Composite lithium supplementing material and preparation method thereof, positive electrode material and secondary battery
By designing conductive channels in lithium supplementary materials, the problems of poor conductivity and high internal impedance are solved, and the life and conduction efficiency of lithium-ion batteries are improved.
Patent Information
- Application Number
- CN202411043935.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-08
AI Technical Summary
The existing lithium supplementary materials have poor conductivity and high internal impedance, resulting in a shortened lithium-ion battery life and low lithium-ion conduction efficiency.
Using composite lithium supplement material, including a lithium-rich core and a protective layer covering its outer layer, a conductive or ion-conducting channel is opened on the protective layer, and the lithium ion conduction is improved by filling the channel with functional materials to reduce internal impedance and decomposition voltage. Pass efficiency.
By forming conductive channels, the conductivity of the lithium-rich core is improved, the internal impedance and decomposition voltage are reduced, the life of the lithium-ion battery is extended, and the lithium-ion conduction efficiency is improved.
Smart Images

Figure CN118919727A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of secondary batteries, and in particular to a composite lithium supplement material and a preparation method thereof, a positive electrode material and a secondary battery. Background Art
[0002] During the first charge and discharge of liquid lithium-ion batteries, the Li + Reacting with the electrolyte, a solid electrolyte interface film (SEI) will be formed on the surface of the negative electrode material. This process will irreversibly consume more than 10% of the lithium source in the positive electrode material, the coulomb efficiency in the first week will be less than 90%, and the active lithium in the positive electrode will continue to be consumed during the charge and discharge cycle of the lithium battery, resulting in a shortened life of the lithium-ion battery. In response to this phenomenon, the current solution is to add appropriate lithium supplement materials to the positive electrode material, and reduce the lithium loss during the cycle by releasing active lithium through the decomposition of the lithium supplement material during the battery charging process. Common positive electrode lithium supplement materials (such as lithium-rich manganese, lithium-rich iron, lithium-rich nickel, etc.) generally have poor conductivity and high internal impedance. Therefore, how to solve the problem of poor conductivity and high internal impedance of lithium supplement materials has become the key. Summary of the invention
[0003] The purpose of the present application is to provide a composite lithium supplement material and a preparation method thereof, a positive electrode material and a secondary battery, so as to solve the problems of poor conductivity and high internal impedance of existing lithium supplement materials.
[0004] To achieve the purpose of this application, this application provides the following technical solutions:
[0005] In a first aspect, the present invention provides a composite lithium supplement material, comprising a lithium-rich core and a protective layer, wherein the protective layer is coated on the outer surface of the lithium-rich core, the protective layer is provided with a first channel, and the first channel is filled with a first functional material.
[0006] The present invention provides a composite lithium supplement material, which includes a lithium-rich core and a protective layer coated on the outer layer thereof, wherein a first channel is opened on the protective layer, and the first channel is filled with a first functional material. Through the first channel and the texture formed by the first functional material, a functional channel (such as a conductive or ion-conducting channel) is formed on the surface of the lithium supplement material to reduce the internal impedance of the lithium-rich core, reduce the overpotential of the lithium supplement material, increase the decomposition rate of the lithium supplement material, increase the lithium ion conduction efficiency, and reduce the decomposition voltage of the lithium supplement material.
[0007] In one embodiment, the lithium-rich core is provided with a second channel, at least a portion of the first channel is connected to the second channel, the second channel is filled with a second functional material, and at least a portion of the first functional material is connected to the second functional material.
[0008] In one embodiment, along the thickness direction of the protective layer, all of the first channels and the second channels are connected, and the first functional material, the second functional material and the lithium-rich core are tightly connected.
[0009] In one embodiment, the second functional material is the same as the first functional material; and / or the first functional material and the second functional material each independently include one or more of a conductive material, an ion conductor material, and a catalyst.
[0010] In one embodiment, there are a plurality of the first channels, the plurality of the first channels extend along the circumference of the lithium-rich core, and at least two of the first channels are interconnected.
[0011] In one embodiment, the protective layer is an atomic layer deposition layer; and / or, the protective layer contains a transition metal oxide.
[0012] In one embodiment, the particle size D50 of the lithium-rich core is 500 nm to 50 μm.
[0013] In one embodiment, the protective layer has a thickness of 100 nm to 1 μm.
[0014] In one embodiment, the depth of the first channel is 100 nm to 1 μm.
[0015] In one embodiment, the second channel has a depth of 100 nm to 20 μm.
[0016] In one embodiment, the mass ratio of the lithium-rich core, the protective layer, and the functional material is 100:(5-30):(1-15), wherein the functional material is the sum of the masses of the first functional material and the second functional material.
[0017] In a second aspect, the present invention provides a method for preparing a composite lithium-replenishing material, comprising the following steps: wrapping a linear template on the outer layer of the lithium-rich core; coating the outer layer of the lithium-rich core with a protective material to form a protective layer, and exposing the linear template outside the protective layer; removing the linear template to form a first channel in the protective layer; depositing a first functional material in the first channel and then sintering to obtain a composite lithium-replenishing material.
[0018] The preparation method of the composite lithium-supplementing material provided by the present invention first combines a linear template with a lithium-rich core to form some specific patterns on the outer layer of the lithium-rich core, then forms a protective layer on the outer layer of the lithium-rich core, and then forms a first channel by removing the linear template, and deposits a first functional material in the first channel for sintering, so as to obtain a modified composite lithium-supplementing material with a protective layer. The first functional material in the composite lithium-supplementing material forms a conductive / or ion-conducting channel on the lithium-rich core, and the channel helps to improve the conductivity of the lithium-rich core, reduce the internal impedance of the lithium-rich core, reduce the overpotential, increase the decomposition rate of the lithium-rich core, improve the lithium ion conduction efficiency, and reduce the decomposition voltage of the lithium-rich core.
[0019] In a third aspect, the present invention further provides a positive electrode material, which includes a positive electrode active material and a lithium supplement material, wherein the lithium supplement material includes the lithium supplement material described in the first aspect, or the positive electrode material includes the lithium supplement material obtained by the preparation method of the lithium supplement material described in the second aspect.
[0020] In a fourth aspect, the present invention further provides a secondary battery, comprising a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises the positive electrode material described in the third aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0022] Figure 1 is a schematic diagram of the external appearance of a composite lithium supplement material according to an embodiment;
[0023] Figure 2 is a schematic diagram of the cross-sectional structure of a composite lithium supplement material according to an embodiment;
[0024] Figure 3 is a schematic diagram of the cross-sectional structure of a composite lithium supplement material according to another embodiment;
[0025] Figure 4 The present invention is a flow chart of a method for preparing a composite lithium supplement material according to an embodiment of the present invention;
[0026] Figure 5 yes Figure 4 A further flow chart of step S30;
[0027] Figure 6 yes Figure 4 Further flow chart of step S40 in FIG. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0029] It should be noted that when a component is said to be "fixed to" another component, it can be directly on the other component or there can be a central component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there can be a central component at the same time.
