by the present invention can be made into an ion battery to establish an excellent conductive network, thereby improving the energy density of the battery and having excellent conductive properties. When it is made into an ion battery, the corresponding metal ions are adsorbed / desorbed on the graphene surface, and the metal ions in the electrolyte undergo redox reactions with the graphene to produce additional capacity, and active substances are generated between the graphene layers, thereby inhibiting the further accumulation of graphene, forming graphene sheets with high conductivity, and expanding the capacity of the ion battery; during the ion battery cycle, some of the racing ions in the electrolyte will also be embedded in the layered structure, and after a long period of circulation, it will be more fully exfoliated and the conductivity will be improved.

[0023] Specifically, when assembled into a lithium-ion battery, additional capacity is generated due to the adsorption / desorption of lithium ions on the graphene surface and the reversible redox reaction between lithium ions in the electrolyte and graphene; lithium iron phosphate nanoparticles generated between graphene layers inhibit further stacking of graphene, while highly conductive graphene sheets help electron migration during charging and discharging, thereby increasing the capacity of lithium-ion batteries. During the cycle, since graphene has a layered structure, some lithium ions in the electrolyte will be embedded in the layered structure, and after a long period of circulation, it will be more fully exfoliated, improving conductivity, overcoming the problem of low electronic conductivity of lithium iron phosphate due to its own structural limitations. After a long period of circulation, the battery internal resistance increases less and the capacity decay decreases less.

[0024] The preparation process of the graphene-based conductive agent of the present invention is simple, low-cost, and easy to achieve large-scale production. In addition, the entire reaction process does not require the addition of any solvent, is low-cost, environmentally friendly, and can achieve commercial production.

[0025] When the graphene-based conductive agent of the present invention is mixed with an active material to prepare a conductive slurry, no dispersant is needed, and uniform dispersion can be achieved by adding only a small amount of solvent. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 XRD comparison diagram of the multilayer graphene intercalation compound prepared in Example 2 and the multilayer graphene;

[0027] Figure 2 TEM images of the multilayer graphene intercalation compound prepared in Example 2, wherein a is a 10 nm TEM image of the multilayer graphene, and b is a local enlarged image of a;

[0028] Figure 3 A Raman comparison chart of the multilayer graphene intercalation compound prepared in Example 2 and the multilayer graphene;

[0029] Figure 4 XRD pattern of the graphene-based conductive agent prepared in Example 9;

[0030] Figure 5 The Raman graph of the graphene-based conductive agent prepared in Example 9;

[0031] Figure 6 HAADF-STEM image of the graphene-based conductive agent prepared in Example 9;

[0032] Figure 7 This is a cycle performance diagram of the graphene-based conductive agent prepared in Example 9;

[0033] Figure 8 This is a rate performance diagram of the graphene-based conductive agent prepared in Example 9 applied to a lithium-ion battery;

[0034] Fig. 9 This is a comparison chart of the impedance of the graphene-based conductive agent, SuperP, carbon nanotubes and Ketjen black prepared in Example 9;

[0035] Fig.10 This is a comparison chart of the specific capacities of the graphene-based conductive agent, SuperP, carbon nanotubes and Ketjen black prepared in Example 9 when applied to lithium iron phosphate positive electrode materials. DETAILED DESCRIPTION

[0036] The present invention provides a method for preparing a graphene-based conductive agent, comprising the following steps:

[0037] The multilayer graphene and the metal chloride are intercalated in a gas phase under a protective atmosphere to obtain a multilayer graphene intercalation compound;

[0038] mixing the multilayer graphene intercalation compound, a phosphorus source and a lithium source to obtain a mixed material;

[0039] The mixed material is heat-treated to obtain the graphene-based conductive agent.

[0040] In the present invention, the metal chloride preferably comprises at least one of anhydrous aluminum chloride, anhydrous cupric chloride, anhydrous ferric chloride, anhydrous sodium chloride, anhydrous cobalt chloride, anhydrous nickel chloride and anhydrous potassium chloride; the mass ratio of the multilayer graphene to the metal chloride is preferably 1:1 to 20, more preferably 1:3 to 15, and even more preferably 1:6 to 12.

