Current collector comprising undercoat layer having improved adhesive strength and method of making same

By forming a uniform base coat and an adhesive layer on the metal foil surface of the secondary battery electrode and planarizing the base coat using rolling technology, the problem of insufficient adhesion between the electrode active material layer and the base coat is solved. , improves electrode performance and productivity.

CN118919736APending Publication Date: 2024-11-08LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411291667.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2020-08-28
Filing Date
2021-06-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The adhesion between the active material layer of the electrode of the existing secondary battery and the basecoat layer is insufficient, resulting in deterioration of the electrode performance.

Method used

By forming a uniform basecoat layer on the surface of the metal foil and forming an adhesive layer thereon, the surface of the basecoat layer is planarized by rolling technology to increase the adhesive content of the adhesive layer to improve adhesion.

Benefits of technology

The interface adhesion between the electrode active material layer and the primer layer is improved, and the electrode performance is prevented from deteriorating, and the electrode productivity and processability are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919736A_ABST
    Figure CN118919736A_ABST
Patent Text Reader

Abstract

The invention relates to a current collector with improved adhesive strength and a manufacturing method thereof. The current collector is a structure including a metal foil and an undercoat layer formed on at least one surface of the metal foil, wherein the surface of the undercoat layer is a flat surface that is rolled to become uniformly flat.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application. The international application number of the original application is PCT / KR2021 / 008072, the application number of the Chinese national phase is 202180005519.7, the application date is June 28, 2021, and the name of the invention is "Current collector including a primer layer with improved adhesion strength and method for manufacturing the same." Technical Field

[0002] This application claims priority to Korean Patent Application No. 10-2020-0109410, filed on August 28, 2020, and the entire contents of the Korean Patent Application are incorporated herein by reference.

[0003] The present invention relates to a current collector including a primer layer and a method for manufacturing the same, and more particularly, to a current collector including a primer layer having improved adhesion and a method for manufacturing the same. Background Art

[0004] In recent years, secondary batteries that can be charged and discharged have been widely used as energy sources for wireless mobile devices. In addition, secondary batteries have attracted attention as energy sources for electric vehicles, hybrid electric vehicles, etc., which are proposed as a solution to air pollution caused by existing gasoline and diesel vehicles that use fossil fuels. Therefore, due to the advantages of secondary batteries, the types of applications in which secondary batteries are currently used are very diverse, and secondary batteries are expected to be used in many fields and products in the future.

[0005] According to the composition of electrodes and electrolytes, such secondary batteries can be divided into lithium-ion batteries, lithium-ion polymer batteries, lithium polymer batteries, etc., among which the use of lithium-ion polymer batteries is increasing, such batteries are less likely to leak electrolytes, and are easy to manufacture. Generally, according to the shape of the battery box, secondary batteries are divided into cylindrical batteries and prismatic batteries (in which the electrode assembly is enclosed in a cylindrical or square metal can) and pouch batteries (in which the electrode assembly is enclosed in a pouch box made of aluminum laminate sheets). The electrode assembly built into the battery box consists of a positive electrode, a negative electrode, and a diaphragm placed between the positive and negative electrodes, and is a power generation element capable of charging and discharging. The electrode assembly is divided into a core-wound type of a wound diaphragm, in which the diaphragm is placed between the positive and negative electrodes in the form of a long sheet and coated with an active material, and a stacked type, in which a plurality of positive and negative electrodes of predetermined sizes are stacked in sequence, with a diaphragm placed between them.

[0006] In addition, the electrode used for such a secondary battery generally has a structure in which an electrode active material layer is formed by coating an electrode slurry containing an electrode active material on a current collector and then performing a drying and rolling process. In this case, a binder is contained in the electrode slurry, but even in this case, a problem occurs due to a reduction in the bonding force between the current collector and the electrode active material layer.

[0007] Figure 1 is a cross-sectional view showing the structure of an electrode and a current collector having a primer layer of a conventional technology. Figure 1 , in the conventional electrode 1 , the electrode active material layer 5 is formed on the current collector 2 , but the primer layer 4 may be formed on the metal foil 3 to form the current collector 2 to prevent the adhesive force between the current collector 2 and the electrode active material layer 5 from being reduced.

[0008] However, the undercoat layer 4 may be formed on the metal foil 3, which is generally formed by applying a slurry for forming the undercoat layer 4 on the metal foil 3 using a roller, etc. In this case, the surface of the undercoat layer 4 has an uneven shape after coating.

[0009] Similarly, when the surface of the undercoat layer 4 has an uneven shape, if the electrode 1 is subsequently manufactured by forming an electrode active material layer 5 on the undercoat layer 4, a space is formed between the electrode active material layer 5 and the undercoat layer 4, resulting in reduced adhesion between the electrode interfaces and deterioration of electrode performance (e.g., output).