[0030] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in this application and in the specification are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this application includes any and all combinations of one or more of the related listed items.
[0031] In conjunction with the accompanying drawings, some embodiments of the present application are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.
[0032] The present invention provides a composite lithium supplement material, please refer to Figure 1 and Figure 2 , including a lithium-rich core 10 and a protective layer 20 , wherein the protective layer 20 is coated on the outer surface of the lithium-rich core 10 , and the protective layer 20 is provided with a first channel 21 , and the first channel 21 is filled with a first functional material 31 .
[0033] Specifically, the lithium-rich core 10 includes a lithium-rich material, which is the main body for lithium supplementation and can contribute a large amount of lithium ions. During the first charging process, the lithium (Li) in the lithium-rich material can be released and migrated to the negative electrode of the battery to offset the irreversible lithium loss caused by the formation of the SEI film, thereby increasing the total capacity and energy density of the battery. However, most of the existing commonly used lithium-rich materials have problems of poor conductivity and excessive internal impedance, resulting in excessively high decomposition voltage of the lithium-rich material and low lithium supplementation capacity. Therefore, how to solve the poor conductivity of lithium-rich materials and excessively high internal impedance has become the key.
[0034] In one embodiment, the lithium-rich material includes a ternary lithium-rich compound, the chemical formula of which includes Li x1 M y1 O z1, wherein M is at least one element selected from Fe, Ni, Mn, Cu, Zn, Co, Cr, Zr, Sb, Ti, V, Mo, and Sn, 1≤x1≤8, 0<y1, 0<z1<7. In a specific embodiment, the lithium-rich material may be Li5FeO4, Li6MnO4, Li6CoO4, Li6ZnO4, Li2NiO2, Li2CuO2, Li2CoO2, Li2MnO2, Li2Ni 0.5 Mn 1.5 O4、Li2Ni d Cu (1-d) At least one of O2 (0<d<1), etc.
[0035] In one embodiment, the lithium-rich material comprises a binary lithium-rich compound, the chemical formula of which comprises Li x2 M y2 , wherein M is one or more elements selected from S, P, I, Br, F, O, B, and Se, 1≤x2≤5, and 0<y2. In a specific embodiment, the lithium-rich material may be one or more selected from lithium sulfide (Li2S), lithium phosphide (Li3P), lithium iodide (LiI), and lithium bromide (LiBr).
[0036] In one embodiment, the lithium-rich material includes organic lithium-rich compounds, including but not limited to lithium oxalate (Li2C2O4), lithium squarate (Li2C6O6), lithium acetate (CH3COOLi), lithium triangular phosphate (Li2C3O3), lithium butynedioate (Li2C4O4), lithium acetonate (Li2C3O5), etc.
[0037] The lithium-rich materials mentioned above may be undoped or modified by doping, or may be surface coated, pre-lithiated, etc. When the lithium-rich materials are used as positive electrode active materials, they may also be a combination of the lithium-rich materials listed above and conventional positive electrode materials such as lithium iron phosphate and ternary positive electrode materials.
[0038] The lithium-rich materials mentioned above can all be used as the lithium-rich core 10 of the composite lithium-supplementing material provided by the present invention. The shape of the lithium-rich core 10 can be, but is not limited to, one or more of a sphere, a quasi-sphere, an ellipsoid, and a polyhedron. The outer surface of the lithium-rich core 10 is covered with a protective layer 20, and the protective layer 20 includes a transition metal oxide. The functions of the protective layer 20 include, but are not limited to, resisting external water vapor erosion, catalyzing the lithium-rich material to reduce voltage, improving the structural stability of the composite lithium-supplementing material, and reducing gas production.
[0039] Furthermore, a first channel 21 is formed on the outer surface of the protective layer 20. On the one hand, the first channel 21 extends toward the lithium-rich core 10 along the thickness direction of the protective layer 20, and on the other hand, the first channel 21 also extends along the circumference of the protective layer 20. The first channel 21 is filled with a first functional material 31, and the type of the first functional material 31 is not specifically limited.
[0040] In a specific embodiment, the first functional material 31 can be used to improve the conductivity or ion conductivity of the lithium-rich material in the lithium-rich core 10, help the lithium-rich material release lithium ions, and improve the lithium replenishment capacity of the composite lithium replenishment material; or, the first functional material 31 can be used to reduce the decomposition voltage of the lithium-rich material, so that the lithium-rich material in the lithium-rich core 10 can release lithium at a lower potential. Optionally, the first functional material 31 includes one or more of a conductive material, an ion conductor material, and a catalyst.
[0041] It can be understood that since the first channel 21 is formed on the outer surface of the protective layer 20, and the first functional material 31 is filled in the first channel 21. Therefore, from the outer surface of the composite lithium supplementing material, it can be seen that the first functional material 31 forms a texture on the protective layer 20, and the path of the texture is the same as the path of the first channel 21. In a specific embodiment, since the first functional material 31 fills the first channel 21, the concave first channel 21 may not be directly seen from the protective layer 20, but the texture extending from the first functional material 31 can be obtained.
[0042] Optionally, in a specific embodiment, part of the first channel 21 is opened on the outer surface of the protective layer 20 and penetrates the inner wall surface of the protective layer 20, that is, the bottom wall of the first channel 21 can be the outer surface of the lithium-rich core 10; the first functional material 31 in the first channel 21 is connected to the outer surface of the lithium-rich core 10. In other specific embodiments, part of the first channel 21 is opened on the outer surface of the protective layer 20, penetrates the inner wall surface of the protective layer 20, and also penetrates into the lithium-rich core 10, that is, part of the first channel 21 is also formed on the lithium-rich core 10; the first functional material 31 in the first channel 21 is connected to the inside of the lithium-rich core 10. In other specific embodiments, part of the first channel 21 is opened on the outer surface of the protective layer 20, but does not penetrate the protective layer 20, and the first functional material 31 is not directly connected to the lithium-rich core 10.
[0043] Optionally, in a specific embodiment, the first functional material 31 is filled in the first channel 21, that is, it is difficult to observe obvious traces of the first channel 21 on the composite lithium supplementing material, but the first functional material 31 forms a curved and extended pattern on the protective layer 20. In other specific embodiments, the first functional material 31 can also be combined on the inner wall of the first channel 21, and the first channel 21 is not completely filled with the first functional material 31, that is, obvious traces of the first channel 21 (groove) can be observed on the composite lithium supplementing material.
[0044] The present invention provides a composite lithium-supplementing material, which includes a lithium-rich core 10 and a protective layer 20 coated on its outer layer, wherein a first channel 21 is opened on the protective layer, and the first channel 21 is filled with a first functional material 31. Through the lines formed by the first channel 21 and the first functional material 31, a conductive / or ion-conducting channel is formed on the lithium-rich core 10, and the channel helps to improve the conductivity of the lithium-rich core 10, reduce the internal impedance of the lithium-rich core 10, reduce the overpotential, increase the decomposition rate of the lithium-rich core 10, improve the lithium ion conduction efficiency, and reduce the decomposition voltage of the lithium-rich core 10.
