Amorphous solid solution type solid electrolyte, preparation method thereof and solid-state battery

Through the framework structure of amorphous solid solution solid electrolyte, the combination of carrier salt and van der Waals crystals is used to solve the problem that solid electrolytes are difficult to introduce beneficial elements and easy to decompose, and a high-performance solid-state battery is realized, supporting low temperature and high magnification. battery running.

CN118919829APending Publication Date: 2024-11-08NINGBO ORIENTAL UNIV OF TECH (TEMPORARY NAME)
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411024548.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, it is difficult to introduce beneficial elements in solid electrolytes and are easily decomposed on the electrode surface, resulting in deterioration of battery performance and failure.

Method used

Amorphous solid solution solid electrolyte is used, with the general formula (CaAb)x-MBy, and is composed of the frame structure of carrier salt CaAb and van der Waals crystal MBy, and part of the anion of the carrier salt replaces part of the B element in the van der Waals crystal. Nanocrystals of dissociated cations C and MBy or B are formed as solid solvents to realize the functionalization of the electrolyte.

Benefits of technology

High air stability and high room temperature ionic conductivity are achieved, supporting extremely low temperature and high magnification solid-state battery performance, and optimize the performance of all-solid-state battery by designing anion in salt CaAb.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919829A_ABST
    Figure CN118919829A_ABST
Patent Text Reader

Abstract

The invention discloses an amorphous solid solution type solid electrolyte, a preparation method thereof and a solid-state battery, and belongs to the technical field of solid-state batteries. The general formula of the amorphous solid solution type solid electrolyte is (CaAb) x-MBy, CaAb is carrier salt, MBy is Van der Waals crystals, B elements in the Van der Waals crystals are replaced by part of anions A in CaAb to form a frame structure, cations C released by dissociation and MBy or B form nanocrystals CeMBf or CB, the dissociated cations C exist in the frame structure, and the nanocrystals CeMBf and CB are on the surface of the frame structure. Through the composition, the Van der Waals crystal MBy plays a role of a solid-state solvent and can dissociate various CaAb salts and form a solid-solution electrolyte; meanwhile, the acting force between the positive ions C and the negative ions in the frame is weak, so that the migration rate of the positive ions C in the frame structure is high, and the high-room-temperature ionic conductivity is shown.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of solid-state batteries, and in particular relates to an amorphous solid solution type solid electrolyte and a preparation method thereof, and a solid-state battery. Background Art

[0002] All-solid-state batteries have become the most promising next-generation energy storage technology due to their high energy density and intrinsic safety. The key to the practical application of all-solid-state batteries is to develop functional solid electrolytes that are well matched with lithium metal anodes and / or high-voltage cathodes, have good air stability, and support devices that can be used under extreme conditions such as low temperature (<-30°C) and high charge / discharge rates (>10C, where 1C corresponds to 1 hour to complete charging or discharging).

[0003] The traditional liquid lithium (sodium, potassium, aluminum, etc.) ion battery field widely adopts the electrolyte (liquid) engineering strategy. By using different solvents, additives and lithium salts to design the electrolyte composition, the low-temperature performance and flammability of the electrolyte are targeted to improve the solvation junction and the solid electrolyte interphase (SEI) composition formed, thereby developing functionalized electrolytes. However, the electrolyte (liquid) engineering strategy is difficult to apply to the development of solid electrolytes. This is because the ion transport of solid electrolytes often depends on a specific crystal structure, such as the halide Li3InCl6 with a layered structure (patent document: CN 111916820 A), the halide Li with a UCl3-type lattice 0.388 Ta 0.238 La 0.475 Cl3 (patent document: CN 113772729 A), Li oxide with perovskite structure 0.33 La 0.56 TiO3 (Solid State Ionics 228, 80-82), oxide with garnet structure Li7La3Zr2O 12 (Angew.Chem.Int.Ed.2007,46,7778–7781), sulfide Li6PS5Cl with face-centered cubic structure (Electrochimica Acta 215,93-99), etc. Therefore, the electrolyte composition can only be regulated by doping and substitution, and it is not possible to flexibly introduce beneficial elements. The doped ions need to have similar ionic radius and valence to the ions at the target lattice site, so the range of options is limited.