[0010] Therefore, technological development is needed to solve this problem. Summary of the invention

[0011] [Technical issues]

[0012] An object of the present invention is to provide a current collector having improved adhesion between an electrode active material layer and an undercoat layer and a method for manufacturing the same.

[0013] [Technical solution]

[0014] A current collector according to an embodiment of the present invention includes: a metal foil; and a primer layer formed on at least one surface of the metal foil, wherein a surface of the primer layer has a flat surface uniformly planarized by rolling.

[0015] In one particular example, the primer layer includes a carbon-based material and a binder.

[0016] In another embodiment of the present invention, the surface of the metal foil has irregularities formed by rolling the primer layer.

[0017] In yet another embodiment of the present invention, the current collector of the present invention further includes a binder layer formed on the primer layer.

[0018] In a specific example, the binder layer includes a carbon-based material and a binder, and the binder content of the binder layer is greater than the binder content of the primer layer.

[0019] In a particular example, the thickness of the adhesive layer is less than the thickness of the primer layer.

[0020] In a specific example, the adhesive layer may be formed in a pattern on a portion of the primer layer.

[0021] Furthermore, the present invention provides an electrode including the current collector as described above, and having a structure in which an electrode active material layer is formed on the current collector as described above.

[0022] In addition, the present invention provides a method for manufacturing a current collector as described above. The method for manufacturing a current collector according to an embodiment of the present invention includes: preparing a metal foil; forming a primer layer by coating a primer composition on at least one surface of the metal foil; and rolling the metal foil on which the primer layer is formed so as to uniformly planarize the surface of the primer layer.

[0023] In one particular example, the primer composition includes a carbon-based material and a binder.

[0024] In another embodiment of the present invention, the irregularities are formed on the surface of the metal foil by rolling the primer layer.

[0025] The method for manufacturing a current collector according to another embodiment of the present invention further includes forming an adhesive layer by coating the adhesive composition on the primer layer.

[0026] In a specific example, the binder composition includes a carbon-based material and a binder, and the binder content of the binder composition is greater than the binder content of the primer composition.

[0027] In a particular example, the thickness of the adhesive layer is less than the thickness of the primer layer.

[0028] In one particular example, the adhesive composition is coated in a pattern on a portion of the base coating.

[0029] In addition, the present invention provides a method for manufacturing an electrode, comprising the method for manufacturing a current collector as described above. The method for manufacturing an electrode comprises: manufacturing a current collector according to the method for manufacturing a current collector as described above, and coating an electrode slurry containing an electrode active material on the current collector to form an electrode active material layer.

[0030] [Beneficial Effects]

[0031] According to the present invention, a primer layer is formed on a current collector, and by rolling the primer layer, the surface of the primer layer is planarized, and the pores in the primer layer can be minimized. Thus, the interfacial adhesion between the primer layer and the electrode active material layer can be improved, and the electrode performance can be prevented from deteriorating.

[0032] Furthermore, by making the thickness of the current collector uniform, the productivity and processability of the electrode can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is a cross-sectional view showing the structure of an electrode having a primer layer and a current collector of a conventional art.

[0034] Figure 2 is a cross-sectional view showing the structure of a current collector according to an embodiment of the present invention.

[0035] Figure 3 is a cross-sectional view showing the structure of a current collector according to another embodiment of the present invention.

[0036] Figure 4 is a cross-sectional view showing the structure of a current collector according to still another embodiment of the present invention.

[0037] Figure 5 It is a cross-sectional view showing the structure of an electrode according to an embodiment of the present invention.

[0038] Figure 6 1 is a flowchart showing the procedure of the current collector manufacturing method of the present invention.

[0039] Figure 7 Schematic diagram showing a method for manufacturing a current collector according to an embodiment of the present invention.

[0040] Figure 8 is a schematic diagram showing a method for manufacturing a current collector according to another embodiment of the present invention.

[0041] Fig. 9 Schematic diagram showing a method for manufacturing a current collector according to another embodiment of the present invention. DETAILED DESCRIPTION

[0042] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings. The terms and words used in this specification and claims should not be interpreted as being limited to common terms or dictionary terms, and the inventor may appropriately define the concepts of the terms in order to best describe his invention. The terms and words should be interpreted as meanings and concepts consistent with the technical ideas of the present invention.