[0045] In one implementation, please refer to Figure 3 The lithium-rich core 10 is provided with a second channel 11 , at least part of the first channel 21 is connected to the second channel 11 , the second channel 11 is filled with a second functional material 32 , and at least part of the first functional material 31 is connected to the second functional material 32 .
[0046] Specifically, a second channel 11 is provided on the outer surface of the lithium-rich core 10, and at least a portion of the first channel 21 is connected to the second channel 11 in the thickness direction of the protective layer 20, so the second functional material 32 is connected to the first functional material 31. The second functional material 32 and the first functional material 31 together form the above-mentioned conductive / ion-conducting channel.
[0047] In a specific embodiment, the types of the second functional material 32 and the first functional material 31 can be the same or different. Of course, the second functional material 32 can also be used to improve the conductivity or ion conductivity of the lithium-rich material in the lithium-rich core 10, help the lithium-rich core 10 release lithium ions, and improve the lithium replenishment capacity of the composite lithium replenishment material; or, the second functional material 32 can be used to reduce the decomposition voltage of the lithium-rich core 10, so that the lithium-rich material in the lithium-rich core 10 can release lithium at a lower potential.
[0048] By opening a second channel 11 connected to the first channel 21 on the lithium-rich core 10, the lithium-rich core 10 and the second functional material 32 are fully connected. The conductive or ion-conducting channel formed by the second functional material 32 in the second channel 11 can improve the conductivity or ion conductivity of the lithium-rich core 10, reduce the internal impedance and overpotential of the lithium-rich core 10, and allow the capacity of the lithium-rich core 10 to be fully released.
[0049] In one implementation, please refer to Figure 3 Along the thickness direction of the protective layer 20 , all the first channels 21 and the second channels 11 are connected, and the first functional material 31 and the second functional material 32 are tightly connected to the lithium-rich core 10 .
[0050] Specifically, the first channel 21 on the protective layer 20 not only penetrates the protective layer 20 but also penetrates into the lithium-rich core 10, that is, the second channel 11 is formed, so all the first channels 21 and the second channels 11 are connected, and the inner wall of the first channel 21 and the inner wall of the second channel 11 are smoothly connected.
[0051] In one embodiment, the second channel 11 is also filled with a portion of lithium-rich material, and the lithium-rich material and the second functional material 32 form an interface connection in the second channel 11. Specifically, the lithium-rich material in the second channel 11 is uniformly mixed with the second functional material 32, and the lithium-rich material and the second functional material 32 form an interface connection.
[0052] By providing the lithium-rich material in the second channel 11 and the second functional material 32 to form an interface connection, and forming the second functional material 32 doping in the lithium-rich core 10, the conductivity of the lithium-rich core can be further improved, and the internal impedance of the lithium-rich core can be reduced.
[0053] In one embodiment, the second functional material 32 is the same as the first functional material 31; and / or the first functional material 31 and the second functional material 32 respectively and independently include one or more of a conductive material, an ion conductor material, and a catalyst.
[0054] Specifically, the second functional material 32 and the first functional material 31 may be the same functional material. When the first channel 21 and the second channel 11 are completely connected, the second functional material 32 and the first functional material 31 may be obtained by the same preparation process.
[0055] Optionally, the first functional material 31 and / or the second functional material 32 include a conductive material, which may be, but not limited to, one or more of a carbon material, a metal material, an alloy material, and a conductive polymer material. Optionally, the first functional material 31 and / or the second functional material 32 include an ion conductor material, which may be, but not limited to, a solid electrolyte and / or a fast ion conductor. Optionally, the first functional material 31 and / or the second functional material 32 include a catalyst, which may be, but not limited to, one or more of a metal oxide, a metal carbide, a metal sulfide, and a metal nitride.
[0056] In one implementation, please refer to Figure 1 and Figure 2 , the number of the first channels 21 is multiple, the multiple first channels 21 extend along the circumference of the lithium-rich core 10, and at least two first channels 21 are interconnected. Specifically, multiple staggered first channels 21 are opened on the protective layer 20, and at least two first channels 21 are interconnected. It can be understood that the first functional material 31 forms multiple curved and extended lines on the protective layer 20, and at least two lines intersect.
[0057] In one embodiment, the protective layer 20 is an atomic layer deposition layer; and / or, the protective layer 20 includes a transition metal oxide.
[0058] Specifically, the protective layer 20 is coated on the outer surface of the lithium-rich core 10 by atomic layer deposition technology (ALD technology). The ALD technology deposits the transition metal oxide layer by layer on the surface of the lithium-rich core 10 in the form of a single atomic film, thereby achieving the purpose of accurately controlling the thickness and quality of the protective layer 20. The ALD technology can achieve atomic-level precision film thickness control with excellent repeatability and uniformity. In a specific embodiment, the first functional material 31 and the second functional material 32 can be deposited in the first channel 21 by the ALD technology.
[0059] Optionally, the chemical formula of the transition metal oxide includes A a O b , wherein 1≤a≤3, 1≤b≤5, A includes one or more of W, Mo, Ni, Co, Nb, Ge, Al, Mn, Ti, Mg. Specifically, the transition metal oxide can be WO3, MoO3, NiO2, CoO2, Nb2O5, GeO2, Al2O3, MnO, TiO2 or MgO, etc., without specific limitation. The above transition metal oxides are used as a protective layer 20, not only to protect the lithium-rich core 10, but also as a catalyst to catalyze high-voltage lithium-rich materials to reduce the decomposition voltage, thereby ensuring that the lithium-rich core 10 can fully release its capacity.
[0060] In one embodiment, the particle size D50 of the lithium-rich core 10 is 500nm-50μm, and further optionally, the particle size D50 of the lithium-rich core 10 is 5μm-50μm. Optionally, the particle size D50 of the lithium-rich core 10 can be 500nm, 800nm, 1μm, 2μm, 5μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm.
[0061] The particle size D50 of the lithium-rich core 10 is within the above range, which is conducive to the processing of the lithium-rich core 10 and ensuring the transmission rate of lithium ions, and makes the composite lithium-supplementing material and the positive electrode active material well adapted. When the particle size D50 of the lithium-rich core 10 is less than the above range, the dispersibility of the lithium-rich core 10 is poor, which easily causes particle agglomeration and is not conducive to the coating of transition metal oxides; when the particle size D50 of the lithium-rich core 10 is greater than the above range, the lithium-rich core 10 is too large, which is not conducive to the complete release of lithium ions inside the lithium-rich core 10, and also causes the particle size of the composite lithium-supplementing material to increase accordingly, making it difficult to adapt to the positive electrode active material.
[0062] In one embodiment, the thickness of the protective layer 20 is 100 nm to 1 μm. Optionally, the thickness of the protective layer 20 may be 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, or 1 μm.