[0004] In addition, during the cycle of liquid batteries, although part of the organic electrolyte decomposes on the electrode surface and forms SEI, the ionic conductivity of the remaining electrolyte is not affected, and it can still infiltrate the electrode surface through the gaps in the SEI membrane, so the ion transport kinetics and interface impedance of the electrolyte / electrode interface will not be significantly affected. However, in all-solid-state batteries, the decomposition of solid electrolytes on the electrode surface will destroy its ion transport channels, greatly reduce ionic conductivity, and cause a sudden increase in electrolyte / electrode interface impedance, which becomes an important factor in battery performance deterioration and failure. Therefore, the strategy of designing solid electrolyte components through electrolyte engineering and then regulating SEI is still difficult to achieve. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and to provide an amorphous solid solution type solid electrolyte and a preparation method thereof and a solid-state battery, so as to solve the problems in the prior art that it is difficult to introduce beneficial elements into the solid electrolyte and the solid electrolyte is easy to decompose on the electrode surface, resulting in easy deterioration of battery performance and failure.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] Amorphous solid solution type solid electrolyte, the general formula is (C a A b ) x -MB y , the (C a A b ) x -MB y It is a frame structure;

[0008] Among them, C a A b is the carrier salt, a and b are the atomic numbers of cation C and anion A in the carrier salt, respectively. y is a van der Waals crystal, y is the number of atoms of element B, x is the number of atoms of element C a A b and MB y The stoichiometric ratio;

[0009] The B element in the van der Waals crystal is C a A b The anion A in the cation is partially replaced, and the dissociated cation C is in the framework structure; the C is attached to the outside of the framework structure. e MB f and CB, C e MB f where e and f are the stoichiometric numbers of cations C and MB, respectively.

[0010] A further improvement of the present invention is:

[0011] Preferably, the van der Waals crystal is one or more of a halide van der Waals crystal, a sulfide van der Waals crystal or an oxide van der Waals crystal;

[0012] The carrier salt is one or more of lithium salt, sodium salt, silver salt, copper salt or potassium salt.

[0013] Preferably, the C a A b C in the + 、Na + 、Ag + , Cu + or K + ; A is a simple anion, a polyanion or a mixture of the two; the simple anion is a halogen, OH-, NH2 - 、O2 2- , O 2- , S 2- or N 3- One or more of; the polyanion is XO m n- or X m O 3m+1 n- , X is one or more of B, S, C, P, Si, As, Mo, W or C;

[0014] MB y Wherein M is one or more of Zr, Hf, Ta, Nb, Al, Fe, Ga, In, Mo, W, Y, Ti, Si, B and Sb, and B is one or more of halogen, S or O.

[0015] Preferably, when A is a polyanion, the B element in the van der Waals crystal is replaced by XO m n- or X m O 3m+1 n- The O element in is substituted.

[0016] Preferably, the C e MB f and CB are nanocrystals, and the content of the nanocrystals in the amorphous solid solution type solid electrolyte is less than 30wt.%.

[0017] Frame structure (C a A b ) x -MB y Granular, C e MB f or CB on the surface of the particles.

[0018] Preferably, the range of x is 0.2-2, and the range of y is 3-6.

[0019] The method for preparing the amorphous solid solution type solid electrolyte comprises the following steps: mixing C a A b Powder and MB y The powders were mixed and solid-phase reacted by mechanical ball milling to obtain the target product (C a A b ) c -MB y .

[0020] Preferably, the ball milling time is 1 h to 30 h, and the ball milling speed is 400 rpm to 800 rpm.

[0021] Preferably, the powder is annealed after ball milling.

[0022] Preferably, the annealing temperature is 200-500° C., and the annealing environment is an inert atmosphere or a vacuum environment.

[0023] A solid-state battery is an all-solid-state lithium battery, comprising a positive electrode sheet, a negative electrode sheet, and a solid electrolyte sheet between the positive electrode sheet and the negative electrode sheet, wherein the material of the solid electrolyte sheet is the amorphous solid solution solid electrolyte described in any one of the above items.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention discloses an amorphous solid solution type solid electrolyte, wherein the functionalized solid electrolyte comprises a carrier salt C a A b and van der Waals MB with van der Waals crystal structure y Composition, C a A b Part of the anion A in the carrier salt replaces part of the B element in the compound with a van der Waals crystal structure, so that the carrier salt and the compound with a van der Waals crystal structure form a framework structure. Because part of the anion A in the carrier salt replaces part of the B element, part of the cation C is dissociated and released, and the dissociated cation C and MB y Or B forms nanocrystals, making the van der Waals crystal MB y Acts as a solid solvent, capable of dissociating a variety of salts C a A b And form a solid solution electrolyte, which is universal and helps to expand the electrolyte system. The amorphous solid solution solid electrolyte realizes solid electrolyte engineering and develops functional solid electrolytes, including solid electrolytes with high air stability, solid electrolytes that can match Li metal negative electrodes, and solid electrolytes that support extremely low temperatures and high rates.