[0043] In the present application, it should be understood that terms such as "including" or "containing" are intended to indicate features, numbers, steps, operations, ingredients, parts or combinations thereof described in the specification, and they do not preclude the possibility of the presence or addition of one or more other features or numbers, steps, operations, ingredients, parts or combinations thereof. In addition, when a part such as a layer, a film, a region, a plate, etc. is referred to as being "on" another part, this includes not only the case where the part is "directly on" another part, but also the case where another part is inserted therebetween. On the other hand, when a part such as a layer, a film, a region, a plate, etc. is referred to as being "under" another part, this includes not only the case where the part is "directly under" another part, but also the case where another part is inserted therebetween. In addition, in the present application, being arranged "on" may include being arranged at the bottom and the top.

[0044] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings.

[0045] Figure 2 is a cross-sectional view showing the structure of a current collector according to an embodiment of the present invention.

[0046] refer to Figure 2 The current collector 10 according to the embodiment of the present invention includes: a metal foil 11; and a primer layer 12 formed on at least one surface of the metal foil 11, and the surface of the primer layer 12 has a structure in which a flat surface is uniformly planarized by rolling.

[0047] As described above, the undercoat layer may be formed on the metal foil, which is generally formed by applying a slurry for forming the undercoat layer on the metal foil using a roller, etc. In this case, the surface of the undercoat layer has an uneven shape after coating.

[0048] Likewise, in the case where the surface of the undercoat layer has an uneven shape, when the electrode active material is subsequently coated on the undercoat layer, Figure 1 As shown, voids are formed between the electrode active material layer and the undercoat layer, resulting in reduced adhesion between electrode interfaces and deterioration of electrode performance (eg, output).

[0049] According to the present invention, a primer layer is formed on a current collector, and the surface of the primer layer is planarized by rolling the primer layer, and the pores in the primer layer can be minimized. Thus, the interfacial adhesion between the primer layer and the electrode active material layer can be improved, and the electrode performance can be prevented from deteriorating.

[0050] refer to Figure 2 The current collector 10 according to the embodiment of the present invention has a structure in which a primer layer 12 is formed on a metal foil 11. In addition, the current collector may be a positive electrode current collector or a negative electrode current collector.

[0051] In the case of the positive electrode current collector, the metal foil 11 generally has a thickness of 3 microns to 500 microns. The metal foil is not particularly limited as long as it has high conductivity and does not cause chemical changes in the battery. For example, the current collector may be made of metals such as stainless steel, aluminum, nickel, titanium, sintered carbon, or aluminum or stainless steel whose surface has been treated with carbon, nickel, titanium or silver, etc. The metal foil may have fine irregularities on its surface to increase the adhesion of the positive electrode active material, and may be in various forms such as films, sheets, foils, nets, porous bodies, foams and non-woven fabrics.

[0052] In the case of the negative electrode current collector, the metal foil 11 generally has a thickness of 3 microns to 500 microns. The metal foil is not particularly limited as long as it has conductivity and does not cause chemical changes in the battery. Examples of negative electrode current collectors include copper, stainless steel, aluminum, nickel, titanium, sintered carbon, copper or stainless steel whose surfaces have been treated with carbon, nickel, titanium or silver, or aluminum-cadmium alloys, etc. In addition, as with the positive electrode current collector, fine unevenness can be formed on the surface of the metal foil to enhance the binding force of the negative electrode active material, and it can be used in various forms, such as films, sheets, foils, nets, porous bodies, foams, and non-woven fabrics.

[0053] In addition, the undercoat layer 12 increases the adhesion of the electrode active material layer to the current collector while suppressing the increase of the electrode internal resistance as much as possible, and may contain a carbon-based material to enhance the electrical conductivity between the electrode active material layer and the metal foil (described later). Figure 2 , the primer layer 12 is formed only on one surface of the metal foil 11. Herein, when an electrode in which an electrode active material layer is formed on both surfaces of the metal foil 11 is manufactured, the primer layer 12 may be formed on both surfaces of the metal foil 11.

[0054] The carbon-based material is not particularly limited as long as it is an element that maintains conductivity by electrically connecting the metal foil 11 to the electrode active material layer. For example, the carbon-based material may be one or more selected from the group consisting of natural graphite, artificial graphite, graphene, carbon black, denka black, acetylene black, ketjen black, super-P, channel black, furnace black, lamp black, summer black, carbon nanotubes, graphite nanofibers, and carbon nanofibers.

[0055] Furthermore, the undercoat layer 12 may fix the carbon-based material as described above on the metal foil 11 and form a coating film, and may further include a binder for bonding the metal foil 11 and the electrode active material layer.

[0056] The type of adhesive is not particularly limited as long as it can show bonding strength. For example, the adhesive may include one or more selected from the group consisting of polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose (HPC), regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber and fluororubber.