[0063] Meeting the thickness of the protective layer 20 within the above range is conducive to ensuring the lithium replenishment capacity of the composite lithium replenishment material and improving the structural stability of the protective layer 20, and reducing the difficulty of preparing the protective layer 20. When the thickness of the protective layer 20 is less than the above range, the protective layer 20 is too thin, the structural stability of the protective layer 20 is reduced, and the deposition requirements of the ALD technology are higher; when the thickness of the protective layer 20 is greater than the above range, the protective layer 20 is too thick, the path of lithium ions passing through the protective layer 20 is increased, the lithium ions are not fully released, and the lithium replenishment capacity is reduced.
[0064] In one embodiment, the depth of the first channel 21 is 100nm to 1μm. Optionally, the depth of the first channel 21 can be 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, or 1μm. It should be noted that the depth of the first channel 21 refers to the depth of the first channel 21 opened or etched, that is, the distance range from the highest point on the outer surface of the protective layer 20 to the lowest point in the first channel 21.
[0065] The depth of the first channel 21 is within the above range to ensure that the first channel 21 penetrates the protective layer 20 so that the first functional material 31 is connected to the lithium-rich core 10, thereby improving the conductivity of the lithium-rich core 10. When the depth of the first channel 21 is less than the above range, the first channel 21 is too shallow, and the first functional material 31 in the first channel 21 cannot be connected to the lithium-rich core 10, resulting in insufficient connection between the first functional material 31 and the lithium-rich core 10.
[0066] In one embodiment, the depth of the second channel 11 is 100nm to 20μm, and further optionally, the depth of the second channel 11 is 1μm to 20μm. Optionally, the depth of the second channel 11 can be 100nm, 200nm, 500nm, 1μm, 2μm, 4μm, 6μm, 8μm, 10μm, 12μm, 14μm, 16μm, 18μm, 20μm. It should be noted that the depth of the second channel 11 refers to the depth of the second channel 11 opened or etched, that is, the distance range from the highest point on the outer surface of the lithium-rich core 10 to the lowest point in the second channel 11.
[0067] The depth of the second channel 11 is within the above range to ensure that the second functional material 32 and the lithium-rich core 10 form a sufficient interface connection, thereby improving the conductivity of the lithium-rich core 10. When the depth of the second channel 11 is less than the above range, the second channel 11 is too shallow, and the second functional material 32 in the second channel 11 and the lithium-rich core 10 are not fully connected; when the depth of the second channel 11 is greater than the above range, the structure of the lithium-rich core 10 is destroyed, which not only reduces the lithium replenishment capacity but also causes the structural stability of the lithium-rich core 10 to deteriorate.
[0068] In one embodiment, the mass ratio of the lithium-rich core 10 , the protective layer 20 , and the functional material is 100:(5-30):(1-15), wherein the functional material is the sum of the masses of the first functional material 31 and the second functional material 32 . Optionally, the mass ratio of the lithium-rich core 10, the protective layer 20, and the functional material can be 100:(5-30):1, 100:(5-30):3, 100:(5-30):5, 100:(5-30):7, 100:(5-30):9, 100:(5-30):11, 100:(5-30):13, 100:(5-30):15, 100:5:(1-15), 100:10:(1-15), 100:15:(1-15), 100:20:(1-15), 100:25:(1-15), and 100:30:(1-15).
[0069] When the mass ratio of the three is within the above range, on the one hand, the capacity of the composite lithium supplement material can be ensured, and on the other hand, the protective layer 20 can be ensured to completely cover the lithium-rich core 10, and the functional materials can fully play their role. When the mass ratio of the protective layer 20 or the functional material is less than the above range, it is difficult for the protective layer 20 to achieve complete coverage, or the protective layer 20 will be too thin, and it will also result in less functional materials and fail to effectively improve the conductivity of the lithium-rich core 10; when the mass ratio of the protective layer 20 or the functional material is greater than the above range, the lithium-rich core 10 accounts for a small proportion, and the lithium supplement capacity of the composite lithium supplement material is affected.
[0070] In one embodiment, the present invention provides a method for preparing a composite lithium supplement material, please refer to Figure 4 , including the following steps:
[0071] Step S10, wrapping the linear template on the outer surface of the lithium-rich core.
[0072] Step S20, coating the outer surface of the lithium-rich core with a protective material to form a protective layer, and making the linear template exposed outside the protective layer.
[0073] Step S30, removing the linear template to form a first channel in the protection layer.
[0074] Step S40, depositing the first functional material in the first channel and then performing a sintering process to obtain a composite lithium supplementing material.
[0075] Specifically, in step S10, the linear template is wrapped on the outer layer of the lithium-rich core, which specifically includes: using lithium-rich material particles as the lithium-rich core, combining the linear template on the outer surface of the lithium-rich core by a liquid phase method, and the linear template forms specific patterns on the outer surface of the lithium-rich core.
[0076] Optionally, the linear template is a linear polymer material, specifically including but not limited to polystyrene, polymethyl methacrylate, nylon, polyethylene, polypropylene, polyurethane, etc., without specific limitation. It can be understood that the molecular chains of the linear polymer are arranged linearly, so when the linear polymer is combined on the surface of the lithium-rich core, a linear staggered pattern can be presented.
[0077] After performing step S10, the obtained material is a composite of a lithium-rich core (lithium-rich material) and a linear template (polymer material), wherein the linear template is distributed on the outer surface of the lithium-rich core and forms linear patterns. Therefore, part of the outer surface of the lithium-rich core is still exposed without being combined with the linear template.
[0078] Furthermore, in step S20, a protective material is coated on the outer surface of the lithium-rich core to form a protective layer, specifically comprising: depositing a protective layer of transition metal oxide on the surface of the lithium-rich core by ALD technology.
[0079] It should be explained that ALD technology is an atomic-level deposition technology, which is deposited by reaction of transition metal oxide precursors in a specific instrument. However, the characteristic of this technology is that the obtained transition metal oxide cannot be deposited on polymer materials. Therefore, based on step S10, the transition metal oxide is mainly deposited on the outer surface of the lithium-rich core where the linear template is not bound.
[0080] It can be understood that since the area of the linear template bound on the outer surface of the lithium-rich core is smaller than the area of the deposited transition metal oxide, it can be regarded as the linear template embedded in the protective layer, and the protective layer forms a discontinuous layer structure, and the linear template is exposed to the external environment.
[0081] Then, in step S30, the linear template is removed, specifically including: treating the lithium-rich core with the protective layer with an organic solvent, washing away the linear template with the organic solvent to obtain an incompletely coated lithium-rich core, and forming a first channel on the protective layer.
[0082] Optionally, the organic solvent for removing the template includes, but is not limited to, ethanol, acetone, ethyl acetate, tetrahydrofuran, dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, etc. It is understandable that the choice of the organic solvent is not specifically limited and can be adapted according to the selected linear template agent.