[0041] In the present invention, the method for preparing the multilayer graphene is preferably to mix artificial graphite powder, sodium carboxymethyl cellulose (CMC) and deionized water and then grind to obtain multilayer graphene;

[0042] In the present invention, before performing vapor phase intercalation, multilayer graphene and metal chloride are preferably placed at both ends of a porcelain boat, and then quickly transferred to a tube furnace; before performing vapor phase intercalation, the heating rate is preferably 2 to 10°C / min, and more preferably 5 to 8°C / min.

[0043] In the present invention, the protective atmosphere comprises at least one of nitrogen, argon and helium; the temperature of the gas phase intercalation is preferably 300-500° C., more preferably 350-400° C.; the time is preferably 5-24 hours, more preferably 8-18 hours, and even more preferably 12-15 hours;

[0044] The phosphorus source comprises at least one of H3PO4 and NH4H2PO4; the lithium source preferably comprises at least one of LiOH, LiH2PO4, Li2CO3 and LiNO3; the molar ratio of the multilayer graphene intercalation compound, the phosphorus source and the lithium source is preferably 1-3:1-3:1-3, and further preferably 2-3:1-2:1-2; the mixed material preferably also comprises a carbon source.

[0045] In the present invention, the carbon source preferably comprises at least one of glucose, PEG12000, sucrose and polypyrrole; the mass of the carbon source is preferably 0-20% of the total mass of the graphene intercalation compound, the phosphorus source and the lithium source, more preferably 5-18%, and even more preferably 10-15%.

[0046] In the present invention, before the heat treatment, the mixed material is preferably ball-milled; the ball-milling medium preferably comprises at least one of stainless steel balls, agate balls, zirconium oxide balls, aluminum oxide balls and silicon carbide balls; the mass ratio of the ball-milling medium to the mixed material is preferably 15 to 200:1, and more preferably 100 to 150:1; the rotation speed of the ball mill is preferably 50 to 580 rpm, and more preferably 200 to 500 rpm; the time is preferably 0.5 to 72 h, and more preferably 2 to 24 h, and more preferably 6 to 12 h.

[0047] In the present invention, the ball milling jar is preferably made of stainless steel, agate or zirconium oxide, and after the ball milling is completed, the ball milling medium is preferably taken out with tweezers.

[0048] In the present invention, the heating rate of the heat treatment is preferably 2-10°C / min, more preferably 5-8°C / min; the temperature is preferably 600-800°C, more preferably 700-750°C; the time is preferably 2-24h, more preferably 4-18h, more preferably 6-12h, and even more preferably 8-10h.

[0049] In the present invention, the heat treatment is preferably carried out in a tubular furnace, and a protective gas needs to be introduced, and the protective gas is preferably at least one of nitrogen, argon and helium.

[0050] The invention provides a graphene-based conductive agent prepared by the preparation method.

[0051] The present invention also provides application of the graphene-based conductive agent in an ion battery.

[0052] In the present invention, the ion battery is preferably a lithium ion battery, a sodium ion battery, a zinc ion battery or a potassium ion battery.

[0053] In the present invention, when the graphene-based conductive agent is used in an ion battery, the graphene-based conductive agent, active material, binder and solvent are preferably mixed to obtain a positive electrode slurry, and the positive electrode slurry is coated on a positive electrode foil to obtain an ion battery positive electrode material;

[0054] The active material preferably comprises lithium iron phosphate or NCM811, the binder preferably comprises PVDF, PTFE or PVA, and the solvent preferably comprises at least one of N-methylpyrrolidone, water, ethanol and isopropanol; the dosage ratio of the graphene-based conductive agent, the active material and the binder is preferably 1-4:6-8:1, and more preferably 2-3:7-8:1; the dosage of the solvent is not particularly limited and can be adjusted according to actual conditions. The dosage ratio of the graphene-based conductive agent to the solvent can preferably be 100 mg:400 μL.