[0057] When the primer layer 12 includes a binder and a carbon-based material, the weight ratio of the carbon-based material to the binder can be 3:7 to 7:3, specifically 4:6 to 6:4. When the weight ratio of the carbon-based material to the binder is within the above range, the conductivity and bonding force of the primer layer 12 can be properly ensured. Specifically, when the weight ratio of the carbon-based material to the binder is less than the above range, the content of the conductive material is too small, so the operating characteristics of the battery are reduced due to the increase in internal resistance. On the contrary, if the weight ratio exceeds the above range, the content of the adhesive material is too small, so sufficient bonding force cannot be obtained.

[0058] Furthermore, the undercoat layer 12 may further contain inorganic particles such as aluminum, nickel, zinc oxide, potassium titanate, and titanium oxide to additionally ensure conductivity.

[0059] The thickness of the primer layer 12 is 0.1 μm to 10 μm, specifically 0.1 μm to 5 μm, and more specifically 0.1 μm to 1 μm. If the thickness of the primer layer 12 is less than this range, the bonding force between the metal foil 11 and the electrode active material layer cannot be fully ensured, and it is difficult to form a uniform layer. On the contrary, if the thickness exceeds this range, the primer layer 12 acts as a resistor, thereby deteriorating the electrical properties of the electrode or increasing the volume of the electrode.

[0060] As a method for forming the undercoat layer, a coating forming method commonly used in the related art can be used. For example, wet coating methods such as gravure coating, slit coating, spin coating, spray coating, rod coating, and deposition coating; and dry coating methods such as thermal evaporation, electron beam evaporation, chemical vapor deposition (CVD), and sputtering can be used.

[0061] At this time, in the present invention, the surface of the primer layer 12 has a structure in which a uniformly planarized flat surface is formed by rolling. Herein, the surface of the primer layer 12 refers to the opposite surface of the surface where the primer layer contacts the metal foil 11. That is, when the primer layer 12 is formed on the metal foil 11, fine irregularities are formed on the surface. At this time, the flat surface can be formed by rolling and squeezing fine irregularities. That is, the current collector 10 can improve the adhesion between the primer layer 12 and the electrode active material layer by preventing the above-mentioned fine irregularities from acting as bubbles in the space between the primer layer 12 and the electrode active material layer.

[0062] Here, for example, a pair of rolling rollers may be used to roll-press the metal foil 11 formed with the primer layer 12. Here, the rolling method is not limited thereto, and various known rolling methods may be used.

[0063] On the other hand, the surface roughness (Ra) of the primer layer 12 may be 0.01 μm to 1 μm, specifically 0.1 μm to 0.5 μm. Herein, the surface roughness (Ra) is also referred to as the "center line average value", which refers to the average value of the absolute value of the length from the center line of the roughness curve to the surface cross-sectional curve within the reference length.

[0064] If the surface roughness is less than the above range, the surface area of ​​the undercoat layer 12 becomes too small, and the adhesive force between the undercoat layer 12 and the electrode active material layer may be reduced. If the surface roughness exceeds the above range, bubbles may be formed between the electrode active material layer and the undercoat layer 12 when the electrode active material layer is formed.

[0065] Figure 3 is a cross-sectional view showing the structure of a current collector according to another embodiment of the present invention.

[0066] refer to Figure 3 , the surface of the metal foil 11 may have a structure in which irregularities (A) are formed by rolling the primer layer 12. Specifically, when the metal foil 11 formed with the primer layer 12 is rolled to planarize the surface of the primer layer 12, irregularities (A) may be formed on the surface of the metal foil 11 due to the particles constituting the primer layer 12 pressing the metal foil 11. Such irregularities (A) may improve the bonding force between the primer layer 12 and the metal foil 11. Therefore, by appropriately adjusting the size (e.g., average particle size) and strength of the particles (i.e., carbon-based material, etc.) constituting the primer layer 12, irregularities of a predetermined size may be formed on the metal foil 11.

[0067] At this time, the surface state of the primer layer 12 and the metal foil 11 and the thickness of the primer layer 12 can be determined according to the rolling degree of the primer layer 12. The rolling degree can be appropriately designed according to the specifications of the current collector to be manufactured. Specifically, the primer layer 12 can be rolled with a rolling strength of 5MPa to 200MPa, specifically 50MPa to 100MPa. In addition, the rolling rate of the primer layer 12 can be 50% to 90%, specifically 60% to 80%. Herein, the rolling rate refers to the percentage obtained by dividing the difference between the density (G1) of the primer layer before rolling and the density (G2) of the primer layer after rolling by the density (G1) of the primer layer before rolling, which can be calculated by {(G2-G1) / G1}*100.