[0026] The solid solution electrolyte of the present invention has high room temperature ionic conductivity because the cation C is removed from the salt C a A b After being dissociated, it is filled with anions A and solvent [MB y ](or [MB y ] n ) in the framework, the interaction force with the anions in the framework is weak, and the framework has a large, three-dimensional free volume, so the mobility of the cation C in the framework structure is high, showing high room temperature ionic conductivity.

[0027] The universality of van der Waals crystal solvent dissociation salts brings a variety of candidate lithium salts and solvents, providing flexibility for designing solid electrolyte components. a A b After being dissociated in the electrolyte, it is easier to participate in the formation of SEI at the electrolyte / electrode interface; and because the solid solution electrolyte has a disordered characteristic similar to that of a liquid electrolyte, ion transport does not depend on a specific crystal structure, and the reduction of A ions will not affect the transport of cation C. Therefore, by designing salt C a A b By regulating the anions in the SEI, we can develop functional solid electrolytes through solid electrolyte engineering and optimize the performance of all-solid-state batteries.

[0028] Furthermore, the framework-type solid solution-type solid electrolyte provided by the present invention is in the form of particles on a macroscopic scale, most of the particles are in an amorphous phase, and a small amount of nanocrystals are distributed on the surface of the particles as by-products. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a typical structural unit of van der Waals crystals SiI4, TaCl5, HfCl4, AlCl3, NbOCl3, and AlOCl;

[0030] Figure 2 It is a pair distribution function diagram of the Li2O-ZrCl4 solid electrolyte provided in Example 1 of the present invention; in the figure, the horizontal axis "r" represents the distance; and the vertical axis "G" represents the atomic pair distribution function.

[0031] Figure 3 It is an open frame structure diagram of the Li2O-ZrCl4 solid electrolyte provided in Example 1 of the present invention.

[0032] Figure 4 This is the X-ray absorption fine structure spectrum of the Li2SO4-ZrCl4 solid electrolyte provided in Example 2 of the present invention. In the figure, the horizontal axis "R" represents the distance; the vertical axis "FT" represents k 3The modulus of the weighted extended X-ray fine structure after Fourier transformation.

[0033] Figure 5 It is a distribution function diagram of the Li2SO4-ZrCl4 solid electrolyte provided in Example 2 of the present invention.

[0034] In the figure, the horizontal axis "r" represents the distance; the vertical axis "G" represents the atomic pair distribution function.

[0035] Figure 6 This is a local structure analysis diagram of the Li2SO4-ZrCl4 solid electrolyte provided in Example 2 of the present invention.

[0036] Figure 7 It is the X-ray diffraction spectrum of Li2CO3-HfCl4, Li2SO4-HfCl4, Li2CO3-ZrCl4, Li2SO4-ZrCl4, Li2O-TaCl5, 2 / 3Li3PO4-ZrCl4, Li2C2O4-TaCl5 lithium salt-van der Waals crystal solid solution type solid electrolyte in the embodiment of the present invention. In the figure, the horizontal axis represents the diffraction angle (2Theta), the unit is degree (°); the vertical axis represents the diffraction intensity.

[0037] Figure 8 The X-ray diffraction spectra of the solid electrolyte Li2O-ZrCl4 prepared by different ball milling times in Example 1 of the present invention are shown in FIG. In the figure, the abscissa represents the diffraction angle (2Theta), the unit is degree (°); the ordinate represents the diffraction intensity.

[0038] Fig. 9 This is a high-resolution cryo-transmission electron micrograph of the solid electrolyte Li2O-ZrCl4 prepared in Example 1 of the present invention. In the figure, the nanocrystals are LiCl.

[0039] Fig.10 This is the EDS surface scan of the Ag2O-ZrCl4 solid electrolyte synthesized in Example 8 of the present invention, including the surface scans of Ag, Zr, and Cl elements.

[0040] Fig.11 The band gap of nanocrystals at different stages in the solid electrolyte Li2O-ZrCl4 solid electrolyte prepared in Example 1 of the present invention is calculated by first principles.

[0041] Fig.12 The charge and discharge curve of the all-solid-state lithium battery assembled in Example 9 of the present invention at a rate of 0.1C for the first three weeks. In the figure, the horizontal axis represents the specific capacity in milliampere hours per gram (mAh g -1 ); the ordinate represents voltage (relative to Li + / Li voltage), the unit is volt (V).