[0055] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0056] Example 1

[0057] 50 kg of artificial graphite powder, 20 kg of sodium carboxymethyl cellulose (CMC) and 100 kg of deionized water were added into a barrel and mixed evenly to obtain a graphene mixed slurry. Zirconium beads with a diameter of 0.6 to 0.8 mm were placed in the grinding chamber of the barrel to grind the above-mentioned graphene mixed slurry. Part of the ground slurry was taken out on time, freeze-dried and tested for XRD until the 002 peak was 2000, and graphene slurry was obtained. After washing and drying, multi-layer graphene was obtained.

[0058] In an anhydrous and oxygen-free glove box, 1 g of multilayer graphene and 6 g of anhydrous ferric chloride were weighed respectively, ground for 5 minutes, and placed at both ends of a porcelain boat (anhydrous ferric chloride was placed at one end of the porcelain boat and multilayer graphene was placed at the other end). Then, they were quickly transferred to a tubular furnace and heated to 400°C at a heating rate of 10°C / min. The temperature was kept for 24 hours, and then naturally cooled to room temperature to form a multilayer graphene intercalation compound.

[0059] Weigh 1 g of a multilayer graphene intercalation compound, 0.2334 g of NH4H2PO4 and 0.3004 g of Li2CO3, and further weigh 0.3068 g of glucose to obtain a mixed material;

[0060] The mixed material is placed in a zirconia ball mill, and the ball mill is placed on a planetary ball mill for ball milling. The ball milling medium is zirconia beads, and the mass ratio of the balls to the materials is 200:1. The ball milling speed is 500 rpm. The ball milling time is 2 hours. After the ball milling, the zirconium beads are taken out with tweezers. The ball-milled product is transferred to a tubular furnace, nitrogen is introduced as a protective gas, and the temperature is increased to 700°C at a heating rate of 5°C / min. The temperature is kept for 10 hours, and then naturally cooled to room temperature to obtain a graphene-based conductive agent.

[0061] Example 2

[0062] In an anhydrous and oxygen-free glove box, 1 g of the multilayer graphene and 15 g of anhydrous ferric chloride obtained in Example 1 were weighed respectively, ground for 5 min respectively, and then placed at both ends of a porcelain boat (anhydrous ferric chloride was placed at one end of the porcelain boat and the multilayer graphene was placed at the other end), and then quickly transferred to a tubular furnace, heated to 400 ° C at a heating rate of 10 ° C / min, kept warm for 24 h, and then naturally cooled to room temperature to form a multilayer graphene intercalation compound.

[0063] Weigh 1 g of a multilayer graphene intercalation compound, 0.1932 g of NH4H2PO4 and 0.1243 g of Li2CO3, and further weigh 0.2635 g of glucose to obtain a mixed material;

[0064] The mixed material is placed in a zirconia ball mill, and the ball mill is placed on a planetary ball mill for ball milling. The ball milling medium is zirconia beads, and the mass ratio of the balls to the materials is 200:1. The ball milling speed is 500 rpm. The ball milling time is 2 hours. After the ball milling, the zirconium beads are taken out with tweezers. The ball-milled product is transferred to a tubular furnace, nitrogen is introduced as a protective gas, and the temperature is increased to 700°C at a heating rate of 5°C / min. The temperature is kept for 10 hours, and then naturally cooled to room temperature to obtain a graphene-based conductive agent.

[0065] Example 3

[0066] In an anhydrous and oxygen-free glove box, 1 g of the multilayer graphene and 15 g of anhydrous ferric chloride obtained in Example 1 were weighed respectively, ground for 5 min respectively, and then placed at both ends of a porcelain boat (anhydrous ferric chloride was placed at one end of the porcelain boat and the multilayer graphene was placed at the other end), and then quickly transferred to a tubular furnace, heated to 400 ° C at a heating rate of 10 ° C / min, kept warm for 24 h, and then naturally cooled to room temperature to form a multilayer graphene intercalation compound.

[0067] Weigh 1 g of a multilayer graphene intercalation compound, 0.1932 g of NH4H2PO4 and 0.2486 g of Li2CO3, and further weigh 0.2884 g of glucose to obtain a mixed material;

[0068] The mixed material is placed in a zirconia ball mill, and the ball mill is placed on a planetary ball mill for ball milling. The ball milling medium is zirconia beads, and the mass ratio of the balls to the materials is 200:1. The ball milling speed is 500 rpm. The ball milling time is 2 hours. After the ball milling, the zirconium beads are taken out with tweezers. The ball-milled product is transferred to a tubular furnace, nitrogen is introduced as a protective gas, and the temperature is increased to 700°C at a heating rate of 5°C / min. The temperature is kept for 2 hours, and then naturally cooled to room temperature to obtain a graphene-based conductive agent.