[0068] In addition, the porosity of the primer layer after rolling may be 10% or less, specifically 5% or less, and more specifically 3% or less. That is, the porosity of the primer layer is preferably as small as possible in terms of bonding performance and conductivity.

[0069] Figure 4 is a cross-sectional view showing the structure of a current collector according to still another embodiment of the present invention.

[0070] refer to Figure 4 The current collector 10 according to another embodiment of the present invention further includes an adhesive layer 13 formed on the primer layer 12 . Figure 4 (a) Shown in Figure 2 An adhesive layer is formed on the current collector. Figure 4 (b) shows Figure 3 An adhesive layer is formed on the current collector shown, and the current collector has a structure in which irregularities are formed on the surface of the metal foil. Figure 4 , since the primer layer 12 is formed only on one surface of the metal foil 11, the adhesive layer 13 is also formed on one surface of the metal foil 11. Herein, if the primer layer 12 is formed on both surfaces of the metal foil 11, the adhesive layer 13 may also be formed on both surfaces of the metal foil 11.

[0071] Therefore, the binder layer 13 provides additional adhesive force to the electrode active material layer in the space between the undercoat layer 12 and the electrode active material layer described later.

[0072] The adhesive layer 13 may include a carbon-based material and an adhesive. At this time, the carbon-based material is used to ensure the conductivity between the primer layer 12 and the metal foil 11 and the electrode active material layer, and the adhesive is used to bond the primer layer 12 to the electrode active material layer. The same materials as described above can be used as the carbon-based material and the adhesive, and the same carbon-based material and adhesive as those used for the primer layer 12 can be used, or different kinds can be used.

[0073] In addition, in the adhesive layer 13, the weight ratio of the carbon-based material and the adhesive can be 0:10 to 7:3, specifically 1:9 to 6:4. That is, the adhesive layer 13 can contain both the carbon-based material and the adhesive, or only the adhesive. When the weight ratio of the carbon-based material and the adhesive is within the above range, the conductivity and bonding force of the adhesive layer 13 can be properly ensured. Here, in order to ensure sufficient bonding force, the content of the adhesive is preferably greater than the content of the adhesive in the primer layer 12. Here, the content of the adhesive can be the ratio of the weight of the adhesive to the total weight of each layer.

[0074] In addition, the thickness of the adhesive layer 13 is 0.1 μm to 5 μm, specifically 0.1 μm to 3 μm, and more specifically 0.1 μm to 2 μm. Herein, in this case, in order to ensure sufficient conductivity between the metal foil 11 and the undercoat layer 12 and the electrode active material layer, the thickness of the adhesive layer 13 is preferably less than the thickness of the undercoat layer 12. When the thickness of the adhesive layer 13 is less than the above range, it may be difficult to ensure the bonding force with the electrode active material layer, and when the thickness of the adhesive layer 13 exceeds the range, since the adhesive layer acts as a resistor, it may be difficult to fully ensure the conductivity between the metal foil 11 and the undercoat layer 12 and the electrode active material layer.

[0075] In addition, since the adhesive layer 13 uses a large amount of adhesive, the adhesive layer 13 may reduce the conductivity between the metal foil 11 and the primer layer 12 and the electrode active material layer compared to the primer layer 12. Therefore, the adhesive layer 13 should be formed in a minimum amount to ensure the bonding force on the primer layer 12. Therefore, the adhesive layer 13 can be formed on a part of the primer layer 12 in a pattern. Specifically, the adhesive layer 13 can be formed on the part between the primer layer 12 and the electrode active material layer that is often separated due to weak bonding force. For example, the adhesive layer 13 can be formed at the two edge portions of the primer layer 12 in a pattern.

[0076] In addition, the present invention provides an electrode comprising the current collector of the present invention.

[0077] Figure 5 is a cross-sectional view showing an electrode structure according to an embodiment of the present invention.

[0078] refer to Figure 5 The electrode 20 of the present invention includes the current collector 10 as described above, and the electrode 20 has a structure in which the electrode active material layer 14 is formed on the current collector 10. That is, the electrode 20 has a structure in which the primer layer 12 and the electrode active material layer 14 are sequentially stacked on the metal foil 11, and the surface of the primer layer 12 may have a structure in which a flat surface is planarized by rolling. In addition, although Figure 5 Although not shown, irregularities may be formed on the surface of the metal foil 11 depending on the rolling conditions. In addition, the binder layer 13 may be formed on the primer layer 12, and the electrode active material layer 14 may be formed on the binder layer 13. At this time, the electrode active material layer 14 may include an electrode active material, a conductive material, and a binder, and the electrode active material may be a positive electrode active material or a negative electrode active material.