[0083] It can be understood that the linear template of the polymer material can be dissolved in organic solvents, while the transition metal oxide cannot be dissolved in organic solvents, so the organic solvent only washes away the linear template on the protective layer. After removing the linear template, the space originally occupied by the linear template is exposed to form a channel.
[0084] Secondly, in step S40, after depositing the first functional material in the first channel, a sintering process is performed, which specifically includes: continuing to deposit the first functional material in the channel by ALD technology, and then sintering to combine the materials in the channel, and obtaining a composite lithium supplement material after the channel is healed.
[0085] The first functional material is deposited in the channel by using the ALD technology for the second time. On the one hand, it is to set up a conductive channel formed by the first functional material; on the other hand, the first functional material deposited by the ALD technology is small in volume, easier to fill in the channel, and easier to combine with the transition metal oxide deposited by the same ALD; on the other hand, the ALD technology can deposit the first functional material in a controllable manner and can adapt to the channel to avoid the first functional material from overflowing and destroying the protective layer of the transition metal oxide.
[0086] In one implementation, please refer to Figure 5In step S30, the linear template is removed to form a first channel in the protective layer, which specifically includes the following steps:
[0087] Step S31, washing away the linear template with an organic solvent to form a first channel on the protective layer to obtain an intermediate material, wherein the linear template includes a linear high molecular polymer.
[0088] Step S32, etching the intermediate material with an etching solution to form a second channel on the outer surface of the lithium-rich core, and the first channel and the second channel are connected.
[0089] Specifically, in step S32, the intermediate material is etched by an etching solution, specifically including: placing the intermediate material in an ALD deposition device, evacuating to 0.1 torr, introducing a specially prepared dilute water vapor, and controlling the depth of water etching by controlling the water introduction time, wherein the dilute water vapor is obtained by mixing water vapor and nitrogen, the water content is 0.1ppm to 10ppm, and the water vapor is introduced by nitrogen at a flow rate of 50ml / min to 500ml / min. In a specific embodiment, the time for treating the lithium-rich material with the dilute water vapor is related to the mass of the lithium-rich material, and can be 6s / g to 60s / g.
[0090] In other embodiments, the etching solution may also be some hydroxyl-containing solutions, such as ammonia water, ethanol, etc. Therefore, in a specific embodiment, the introduced special dilute water vapor may also be replaced by dilute ammonia water or ethanol, etc.
[0091] It should be explained that due to the particularity of the physicochemical properties of lithium-rich materials, in the existing technical solutions, when using lithium-rich materials to prepare composite lithium-supplementing materials, the lithium-rich materials are prevented from contacting with water or hydroxyl-containing solutions. The present invention uses an etching solution to treat the surface of the lithium-rich core because, after removing the linear template, most of the surface of the lithium-rich core is coated with transition metal oxides, and water will enter the channel along the uncoated lines, and decompose the lithium-rich material along the position of the lines to the inside of the lithium-rich core, so that the lithium-rich core forms a second channel from the outer surface (that is, the channel is deepened at the position of the original channel).
[0092] It is understandable that etching the lithium-rich core with an etching solution requires strict control of the etching time and etching dosage to avoid over-etching or under-etching. Over-etching will damage the structure of the lithium-rich core and most of the lithium-rich core will fail; under-etching will cause the channel to be too shallow or fail to form a channel on the lithium-rich core.
[0093] In one implementation, please refer to Figure 6In step S40, after depositing the first functional material in the first trench, a sintering process is performed, which specifically includes the following steps:
[0094] Step S41, depositing the second functional material in the second channel, and depositing the first functional material in the first channel.
[0095] Step S42, after sintering, the first functional material, the second functional material and the lithium-rich core are tightly connected.
[0096] Furthermore, in step S41, since the lithium-rich core is etched, the second functional material can enter the lithium-rich core, and during the sintering process of the material, the substance (compounds containing lithium and transition metals) formed by the etching solution is sintered in situ to reform the lithium-rich material, so that the channel on the lithium-rich core is healed, and at the same time, the interface formed by the lithium-rich material and the second functional material deposited in the second channel is connected.
[0097] It needs to be explained that in the prior art, the use of ALD technology on different materials faces the problem of reliability of the combination of the two. That is, the stability of the combination of the first functional material on the lithium-rich core. If the first functional material is simply filled in the channel and connected to the inner wall of the channel (i.e., the lithium-rich core), the improvement of the material conductivity is limited. Therefore, it is particularly important to make the first functional material and the lithium-rich material form a close connection in the ALD technology.
[0098] The present invention uses an etching solution to etch the lithium-rich core in step S32, which can not only produce the second channel as described above, but also decompose the lithium-rich material. Based on the particularity of the lithium-rich material, the lithium-rich material will quickly decompose to form lithium-containing compounds and transition metal compounds after reacting with the etching solution. Such compounds will also remain in the channel. After the second functional material is deposited by the ALD technology, the second functional material is mixed with such compounds. Through the key step of sintering, the lithium-containing compound and the transition metal compound are dehydrated again to form a lithium-rich material, and the lithium-rich material and the second functional material form a tight interface connection.
[0099] The preparation method of the composite lithium-supplementing material provided by the present invention first combines a linear template with a lithium-rich core to form some specific patterns on the outer layer of the lithium-rich core, then forms a protective layer on the outer layer of the lithium-rich core, and then forms a first channel by removing the linear template, and deposits a first functional material in the first channel for sintering, so as to obtain a modified composite lithium-supplementing material with a protective layer. The first functional material in the composite lithium-supplementing material forms a conductive / or ion-conducting channel on the lithium-rich core, and the channel helps to improve the conductivity of the lithium-rich core, reduce the internal impedance of the lithium-rich core, reduce the overpotential, increase the decomposition rate of the lithium-rich core, improve the lithium ion conduction efficiency, and reduce the decomposition voltage of the lithium-rich core.
[0100] In addition, the present invention further etches a second channel on the lithium-rich core by combining atomic layer deposition and etching with an etching solution, and utilizes sintering to allow the lithium-rich material after etching and decomposition to be sintered in situ to reform the lithium-rich material. The lithium-rich material in the second channel forms a tight interface connection with the second functional material, and the second functional material is doped in the lithium-rich core, thereby further improving the conductivity of the conductive and / or ion-conducting channel formed by the second functional material and reducing the internal impedance of the lithium-rich material.
[0101] In one embodiment, the present invention further provides a positive electrode material, the positive electrode material includes a positive electrode active material and a lithium supplement material. The lithium supplement material is the lithium supplement material provided in the above embodiment. Optionally, the positive electrode active material can be a phosphate positive electrode active material or a ternary positive electrode active material. In a specific embodiment, the positive electrode active material includes one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium oxyphosphate, lithium fluorinated vanadium phosphate, lithium titanate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide.