[0069] Example 4

[0070] In an anhydrous and oxygen-free glove box, 1 g of the multilayer graphene and 15 g of anhydrous ferric chloride obtained in Example 1 were weighed respectively, ground for 5 min respectively, and then placed at both ends of a porcelain boat (anhydrous ferric chloride was placed at one end of the porcelain boat and the multilayer graphene was placed at the other end), and then quickly transferred to a tubular furnace, heated to 400 ° C at a heating rate of 10 ° C / min, kept warm for 24 h, and then naturally cooled to room temperature to form a multilayer graphene intercalation compound.

[0071] Weigh 1 g of a multilayer graphene intercalation compound, 0.1932 g of NH4H2PO4 and 0.1243 g of Li2CO3, and further weigh 0.2635 g of glucose to obtain a mixed material;

[0072] The mixed material is placed in a zirconia ball mill, and the ball mill is placed on a planetary ball mill for ball milling. The ball milling medium is zirconia beads, and the mass ratio of the balls to the materials is 200:1. The ball milling speed is 500 rpm. The ball milling time is 2 hours. After the ball milling, the zirconium beads are taken out with tweezers. The ball-milled product is transferred to a tubular furnace, nitrogen is introduced as a protective gas, and the temperature is increased to 700°C at a heating rate of 5°C / min. The temperature is kept for 4 hours, and then naturally cooled to room temperature to obtain a graphene-based conductive agent.

[0073] Example 5

[0074] In an anhydrous and oxygen-free glove box, 1 g of the multilayer graphene and 15 g of anhydrous ferric chloride obtained in Example 1 were weighed respectively, ground for 5 min respectively, and then placed at both ends of a porcelain boat (anhydrous ferric chloride was placed at one end of the porcelain boat and the multilayer graphene was placed at the other end), and then quickly transferred to a tubular furnace, heated to 400 ° C at a heating rate of 10 ° C / min, kept warm for 24 h, and then naturally cooled to room temperature to form a multilayer graphene intercalation compound.

[0075] Weigh 1 g of a multilayer graphene intercalation compound, 0.1932 g of NH4H2PO4 and 0.1243 g of Li2CO3, and further weigh 0.2635 g of glucose to obtain a mixed material;

[0076] The mixed material is placed in a zirconia ball mill, and the ball mill is placed on a planetary ball mill for ball milling. The ball milling medium is zirconia beads, and the mass ratio of the balls to the materials is 200:1. The ball milling speed is 500 rpm. The ball milling time is 2 hours. After the ball milling, the zirconium beads are taken out with tweezers. The ball-milled product is transferred to a tubular furnace, nitrogen is introduced as a protective gas, and the temperature is increased to 700°C at a heating rate of 5°C / min. The temperature is kept for 6 hours, and then naturally cooled to room temperature to obtain a graphene-based conductive agent.

[0077] Example 6

[0078] In an anhydrous and oxygen-free glove box, 1 g of the multilayer graphene and 15 g of anhydrous ferric chloride obtained in Example 1 were weighed respectively, ground for 5 min respectively, and then placed at both ends of a porcelain boat (anhydrous ferric chloride was placed at one end of the porcelain boat and the multilayer graphene was placed at the other end), and then quickly transferred to a tubular furnace, heated to 400 ° C at a heating rate of 10 ° C / min, kept warm for 24 h, and then naturally cooled to room temperature to form a multilayer graphene intercalation compound.