[0079] In the present invention, the positive electrode active material is a material capable of causing an electrochemical reaction and is a lithium transition metal oxide containing two or more transition metals. Examples thereof include: layered compounds, for example, lithium cobalt oxide (LiCoO2) and lithium nickel oxide (LiNiO2) substituted with one or more transition metals; lithium manganese oxide substituted with one or more transition metals; 1-y M y Lithium nickel oxide represented by O2 (wherein M = Co, Mn, Al, Cu, Fe, Mg, B, Cr, Zn or Ga, and contains at least one of the above elements, 0.01≤y≤0.7); 1+z Ni b Mn c Co 1-(b+c+d) M d O (2-e) A eThe represented lithium nickel cobalt manganese composite oxide, such as Li 1+z Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O2, Li 1+z Ni 0.4 Mn 0.4 Co 0.2 O2, etc. (where -0.5 ≤ z ≤ 0.5, 0.1 ≤ b ≤ 0.8, 0.1 ≤ c ≤ 0.8, 0 ≤ d ≤ 0.2, 0 ≤ e ≤ 0.2, b + c + d < 1, M = Al, Mg, Cr, Ti, Si or Y, and A = F, P or Cl); the olivine-type lithium metal phosphate represented by the formula Li 1+x M 1-y M' y PO 4-z X z (where M = transition metal, preferably Fe, Mn, Co or Ni, M' = Al, Mg or Ti, X = F, S or N, and -0.5 ≤ x ≤ 0.5, 0 ≤ y ≤ 0.5, 0 ≤ z ≤ 0.1).

[0080] Examples of the negative electrode active material include: carbon, such as non-graphitized carbon and graphitic carbon; metal composite oxides, such as Li x Fe2O3 (0 ≤ x ≤ 1), Li x WO2 (0 ≤ x ≤ 1), Sn x Me 1-x Me’ y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, Groups 1, 2 and 3 of the periodic table, halogen; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8); lithium alloys; silicon alloys; tin alloys; metal oxides, such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4 and Bi2O5; conductive polymers, such as polyacetylene; and Li-Co-Ni-based materials).

[0081] The addition amount of the conductive material is usually 1 wt% to 30 wt% of the total weight of the mixture containing the positive electrode active material. The conductive material is not particularly limited as long as it has conductivity and does not cause chemical changes in the battery. Examples thereof include: graphite, such as natural graphite and artificial graphite; carbon black, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black and summer black; conductive fibers, such as carbon fibers and metal fibers; metal powders, such as carbon fluoride, aluminum powder and nickel powder; conductive whiskers, such as zinc oxide and potassium titanate; conductive metal oxides, such as titanium oxide; and conductive materials such as polyphenylene derivatives, etc.

[0082] As a component that helps the adhesion between the active material and the conductive material and the adhesion with the current collector, the binder is added in an amount of 1% to 30% by weight of the total weight of the mixture containing the positive electrode active material. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene butene rubber, fluororubber, various copolymers, etc.

[0083] The present invention also provides a method for manufacturing the current collector as described above.

[0084] Figure 6 1 is a flowchart showing the procedure of the current collector manufacturing method of the present invention.

[0085] refer to Figure 6 The current collector manufacturing method according to an embodiment of the present invention includes: preparing a metal foil (S10); forming a primer layer by coating a primer composition on at least one surface of the metal foil (S20); and rolling the metal foil on which the primer layer is formed, thereby uniformly planarizing the surface of the primer layer (S30).

[0086] According to the present invention, a primer layer is formed on a current collector, and the surface of the primer layer is planarized by rolling the primer layer, and the pores in the primer layer can be minimized. Thus, the interfacial adhesion between the primer layer and the electrode active material layer can be improved, and the electrode performance can be prevented from deteriorating.

[0087] Figure 7 Schematic diagram showing a method for manufacturing a current collector according to an embodiment of the present invention.

[0088] refer to Figure 6 and 7 In the current collector manufacturing method of the present invention, first, a primer layer 12 is formed on at least one surface of a metal foil 11. The primer layer 12 is formed by coating a primer composition on at least one surface of the metal foil 11. Here, the primer composition includes a carbon-based material and a binder.

[0089] The carbon-based material is not particularly limited as long as it is an element that maintains conductivity by electrically connecting the metal foil 11 to the electrode active material layer. For example, the carbon-based material may be one or more selected from the group consisting of natural graphite, artificial graphite, graphene, carbon black, denka black, acetylene black, ketjen black, super-P, channel black, furnace black, lamp black, summer black, carbon nanotubes, graphite nanofibers, and carbon nanofibers.