[0102] In one embodiment, the content of lithium-supplementing material in the positive electrode material can be controlled at 1% to 6% of the mass of the positive electrode active material. This ratio can just make up for the loss of active lithium in the battery during the first charging process. If the amount of lithium-supplementing material added to the positive electrode material is too low, the active lithium lost in the positive electrode active material cannot be fully replenished, which is not conducive to improving the energy density and capacity retention rate of the battery. If the amount of lithium-supplementing material added to the positive electrode active material is too high, the original reversible capacity will be occupied and the cost will be increased. In some specific embodiments, in the positive electrode material, the mass percentage of the lithium-supplementing material can be 1%, 2%, 4%, 6%, etc.
[0103] In one embodiment, the present invention further provides a positive electrode plate, the positive electrode plate includes a current collector and an active material layer disposed on the current collector, the active material layer includes the lithium supplement material of any one of the above embodiments. Or the active material layer includes the lithium supplement material obtained by the preparation method of the lithium supplement material in the above embodiments.
[0104] In one embodiment, the positive electrode sheet includes a positive electrode current collector, and the positive electrode current collector has a positive electrode active layer, and the positive electrode active layer includes components such as positive electrode active materials, lithium supplement materials, conductive agents, and binders. The present invention does not specifically limit these materials, and suitable materials can be selected according to actual application requirements. The positive electrode current collector includes but is not limited to any one of copper foil and aluminum foil. The conductive agent includes one or more of graphite, carbon black, acetylene black, graphene, carbon fiber, C60 and carbon nanotubes, and the content of the conductive agent in the positive electrode active layer is 3wt% to 5wt%. The types of binders include polyvinylidene chloride, soluble polytetrafluoroethylene, styrene-butadiene rubber, hydroxypropyl methylcellulose, methylcellulose, carboxymethyl cellulose, polyvinyl alcohol, acrylonitrile copolymer, sodium alginate, chitosan and chitosan derivatives, and the content of the binder in the positive electrode active layer is 2wt% to 4wt%.
[0105] In one embodiment, the present invention further provides a secondary battery, the secondary battery comprising a negative electrode, a positive electrode and an electrolyte, wherein the positive electrode comprises the above-mentioned positive electrode material; the electrolyte may be an electrolyte solution, in which case the secondary battery further comprises a diaphragm disposed between the positive electrode plate and the negative electrode plate; or, the electrolyte may be a solid electrolyte solution, in which case the secondary battery does not have a diaphragm and is replaced by a solid electrolyte.
[0106] The technical solution of the present invention is described in detail below through specific embodiments.
[0107] Example 1
[0108] This embodiment provides a composite lithium supplement material. The composite lithium supplement material includes a lithium-rich core and a protective layer, the protective layer is coated on the outer surface of the lithium-rich core, the lithium-rich core includes Li6CoO4, and the protective layer includes TiO2. A first channel is opened on the protective layer, and a second channel is opened on the lithium-rich core. The first channel and the second channel are completely connected, and the first channel and the second channel are filled with the same functional material (Ag).
[0109] Among them, the particle size D50 of the lithium-rich core is 30μm, the thickness of the protective layer is about 500nm, the depth of the first channel is about 500nm, the depth of the second channel is about 8μm, and the mass ratio of the lithium-rich core, the protective layer and the functional material is 100:15:5.
[0110] The preparation method of the composite lithium supplement material comprises the following steps:
[0111] 1) Through liquid phase coating, a linear polymer template (polystyrene) is combined with the surface of Li6CoO4 to form a specific texture, and then the transition metal oxide TiO2 is deposited on the surface of Li6CoO4 through ALD metal, and then the template is washed away by the organic solvent NMP to obtain an incompletely coated lithium-rich core.
[0112] 2) The lithium-rich core with the protective layer is etched by water etching, and the Li6CoO4 in the lithium-rich core is destroyed by water along the grooves.
[0113] 3) Depositing functional materials in the first channel and the second channel by ALD technology.
[0114] 4) The material formed by water etching and decomposition is sintered in situ through high temperature sintering to reform Li6CoO4, so that the second channel on the lithium-rich core is healed, and at the same time, the functional material at the second channel forms an interface contact with Li6CoO4 to obtain a composite lithium supplement material.
[0115] Example 2
[0116] This embodiment provides a composite lithium supplement material. The composite lithium supplement material includes a lithium-rich core and a protective layer, the protective layer is coated on the outer surface of the lithium-rich core, a first channel is opened on the protective layer, a second channel is opened on the lithium-rich core, the first channel and the second channel are completely connected, and the first channel and the second channel are both filled with functional materials.
[0117] The difference between the second embodiment and the first embodiment is that the depth of the second trench is about 1 μm.
[0118] Example 3
[0119] This embodiment provides a composite lithium supplement material. The composite lithium supplement material includes a lithium-rich core and a protective layer, the protective layer is coated on the outer surface of the lithium-rich core, a first channel is opened on the protective layer, a second channel is opened on the lithium-rich core, the first channel and the second channel are completely connected, and the first channel and the second channel are both filled with functional materials.
[0120] The difference between the present embodiment 3 and the embodiment 1 is that the depth of the second trench is about 20 μm.
[0121] Example 4
[0122] This embodiment provides a composite lithium supplement material. The composite lithium supplement material includes a lithium-rich core and a protective layer, the protective layer is coated on the outer surface of the lithium-rich core, a first channel is opened on the protective layer, a second channel is opened on the lithium-rich core, the first channel and the second channel are completely connected, and the first channel and the second channel are both filled with functional materials.
[0123] The difference between Example 4 and Example 1 is that the thickness of the protective layer is about 100 nm, the depth of the first channel is about 100 nm, and the mass ratio of the lithium-rich core, the protective layer and the functional material is 100:5:1.
[0124] Example 5
[0125] This embodiment provides a composite lithium supplement material. The composite lithium supplement material includes a lithium-rich core and a protective layer, the protective layer is coated on the outer surface of the lithium-rich core, a first channel is opened on the protective layer, a second channel is opened on the lithium-rich core, the first channel and the second channel are completely connected, and the first channel and the second channel are both filled with functional materials.
[0126] The difference between Example 5 and Example 1 is that the thickness of the protective layer is about 1 μm, the depth of the first channel is about 1 μm, and the mass ratio of the lithium-rich core, the protective layer and the functional material is 100:30:15.
[0127] Example 6
[0128] This embodiment provides a composite lithium supplement material. The composite lithium supplement material includes a lithium-rich core and a protective layer, the protective layer is coated on the outer surface of the lithium-rich core, a first channel is opened on the protective layer, a second channel is opened on the lithium-rich core, the first channel and the second channel are completely connected, and the first channel and the second channel are both filled with functional materials.
[0129] The difference between Example 6 and Example 1 is that the particle size D50 of the lithium-rich core is 5 μm.
[0130] Example 7
[0131] This embodiment provides a composite lithium supplement material. The composite lithium supplement material includes a lithium-rich core and a protective layer, the protective layer is coated on the outer surface of the lithium-rich core, a first channel is opened on the protective layer, a second channel is opened on the lithium-rich core, the first channel and the second channel are completely connected, and the first channel and the second channel are both filled with functional materials.