[0079] Weigh 1 g of a multilayer graphene intercalation compound, 0.1932 g of NH4H2PO4 and 0.1243 g of Li2CO3, and further weigh 0.2635 g of glucose to obtain a mixed material;

[0080] The mixed material is placed in a zirconia ball mill, and the ball mill is placed on a planetary ball mill for ball milling. The ball milling medium is zirconia beads, and the mass ratio of the balls to the materials is 200:1. The ball milling speed is 500 rpm. The ball milling time is 2 hours. After the ball milling, the zirconium beads are taken out with tweezers. The ball-milled product is transferred to a tubular furnace, nitrogen is introduced as a protective gas, and the temperature is increased to 700°C at a heating rate of 5°C / min. The temperature is kept for 8 hours, and then naturally cooled to room temperature to obtain a graphene-based conductive agent.

[0081] Example 7

[0082] In an anhydrous and oxygen-free glove box, 1 g of the multilayer graphene and 15 g of anhydrous ferric chloride obtained in Example 1 were weighed respectively, ground for 5 min respectively, and then placed at both ends of a porcelain boat (anhydrous ferric chloride was placed at one end of the porcelain boat and the multilayer graphene was placed at the other end), and then quickly transferred to a tubular furnace, heated to 400 ° C at a heating rate of 10 ° C / min, kept warm for 24 h, and then naturally cooled to room temperature to form a multilayer graphene intercalation compound.

[0083] Weigh 1 g of a multilayer graphene intercalation compound, 0.1932 g of NH4H2PO4 and 0.1243 g of Li2CO3, and further weigh 0.2635 g of glucose to obtain a mixed material;

[0084] The mixed material is placed in a zirconia ball mill, and the ball mill is placed on a planetary ball mill for ball milling. The ball milling medium is zirconia beads, and the mass ratio of the balls to the materials is 200:1. The ball milling speed is 500 rpm. The ball milling time is 2 hours. After the ball milling, the zirconium beads are taken out with tweezers. The ball-milled product is transferred to a tubular furnace, nitrogen is introduced as a protective gas, and the temperature is increased to 700°C at a heating rate of 5°C / min. The temperature is kept for 12 hours, and then naturally cooled to room temperature to obtain a graphene-based conductive agent.

[0085] Example 8

[0086] In an anhydrous and oxygen-free glove box, 1 g of the multilayer graphene and 15 g of anhydrous ferric chloride obtained in Example 1 were weighed respectively, ground for 5 min respectively, and then placed at both ends of a porcelain boat (anhydrous ferric chloride was placed at one end of the porcelain boat and the multilayer graphene was placed at the other end), and then quickly transferred to a tubular furnace, heated to 400 ° C at a heating rate of 10 ° C / min, kept warm for 24 h, and then naturally cooled to room temperature to form a multilayer graphene intercalation compound.

[0087] Weigh 1 g of a multilayer graphene intercalation compound, 0.1932 g of NH4H2PO4 and 0.1243 g of Li2CO3, and further weigh 0.1318 g of glucose to obtain a mixed material;

[0088] The mixed material is placed in a zirconia ball mill, and the ball mill is placed on a planetary ball mill for ball milling. The ball milling medium is zirconia beads, and the mass ratio of the balls to the materials is 200:1. The ball milling speed is 500 rpm. The ball milling time is 2 hours. After the ball milling, the zirconium beads are taken out with tweezers. The ball-milled product is transferred to a tubular furnace, nitrogen is introduced as a protective gas, and the temperature is increased to 700°C at a heating rate of 5°C / min. The temperature is kept for 12 hours, and then naturally cooled to room temperature to obtain a graphene-based conductive agent.

[0089] Example 9

[0090] In an anhydrous and oxygen-free glove box, 1 g of the multilayer graphene and 15 g of anhydrous ferric chloride obtained in Example 1 were weighed respectively, ground for 5 min respectively, and then placed at both ends of a porcelain boat (anhydrous ferric chloride was placed at one end of the porcelain boat and the multilayer graphene was placed at the other end), and then quickly transferred to a tubular furnace, heated to 400 ° C at a heating rate of 10 ° C / min, kept warm for 24 h, and then naturally cooled to room temperature to form a multilayer graphene intercalation compound.