[0090] The type of adhesive is not particularly limited as long as it can show bonding strength. For example, the adhesive may include one or more selected from the group consisting of polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose (HPC), regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber and fluororubber.

[0091] When the primer composition includes a binder and a carbon-based material, the weight ratio of the carbon-based material to the binder may be 3:7 to 7:3, specifically 4:6 to 6:4. When the weight ratio of the carbon-based material to the binder is within the above range, the conductivity and bonding force of the primer layer 12 can be appropriately ensured.

[0092] In addition, the primer composition may further include a dispersant for dispersing the carbon-based material and inorganic particles for ensuring additional conductivity.

[0093] The primer composition may be applied with a thickness of 0.1 μm to 10 μm, specifically 0.1 μm to 5 μm, more specifically 0.1 μm to 1 μm. If the thickness is less than this range, the bonding force between the metal foil 11 and the electrode active material layer cannot be sufficiently ensured, and it is difficult to form a uniform layer. On the contrary, if the thickness exceeds this range, the primer layer 12 acts as a resistor, thereby deteriorating the electrical properties of the electrode or increasing the volume of the electrode.

[0094] The coating formation method commonly used in the prior art can be used as a method for forming the undercoat layer. For example, wet coating methods such as gravure coating, slit coating, spin coating, spray coating, rod coating, and deposition coating; and dry coating methods such as thermal evaporation, electron beam evaporation, chemical vapor deposition (CVD), and sputtering can be used.

[0095] If the primer layer 12 is formed, the surface of the primer layer 12 is planarized by rolling the primer layer 12. When the primer layer 12 is formed on the metal foil 11, fine irregularities are formed on the surface. At this time, a flat surface can be formed by rolling and squeezing these fine irregularities. That is, the current collector 10 can improve the adhesion between the primer layer 12 and the electrode active material layer by preventing the above-mentioned fine irregularities from acting as bubbles in the space between the primer layer 12 and the electrode active material layer.

[0096] Herein, for example, the metal foil 11 formed with the primer layer 12 may be rolled using a pair of rolling rollers (not shown). Herein, the rolling method is not limited thereto, and various known rolling methods may be used.

[0097] Figure 8 is a schematic diagram showing a method for manufacturing a current collector according to another embodiment of the present invention.

[0098] refer to Figure 6 and 8 By rolling the metal foil 11 (on which the primer layer 12 is formed) with an appropriate rolling strength, irregularities (A) can be formed on the surface of the metal foil 11. When the metal foil 11 on which the primer layer 12 is formed is rolled to planarize the surface of the primer layer 12, since the particles constituting the primer layer 12 press the metal foil 11, irregularities (A) can be formed on the surface of the metal foil 11. Therefore, by appropriately adjusting the size (e.g., average particle diameter) and strength of the particles (i.e., carbon-based material, etc.) constituting the primer layer 12, irregularities (A) of a predetermined size can be formed on the metal foil 11.

[0099] The rolling conditions for forming irregularities on the surface of the metal foil 11 and planarizing the undercoat layer 12 can be appropriately designed by a person of ordinary skill in the art, and the detailed description thereof is described above.

[0100] Fig. 9 Schematic diagram showing a method for manufacturing a current collector according to another embodiment of the present invention.

[0101] refer to Figure 6 and 9 The current collector manufacturing method of the present invention further includes forming an adhesive layer 13 by coating an adhesive composition on the primer layer 12 .

[0102] The adhesive composition includes a carbon-based material and an adhesive. As the carbon-based material and the adhesive, the same materials as described above may be used, the same carbon-based material and the adhesive as used for the primer composition may be used, or different kinds may be used.

[0103] In addition, in the adhesive composition, the weight ratio of the carbon-based material to the adhesive can be 0:10 to 7:3, specifically 1:9 to 6:4. That is, the adhesive composition can include the carbon-based material and the adhesive at the same time, or can only include the adhesive. When the weight ratio of the carbon-based material and the adhesive is within the above range, the conductivity and bonding force of the primer layer 12 can be appropriately ensured. Here, to ensure sufficient bonding force, the content of the adhesive is preferably greater than the adhesive content in the primer composition. Here, the content of the adhesive can be the ratio of the weight of the adhesive to the gross weight of each layer.