[0132] The difference between Example 7 and Example 1 is that the particle size D50 of the lithium-rich core is 50 μm.
[0133] Example 8
[0134] This embodiment provides a composite lithium supplement material, which includes a lithium-rich core and a protective layer, wherein the protective layer is coated on the outer surface of the lithium-rich core, a first channel is formed on the protective layer, and the first channel is filled with a first functional material (Ag).
[0135] The difference between Example 8 and Example 1 is that the second channel is not opened on the lithium-rich core, and in the preparation method, step 2) is not performed.
[0136] Example 9
[0137] This embodiment provides a composite lithium supplement material. The composite lithium supplement material includes a lithium-rich core and a protective layer, the protective layer is coated on the outer surface of the lithium-rich core, a first channel is opened on the protective layer, a second channel is opened on the lithium-rich core, the first channel and the second channel are completely connected, and the first channel and the second channel are both filled with functional materials.
[0138] The difference between this embodiment 9 and embodiment 1 is that the protective layer includes ZrO2.
[0139] Example 10
[0140] This embodiment provides a composite lithium supplement material. The composite lithium supplement material includes a lithium-rich core and a protective layer, the protective layer is coated on the outer surface of the lithium-rich core, a first channel is opened on the protective layer, a second channel is opened on the lithium-rich core, the first channel and the second channel are completely connected, and the first channel and the second channel are both filled with functional materials.
[0141] The difference between Example 10 and Example 1 is that the functional material is ZnO.
[0142] Embodiment 11
[0143] This embodiment provides a composite lithium supplement material. The composite lithium supplement material includes a lithium-rich core and a protective layer, the protective layer is coated on the outer surface of the lithium-rich core, a first channel is opened on the protective layer, a second channel is opened on the lithium-rich core, the first channel and the second channel are completely connected, the first channel is filled with a first functional material (Ag), and the second channel is filled with a second functional material (ZnO).
[0144] The difference between this embodiment 11 and embodiment 1 is that the first functional material and the second functional material are different.
[0145] Example 12
[0146] This embodiment provides a composite lithium supplement material. The composite lithium supplement material includes a lithium-rich core and a protective layer, the protective layer is coated on the outer surface of the lithium-rich core, a first channel is opened on the protective layer, a second channel is opened on the lithium-rich core, the first channel and the second channel are completely connected, and the first channel and the second channel are both filled with functional materials.
[0147] The difference between this embodiment 12 and embodiment 1 is that the lithium-rich core includes Li2NiO2.
[0148] Comparative Example 1
[0149] This comparative example provides a lithium-rich material (Li6CoO4).
[0150] Comparative Example 2
[0151] This comparative example provides a composite lithium supplement material, which includes a simple mixture of Li6CoO4, a transition metal oxide, and a functional material.
[0152] Comparative Example 3
[0153] This comparative example provides a composite lithium supplement material, which includes a lithium-rich core and a protective layer, wherein the protective layer is coated on the outer surface of the lithium-rich core, the lithium-rich core includes Li6CoO4, and the protective layer includes TiO2.
[0154] The parameters of the composite lithium supplement materials provided by Examples 1 to 12 and Comparative Examples 1 to 3 are shown in Table 1:
[0155] Table 1 Parameters of composite lithium supplement materials provided in Examples and Comparative Examples
[0156]
[0157] In Table 1, parameter A is the particle size D50 of the lithium-rich core, parameter B is the thickness of the protective layer, parameter C is the depth of the first channel, parameter D is the depth of the second channel, and parameter E is the mass ratio of the lithium-rich core, the protective layer and the functional material.
[0158] The composite lithium supplement materials provided in the above-mentioned Examples 1 to 12 and the composite lithium supplement materials provided in Comparative Examples 1 to 3 are respectively assembled into positive electrode sheets and lithium-ion batteries according to the following methods:
[0159] Positive electrode sheet: The composite lithium supplement material, SP and PVDF are mixed in a mass ratio of 90:4:6 to form a positive electrode slurry, the positive electrode slurry is coated on the surface of aluminum foil, vacuum dried at 110°C overnight, and rolled to obtain a positive electrode sheet;
[0160] Negative electrode: lithium sheet;
[0161] Electrolyte: Ethylene carbonate and ethyl methyl carbonate were mixed in a volume ratio of 3:7, and LiPF6 was added to form an electrolyte, and the concentration of LiPF6 was 1 mol / L;
[0162] Diaphragm: Polypropylene microporous separator;
[0163] Lithium-ion battery assembly: Assemble button-type lithium-ion full batteries in an inert atmosphere glove box in the order of negative electrode sheet - separator - electrolyte - positive electrode sheet.
[0164] The electrochemical performance of each lithium-ion battery assembled in the above lithium-ion battery embodiment was tested under the following test conditions:
[0165] The battery was charged at a rate of 0.1C with a cut-off voltage of 4.7V; constant voltage charging was performed at a cut-off voltage of 4.7V; after the charging process was completed, the battery was allowed to stand for 10 minutes and then discharged at a rate of 0.1C with a cut-off voltage of 2.5V; the charging platform was observed during the charging process to obtain the decomposition voltage of the composite lithium supplement material; and the first cycle efficiency = (charge specific capacity / discharge specific capacity)*100%.
[0166] The test results of the above composite lithium supplement material and lithium battery are shown in Table 2 below:
[0167] Table 2. Test results of embodiments and comparative examples
[0168]
[0169] From the test results of Example 1 and Comparative Examples 1 to 3 in Table 2, it can be seen that by modifying Li6CoO4 using the method of Example 1, the capacity of the lithium supplement material can be greatly improved, and the decomposition voltage of the lithium supplement material can be reduced. Due to the presence of the coating layer, the structural stability of the lithium supplement material is enhanced, and the volume change rate of the pole piece can also be reduced. In addition, the transition metal oxide in the coating layer can reduce the decomposition voltage of the material, and the functional material can reduce the impedance of the material, so that Example 1 shows that the capacity of its composite lithium supplement material is improved and the discharge specific capacity is reduced.
[0170] From the test results of Examples 1 to 3 in Table 2, it can be seen that the depth of the second channel has a great influence on the performance of the composite lithium supplement material. When the depth of the second channel is too shallow, the embedding depth of the functional material in the lithium-rich core is insufficient, and the effect of reducing the decomposition voltage and improving the conductivity of the material cannot be fully exerted; when the depth of the second channel is too deep, the structure of the lithium-rich core will be destroyed, so that when the lithium-rich core decomposes, the protective layer cannot maintain its original structure, resulting in a large change rate of the electrode.