[0042] Fig.13 The electrochemical performance of the battery assembled using 2 / 3Li3PO4-ZrCl4 solid electrolyte in Example 10 of the present invention and the battery assembled using comparative example Li2ZrCl6 solid electrolyte in Example 11 in the first 100 weeks. The rate was 0.1C in the first three weeks and 1C after 3 weeks. In the figure, the horizontal axis represents the number of cycles; the vertical axis on the left represents the specific capacity in milliampere hours per gram (mAh g -1 ); the vertical axis on the right represents the Coulomb efficiency. DETAILED DESCRIPTION

[0043] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0044] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0045] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0046] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the present invention equally.

[0047] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0048] In one aspect of the present invention, an amorphous solid solution type solid electrolyte is provided, the general formula of the solid electrolyte is (C a A b ) x -MB y , where C a A bis a carrier salt, where a and b are the atomic numbers of the cation C and the anion A in the carrier salt, respectively, and MB y is a van der Waals crystal, y is the atomic number of element B, and x is C a A b and MB y is the stoichiometric ratio; C e MB f where e and f in MB are the stoichiometric numbers of C and MB, respectively.

[0049] The said C a A b partially replaces part of element B in the van der Waals crystal with the anion A in it. While connecting C a A b and MB y together, a framework structure is formed, and the dissociated cation C is in the framework structure; C is attached outside the framework structure e MB f and CB, and e and f in C e MB f are the stoichiometric numbers of the cation C and MB, respectively.

[0050] In the above structure, because part of the anion A in the carrier salt replaces part of element B, some cations C are dissociated and released. The dissociated and released cation C and MB y or B form nanocrystals, that is, C e MB f and CB. However, the interaction force between C and MB y or B is weak, enabling C to shuttle and migrate in a relatively large and three-dimensional framework, resulting in a high mobility of the cation C in this framework structure and exhibiting high room-temperature ionic conductivity.

[0051] Among them, 0.2 < x < 2, y is 3 to 6, and x is when setting MB y to 1 mole, C a A b and MB y is the mixed molar ratio.

[0052] In some embodiments of the present invention, C a A b includes one or more of lithium salts, sodium salts, silver salts, copper salts, potassium salts, and C is Li + or Na + or Ag + or Cu + or K + cation, A is a simple anion or a polyanion or a mixture thereof. The simple anions include halogens, OH - 、NH2 - 、O2 2-, O 2- , S 2- 、N 3- One or more of; polyanions include XO m n- and X m O 3m+1 n- , X is one or more of B, S, C, P, Si, As, Mo, W, and O is oxygen. XO m n- Where m is the number of oxygen atoms in the polyanion, n- is the valence state of the polyanion; X m O 3m+1 n- Here, m is the number of atoms of element X in the anion, and n- is the valence state of the polyanion.

[0053] Example C a A b Can be: Li2O, Li2S, Li3N, LiOH, Li3N, Li2O2, LiBO2, Li4SiO4, Li2MoO3, Li2CO3, Li3PO4, Li2SO4, Na2O, Na2S, Na3N, NaOH, Na3N, Na2O2, NaBO2, Na4SiO4, Na2MoO3, Na2CO3, Na3P O4, Na2SO4, K2O, K2S, K3N, KOH, K2O2, KBO2, K4SiO4, K2MoO3, K2CO3, K3PO4, K2SO4, Ag2 O, Ag2S, Ag3N, AgOH, Ag3N, Ag2O2, AgBO2, Ag4SiO4, Ag2MoO3, Ag2CO3, Ag3PO4, Ag2SO4.

[0054] MB y is a van der Waals crystal, which is a compound having a van der Waals crystal structure. In some embodiments of the present invention, MB y It is one or more of halide van der Waals crystals, sulfide van der Waals crystals and oxide van der Waals crystal materials.

[0055] Preferably, M is one or more of Zr, Hf, Ta, Nb, Al, Fe, Ga, In, Mo, W, Y, Ti or V; B is one or more of halogen, S or O, MB y It can also be one or more of SiI4, BI3, SbI3.

[0056] Exemplary, MB yCan be ZrCl4, HfCl4, TaCl5, NbCl5, AlCl3, FeCl3, GaCl3, InCl3, YCl3, MoCl5, MoCl6, WCl6, SiI4, BI3, SbI3, NbOCl3, AlOCl, WOCl4, TiOCl, VOCl.

[0057] Van der Waals crystals, also known as inorganic molecular crystals, are formed by the accumulation of zero-dimensional, one-dimensional or two-dimensional structural units under the action of van der Waals forces (intermolecular forces). y The structural elements of van der Waals crystals include the zero-dimensional [MB y ] polyhedron (e.g. [SiI4] tetrahedron in SiI4 van der Waals crystal) and its dimer / polymer (e.g. [TaCl5]2 dimer in TaCl5 van der Waals crystal), [MB y ]One-dimensional chain polymer formed by the shared edges of polyhedrons[MB y ] n (such as [ZrCl4] in ZrCl4 van der Waals crystals n chain) and by [MB y ]Two-dimensional layered polymers formed by shared edges of polyhedrons [MB y ] n (such as [AlCl3] in AlCl3 van der Waals crystals n layer); the structural unit of a typical van der Waals crystal is shown in the attached Figure 1 .