[0091] Weigh 1 g of multilayer graphene intercalation compound, 0.1932 g of NH4H2PO4 and 0.1243 g of Li2CO3, and also weigh 0.0659 g of glucose to obtain a mixed material;

[0092] The mixed material is placed in a zirconia ball mill, and the ball mill is placed on a planetary ball mill for ball milling. The ball milling medium is zirconia beads, and the mass ratio of the balls to the materials is 200:1. The ball milling speed is 500 rpm. The ball milling time is 2 hours. After the ball milling, the zirconium beads are taken out with tweezers. The ball-milled product is transferred to a tubular furnace, nitrogen is introduced as a protective gas, and the temperature is increased to 700°C at a heating rate of 5°C / min. The temperature is kept for 12 hours, and then naturally cooled to room temperature to obtain a graphene-based conductive agent.

[0093] Example 10

[0094] In an anhydrous and oxygen-free glove box, 1 g of the multilayer graphene and 15 g of anhydrous ferric chloride obtained in Example 1 were weighed respectively, ground for 5 min respectively, and then placed at both ends of a porcelain boat (anhydrous ferric chloride was placed at one end of the porcelain boat and the multilayer graphene was placed at the other end), and then quickly transferred to a tubular furnace, heated to 400 ° C at a heating rate of 10 ° C / min, kept warm for 24 h, and then naturally cooled to room temperature to form a multilayer graphene intercalation compound.

[0095] Weigh 1 g of a multilayer graphene intercalation compound, 0.1932 g of NH4H2PO4 and 0.1243 g of Li2CO3, and further weigh 0.1976 g of glucose to obtain a mixed material;

[0096] The mixed material is placed in a zirconia ball mill, and the ball mill is placed on a planetary ball mill for ball milling. The ball milling medium is zirconia beads, and the mass ratio of the balls to the materials is 200:1. The ball milling speed is 500 rpm. The ball milling time is 2 hours. After the ball milling, the zirconium beads are taken out with tweezers. The ball-milled product is transferred to a tubular furnace, nitrogen is introduced as a protective gas, and the temperature is increased to 700°C at a heating rate of 5°C / min. The temperature is kept for 12 hours, and then naturally cooled to room temperature to obtain a graphene-based conductive agent.

[0097] Embodiment 11

[0098] In an anhydrous and oxygen-free glove box, 1 g of the multilayer graphene and 15 g of anhydrous ferric chloride obtained in Example 1 were weighed respectively, ground for 5 min respectively, and then placed at both ends of a porcelain boat (anhydrous ferric chloride was placed at one end of the porcelain boat and the multilayer graphene was placed at the other end), and then quickly transferred to a tubular furnace, heated to 400 ° C at a heating rate of 10 ° C / min, kept warm for 24 h, and then naturally cooled to room temperature to form a multilayer graphene intercalation compound.

[0099] Weigh 1 g of a multilayer graphene intercalation compound, 0.1932 g of NH4H2PO4, and 0.1243 g of Li2CO3, and mix them to obtain a mixed material;

[0100] The mixed material is placed in a zirconia ball mill, and the ball mill is placed on a planetary ball mill for ball milling. The ball milling medium is zirconia beads, and the mass ratio of the balls to the materials is 200:1. The ball milling speed is 500 rpm. The ball milling time is 2 hours. After the ball milling, the zirconium beads are taken out with tweezers. The ball-milled product is transferred to a tubular furnace, nitrogen is introduced as a protective gas, and the temperature is increased to 700°C at a heating rate of 5°C / min. The temperature is kept for 12 hours, and then naturally cooled to room temperature to obtain a graphene-based conductive agent.

[0101] Test Case

[0102] XRD detection was performed on the multilayer graphene intercalation compound prepared in Example 2 and the multilayer graphene prepared in Example 1. The results are as follows: Figure 1 As shown;

[0103] pass Figure 1 It can be seen that the characteristic peaks of multilayer graphene disappear after FeCl3 vapor intercalation, and a series of intercalation characteristic peaks appear.

[0104] The multilayer graphene intercalation compound prepared in Example 2 was subjected to TEM detection, and the results were as follows: Figure 2 As shown, a is a 10 nm TEM image of a multilayer graphene intercalation compound, and b is a local enlarged image of a;

[0105] pass Figure 2 It can be found that the interlayer spacing of graphite expanded from 0.34nm to 0.41nm after intercalation, indicating that anhydrous ferric chloride was successfully inserted into the graphite interlayer.