[0104] The adhesive composition may be applied at a thickness of 0.1 μm to 5 μm, specifically 0.1 μm to 3 μm, and more specifically 0.1 μm to 2 μm. Herein, in this case, to ensure sufficient conductivity between the metal foil 11 and the undercoat layer 12 and the electrode active material layer, the thickness of the adhesive layer 13 is preferably less than the thickness of the undercoat layer 12. When the thickness of the adhesive layer 13 is less than the above range, it may be difficult to ensure the bonding force with the electrode active material layer, and when the thickness of the adhesive layer 13 exceeds the range, since the adhesive layer acts as a resistor, it may be difficult to fully ensure the conductivity between the metal foil 11 and the undercoat layer 12 and the electrode active material layer.

[0105] In addition, since the adhesive layer 13 uses a large amount of adhesive, the adhesive layer 13 may reduce the conductivity between the metal foil 11 and the primer layer 12 and the electrode active material layer compared to the primer layer 12. Therefore, the adhesive layer 13 should be formed with the minimum amount of the bonding force on the primer layer 12 to ensure the bonding force. Therefore, the adhesive composition can be formed on a part of the primer layer 12 in a pattern. Specifically, the adhesive composition can be formed on the part that is often separated due to the weak bonding force between the primer layer 12 and the electrode active material layer. For example, the adhesive layer 13 can be formed on the two edge portions of the primer layer 12 in a pattern.

[0106] In addition, the present invention provides a method for manufacturing an electrode, the electrode manufacturing method of the present invention comprising: manufacturing a current collector according to the current collector manufacturing method as described above; and forming an electrode active material layer by coating an electrode slurry containing an electrode active material on the current collector. The details of the electrode active material and the electrode slurry are as described above.

[0107] The above description only illustrates the technical idea of ​​the present invention, and those skilled in the art to which the present invention belongs can make various modifications and changes without departing from the basic features of the present invention. Therefore, the drawings disclosed in the present invention are not intended to limit the technical idea of ​​the present invention, but to describe the present invention, and the scope of the technical idea of ​​the present invention is not limited by these drawings. The scope of protection of the present invention shall be interpreted by the following claims, and all technical ideas within the scope equivalent thereto shall be interpreted as included within the scope of the present invention.

[0108] On the other hand, in this specification, terms indicating directions such as up, down, left, right, front, and back are used, but it is obvious that these terms are only for convenience of description and may change depending on the position of the object or the position of the observer.

[0109] [Description of Reference Signs]

[0110] 1,20: Electrode

[0111] 2,10: Current collector

[0112] 3,11: Metal foil

[0113] 4,12: Base coating

[0114] 5,14: Electrode active material layer

[0115] 13: Adhesive layer

Claims

1. A current collector, comprising: metal foil; and a primer layer formed on at least one surface of the metal foil, wherein the surface of the undercoat layer on which the electrode active material layer is to be formed has a flat surface uniformly planarized by rolling; wherein the surface of the metal foil in contact with the primer layer has irregularities formed by rolling the primer layer; wherein the rolling rate of the primer layer is 50% to 90% and the porosity of the primer layer after rolling is less than 10%; wherein the rolling rate is {(G2-G1) / G1}*100, wherein G1 is the density of the primer layer before rolling, and G2 is the density of the primer layer after rolling.

2. The current collector according to claim 1, wherein: The primer layer includes a carbon-based material and a binder.

3. The current collector according to claim 1, wherein: The irregularities in the surface of the metal foil are formed by particles constituting the primer layer being pressed against the metal foil under the roller pressure. 4 . The current collector of claim 1 , further comprising an adhesive layer formed on the primer layer.

5. The current collector according to claim 4, wherein: The adhesive layer comprises a carbon-based material and an adhesive, and The adhesive content of the adhesive layer is greater than the adhesive content of the primer layer.

6. The current collector according to claim 4, wherein: The thickness of the adhesive layer is smaller than the thickness of the primer layer.

7. The current collector according to claim 4, wherein: The adhesive layer is formed in a pattern on a portion of the primer layer.

8. The current collector according to claim 1, wherein: The rolling is performed at a rolling intensity of 5 MPa to 200 MPa, preferably 50 MPa to 100 MPa.

9. The current collector according to claim 1, wherein: The roll pressing rate of the primer layer is 60% to 80%, and the porosity of the primer layer after rolling is 5% or less. 10 . An electrode having a structure in which an electrode active material layer is formed on the current collector according to claim 1 .

11. A method for manufacturing the current collector according to any one of claims 1 to 9, the method comprising: Prepare the metal foil; forming a primer layer by coating a primer composition on at least one surface of the metal foil; and The metal foil having the primer layer formed thereon is rolled to uniformly planarize the surface of the primer layer.

12. A method for manufacturing an electrode, the method comprising: The method according to claim 11, wherein the current collector is manufactured, and An electrode slurry including an electrode active material is coated on the current collector to form an electrode active material layer.