[0171] From the test results of Example 1, Example 4 and Example 5 in Table 2, it can be seen that the thickness of the protective layer has a great influence on the performance of the composite lithium supplement material. When the thickness of the protective layer is too small, the proportion of the protective layer and the functional material is also small, and the performance of the composite lithium supplement material is not significantly improved, including capacity, decomposition voltage, and a decrease in the volume change rate of the pole piece. This is because the proportion of the functional material is too small, which makes it impossible to play its due role, and also causes the structure of the composite lithium supplement material to be destroyed, so that when the composite lithium supplement material decomposes, the protective layer cannot maintain the original structure, resulting in an increase in the pole piece change rate; when the thickness of the protective layer is too large, the proportion of the protective layer and the functional material is too large. Although the pole piece change rate can be greatly reduced, the effect on the decomposition voltage of the lithium-rich core becomes smaller, and due to the relative mass of the composite lithium supplement material is reduced, the capacity of the pole piece will decrease, but it will cause incomplete decomposition of the composite lithium supplement material and a decrease in the capacity of the composite lithium supplement material.
[0172] From the test results of Example 1, Example 6 and Example 7 in Table 2, it can be learned that the particle size of the lithium-rich core has a great influence on the performance of the composite lithium-supplementing material, and the influence of the particle size of the lithium-rich core is similar to the combination of the influence of the second channel depth and the influence of the thickness of the protective layer. When the particle size of the lithium-rich core is too small, the depth of the second channel is too large relative to the core, and the thickness of the protective layer is too large, making it difficult for the lithium-rich core to fully decompose and release capacity. Although the decomposition voltage is low, it will cause the structure of the composite lithium-supplementing material to be destroyed, so that when the composite lithium-supplementing material decomposes, the protective layer cannot maintain the original structure, resulting in an increase in the rate of change of the pole piece. When the particle size of the lithium-rich core is too large, the depth of the second channel is too small relative to the core, and the thickness of the protective layer is too small, which will cause the decomposition voltage to increase, the capacity of the lithium-rich core is limited, and the rate of change of the pole piece volume will increase.
[0173] From the test results of Example 1 and Example 8 in Table 2, it can be seen that if the composite lithium-supplementing material has only the first channel, the functional material does not penetrate into the lithium-rich core and cannot improve the conductivity of the lithium-rich core, which will increase the decomposition voltage of the composite lithium-supplementing material and limit the capacity release; however, compared with the modified lithium-rich material, due to the presence of the protective layer, it still has a significant effect on reducing the volume change rate of the electrode of the composite lithium-supplementing material.
[0174] It can be seen from the test results of Example 1 and Example 9 in Table 2 that when the protective layer material is replaced, the capacity is also increased and the decomposition voltage is reduced, which shows that the advantages of the protective layer are not limited to a certain metal compound material.
[0175] It can be seen from the test results of Example 1 and Example 10 in Table 2 that when the functional material is replaced, the capacity is also increased and the decomposition voltage is reduced, which means that the advantages of the protective layer are not limited to the functional materials, and the structural advantages can enable the effects of various functional materials to be brought into play.
[0176] From the test results of Example 1 and Example 11 in Table 2, it can be seen that when the functional materials of the first channel and the second channel are different, each functional material will play a role alone, but the role of each material is relatively weak. For example, if the conductive material only exists in the first channel, it can only improve the conductivity of part of the lithium-rich core, and when the transition metal oxide only exists in the second channel, it cannot play a synergistic effect, which will cause the performance of Example 11 to be weaker than that of Example 1.
[0177] From the test results of Example 1 and Example 12 in Table 2, it can be seen that when the lithium-rich material is Li2NiO2, it also has the effects of increasing capacity, reducing decomposition voltage, and reducing the volume change rate of the electrode, which shows that the advantages of this structure are not limited to a certain material, but have similar effects on a variety of lithium-rich materials.
[0178] In the description of the embodiments of the present application, it should be noted that the orientation or positional relationship of terms such as "center", "up", "down", "left", "right", "vertical", "horizontal", "inside" and "outside" are based on the orientation or positional relationship described in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.
[0179] What is disclosed above is only a preferred embodiment of the present application, and it certainly cannot be used to limit the scope of rights of the present application. Ordinary technicians in this field can understand that all or part of the processes of implementing the above embodiment and equivalent changes made according to the claims of the present application are still within the scope covered by the present application.
Claims
1. A composite lithium supplement material, characterized in that: It comprises a lithium-rich core and a protective layer, wherein the protective layer is coated on the outer surface of the lithium-rich core, the protective layer is provided with a first channel, and the first channel is filled with a first functional material.
2. The composite lithium supplement material according to claim 1, characterized in that: The lithium-rich core is provided with a second channel, at least a portion of the first channel is connected to the second channel, the second channel is filled with a second functional material, and at least a portion of the first functional material is connected to the second functional material.
3. The composite lithium supplement material according to claim 2, characterized in that: Along the thickness direction of the protective layer, all the first channels are connected to the second channels, and the first functional material, the second functional material and the lithium-rich core are tightly connected.
4. The composite lithium supplement material according to claim 2, characterized in that: The second functional material is the same as the first functional material; and / or the first functional material and the second functional material each independently include one or more of a conductive material, an ion conductor material, and a catalyst.
5. The composite lithium supplement material according to any one of claims 1 to 4, characterized in that: There are a plurality of the first channels, the plurality of the first channels extend along the circumference of the lithium-rich core, and at least two of the first channels are interconnected.
6. The composite lithium supplement material according to any one of claims 1 to 4, characterized in that: The protective layer is an atomic layer deposition layer; and / or the protective layer contains a transition metal oxide.
7. The composite lithium supplement material according to any one of claims 2 to 4, characterized in that: The particle size D50 of the lithium-rich core is 500nm to 50μm; and / or The thickness of the protective layer is 100 nm to 1 μm; and / or The depth of the first channel is 100 nm to 1 μm; and / or The depth of the second channel is 100 nm to 20 μm; and / or The mass ratio of the lithium-rich core, the protective layer, and the functional material is 100:(5-30):(1-15), wherein the functional material is the sum of the masses of the first functional material and the second functional material.
8. A method for preparing a composite lithium supplement material, characterized in that: The steps include: Wrapping a linear template on the outer surface of the lithium-rich core; Coating the outer layer of the lithium-rich core with a protective material to form a protective layer, and allowing the linear template to be exposed outside the protective layer; removing the linear template to form a first channel in the protective layer; After depositing the first functional material in the first channel, a sintering treatment is performed to obtain a composite lithium supplementing material.
9. A positive electrode material, characterized in that: The positive electrode material includes a positive electrode active material and a lithium supplement agent, and the lithium supplement agent includes the composite lithium supplement material according to any one of claims 1 to 7, or includes the composite lithium supplement material obtained by the preparation method of the composite lithium supplement material according to claim 8.
10. A secondary battery, characterized in that: The invention comprises a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises the positive electrode material as claimed in claim 9.
Citation Information
Cited By
Positive active slurry of lithium ion battery, positive pole piece and lithium ion battery
CN120613383A