[0106] The multilayer graphene intercalation compound prepared in Example 2 and the multilayer graphene prepared in Example 1 were subjected to Raman detection, and the results were as follows: Figure 3 As shown;

[0107] pass Figure 3 It can be seen that the G peak shows a “blue shift” phenomenon, indicating that the interlayer space increases and a first-order intercalation peak appears. The increase in 2D peak intensity represents a decrease in the number of graphene layers.

[0108] The graphene-based conductive agent prepared in Example 9 was subjected to XRD detection, and the results were as follows: Figure 4 As shown;

[0109] pass Figure 4 It can be found that the peak position of the obtained graphene-based conductive agent has an additional characteristic peak of graphite 002 compared to the standard card position of lithium iron phosphate. Multilayer graphene is peeled off into few-layer graphene and lithium iron phosphate is successfully synthesized at the same time.

[0110] The graphene-based conductive agent prepared in Example 9 was subjected to Raman detection, and the results were as follows: Figure 5 As shown;

[0111] pass Figure 5 It can be found that there is PO4 in the graphene-based conductive agent 3- Peak represents the successful synthesis of lithium iron phosphate.

[0112] The graphene-based conductive agent prepared in Example 9 was subjected to HAADF-STEM detection, and the results were as follows: Figure 6 As shown;

[0113] pass Figure 6 It can be found that there are 211 crystal planes corresponding to the lattice size of lithium iron phosphate in the graphene-based conductive agent.

[0114] Method for preparing button-type batteries from the graphene-based conductive agent prepared by the present invention:

[0115] Weigh 100 mg of the graphene-based conductive agent prepared in Example 9, 800 mg of lithium iron phosphate and 100 mg of PVDF, grind and mix them in an agate mortar for 10 min, transfer the mixture into a small glass bottle, and place it in a vacuum oven for drying at 80°C for 8 h. After the powder is dry, place it on a magnetic stirrer, add 400 μL of N-methylpyrrolidone as a solvent to form a slurry with moderate viscosity, seal the bottle mouth with sealing glue, and stir for 12 h to form a uniformly dispersed positive electrode slurry.

[0116] Use the 100 μm surface of the four-sided film coating machine to scrape the positive electrode slurry onto the carbon-coated aluminum foil, and then place it in a vacuum oven to dry thoroughly (dry at 80°C for 12 hours);

[0117] The dried positive electrode sheet was compacted with a roller press, and cut into discs with a diameter of 12 mm with a slicer for later use. A commercial lithium sheet was used as the negative electrode, the diaphragm was a Celgard 2400 diaphragm, and the electrolyte was 1M LiPF6 (EC:DMC:EMC=1:1:1). The buttons were assembled into button cells in a glove box and left to stand for 12 hours for aging to obtain button cells.

[0118] The graphene-based conductive agent prepared in Example 9 was tested for cycle performance. The results are as follows: Figure 7 As shown;

[0119] pass Figure 7 It can be seen that the graphene-based conductive agent has excellent rate performance. Under large current discharge, at a rate of 0.5C, it can still maintain a capacity of about 150mAh / g; at a rate of 10C, it can still maintain a capacity of about 50mAh / g.

[0120] The graphene-based conductive agent prepared in Example 9 was assembled into a button-type battery using the above method for rate performance testing. The results are as follows: Figure 8 As shown;

[0121] pass Figure 8 It can be seen that the initial capacity of the graphene-based conductive agent is 175 mAh / g under the rate condition of 0.1C, which exceeds the theoretical capacity of lithium iron phosphate, and has a long cycle life. The long cycle capacity retention rate after 100 cycles is 95.5%.

[0122] SuperP (SP), carbon nanotubes (CNT) and Ketjen black conductive agent (KB) were used to replace the graphene-based conductive agent (LFP / G) and assembled into button cells using the above method;

[0123] The impedance test of the button cell was carried out, and the results were as follows: Fig. 9 as stated;

[0124] pass Fig. 9 It can be found that the conductivity of the graphene-based conductive agent prepared by the present invention is excellent, which is significantly higher than that of SuperP, carbon nanotubes and Ketjen black conductive agents;

[0125] The specific capacity test of the button cell was carried out, and the results were as follows: Fig.10 As shown:

[0126] pass Fig.10 It can be found that in the button cell assembled with the graphene-based conductive agent prepared by the present invention, the actual specific capacity of the lithium iron phosphate positive electrode can reach 178 mAh / g, breaking through the current theoretical capacity of 170 mAh / g of the lithium iron phosphate positive electrode. It can be seen that when the conductive agent prepared by the method of the present invention is applied to lithium-ion batteries, it can significantly improve the specific capacity of the lithium iron phosphate positive electrode material.

[0127] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a graphene-based conductive agent, characterized in that: The following steps are involved: The multilayer graphene and the metal chloride are intercalated in a gas phase under a protective atmosphere to obtain a multilayer graphene intercalation compound; mixing the multilayer graphene intercalation compound, a phosphorus source and a lithium source to obtain a mixed material; The mixed material is heat-treated to obtain the graphene-based conductive agent.

2. The preparation method according to claim 1, characterized in that: The metal chloride comprises at least one of anhydrous aluminum chloride, anhydrous cupric chloride, anhydrous ferric chloride, anhydrous sodium chloride, anhydrous cobalt chloride, anhydrous nickel chloride and anhydrous potassium chloride; and the mass ratio of the multilayer graphene to the metal chloride is 1:1-20.

3. The preparation method according to claim 1, characterized in that: The protective atmosphere comprises at least one of nitrogen, argon and helium; the temperature of the gas phase intercalation is 300-500°C and the time is 5-24 hours; the phosphorus source comprises at least one of H3PO4 and NH4H2PO4; the lithium source comprises at least one of LiOH, LiH2PO4, Li2CO3 and LiNO3; the molar ratio of the multilayer graphene intercalation compound, the phosphorus source and the lithium source is 1-3:1-3:1-3; the mixed material also comprises a carbon source.

4. The preparation method according to claim 3, characterized in that: The carbon source comprises at least one of glucose, PEG12000, sucrose and polypyrrole; the mass of the carbon source is 0-20% of the total mass of the graphene intercalation compound, the phosphorus source and the lithium source.

5. The preparation method according to claim 1, characterized in that: Before the heat treatment, the mixed material is ball-milled; the ball-milling medium comprises at least one of stainless steel balls, agate balls, zirconium oxide balls, aluminum oxide balls and silicon carbide balls; the mass ratio of the ball-milling medium to the mixed material is 15 to 200:1; the ball-milling speed is 50 to 580 rpm, and the time is 0.5 to 72 hours.

6. The preparation method according to claim 1, characterized in that: The heating rate of the heat treatment is 2-10°C / min, the temperature is 600-800°C, and the time is 2-24h.

7. The graphene-based conductive agent obtained by the preparation method according to claims 1 to 6.

8. Use of the graphene-based conductive agent obtained by the preparation method of claims 1 to 6 or the graphene-based conductive agent of claim 7 in an ion battery.

9. The use according to claim 8, characterized in that: The ion battery is a lithium ion battery, a sodium ion battery, a zinc ion battery or a potassium ion battery.

10. The use according to claim 8, characterized in that: The graphene-based conductive agent, active material, binder and solvent are mixed to obtain positive electrode slurry, and the positive electrode slurry is coated on a positive electrode foil to obtain a positive electrode material for an ion battery; The active material comprises lithium iron phosphate or NCM811, the binder comprises PVDF, PTFE or PVA, and the solvent comprises at least one of N-methylpyrrolidone, water, ethanol and isopropanol; the mass ratio of the graphene-based conductive agent, the active material and the binder is 1 to 4:6 to 8:1.

Citation Information

Patent Citations

  • High-conductivity graphene-based lithium iron phosphate sphere composite, preparation method thereof and lithium ion battery containing same

    CN107394152A

  • Preparation method of dispersible graphene intercalation compound

    CN108516540A

  • Exfoliated graphite worm-protected metal fluoride and metal chloride cathode active materials for lithium batteries

    CN110352524A