[0058] In the present invention, the van der Waals crystal MB y C a A b The dissociation ability of van der Waals crystal MB y It has a characteristic structure in which the structural elements are connected by van der Waals forces, similar to the solvent of the liquid electrolyte. The van der Waals forces are easily destroyed under the action of mechanical energy (ball milling in the preparation process), providing good solid-phase diffusion conditions and facilitating [MB y ](or [MB y ] n ) Structural elements and salt C a A b Form atomic-level contact; on the other hand, due to the M cation in its structural unit and the salt C a A b The A anions have strong interactions, similar to the solvation effect in liquid electrolytes, which realizes the C a A b Dissociation and reconstruction of C and A.

[0059] The amorphous solid solution type solid electrolyte material (C a A b )c -MB y Structurally, van der Waals crystal MB y By salt C a A b The anion A in the Figure 1 ), and the cation C fills the vacancies in the open framework to form an amorphous solid solution with long-range disorder and short-range order, which has a large free volume. Furthermore, its short-range structural feature is that when A is a simple anion, A replaces the van der Waals crystal structure unit [MB y ](or [MB y ] n ) and multiple [MB y ](or [MB y ] n ) are connected to form a framework structure. When A is a polyanion XO m and X m O 3m+1 When [MB y ](or [MB y ] n ) is replaced by O and by XO m and X m O 3m+1 The polyhedrons are connected into a network to form a framework structure, and the structural framework can be detected by characteristic peaks in the distribution function (PDF) including but not limited to the following CB, MO, and MX characteristic peaks.

[0060] In some embodiments of the present invention, the framework structure (C a A b ) x -MB y It is granular in macroscopic appearance, with a small amount of nanocrystalline phase on the surface, and its crystal content is less than 30wt.%, which is C e MB f , CB or one or more of the residual raw material phases. The nanocrystals are concentrated on the surface of the particles, and the interior of the particles is mainly amorphous solid solution, forming a "core-shell" structure. By regulating the composition and size of the nanocrystalline phase, the air stability of the material can be improved, and the grain boundary electronic conductivity after cold pressing of the powder can be reduced.

[0061] The room temperature carrier conduction rate of the amorphous solid solution solid electrolyte material of the present invention is>10 -5 mS / cm, can be well used in all-solid-state battery systems as a solid-phase electrolyte material and carrier conduction material additive.

[0062] The second aspect of the present invention discloses a method for preparing an amorphous solid solution type solid electrolyte, the specific process is: in an inert atmosphere without water and oxygen, the raw material C is mixed at a stoichiometric ratio of x:1. a A b Powder and MB y The powders were mixed in a ball mill and solid phase reaction occurred by mechanical ball milling to obtain the target product (C a A b ) c -MB y .

[0063] In some embodiments of the present invention, the anhydrous and oxygen-free inert atmosphere is N2 or Ar gas, preferably, Ar gas is used.

[0064] In some embodiments of the present invention, the grinding beads in the mechanical ball milling process are one or more grinding beads with a diameter of 3 mm to 10 mm, such as grinding beads with a diameter of 3 mm, 5 mm, and 10 mm.

[0065] In some embodiments of the present invention, the total mass ratio of grinding beads to raw materials (ie, the ball-to-material ratio) is 60:1 to 20:1; for example, the material-to-ball ratio is 20:1, 40:1, or 60:1.

[0066] As a more preferred solution, 3 mm grinding beads are used with a ball-to-material ratio of 30:1.

[0067] In some embodiments of the present invention, the ball milling time is 1 h to 30 h, such as 1.5 h, 5 h, 10 h, 20 h, 30 h; and the ball mill speed is 400 rpm to 800 rpm.

[0068] As a more preferred solution, the ball milling time is 5 h and the ball mill speed is 500 rpm.

[0069] It should be noted that too long ball milling time or too high ball milling speed may lead to the formation of CB crystal phase and a decrease in ionic conductivity. By adjusting the ball milling parameters, an amorphous solid solution electrolyte with the highest ionic conductivity or an electronically insulating and air-stable amorphous solid solution electrolyte containing a small amount of nanocrystals can be obtained.

[0070] In some embodiments of the present invention, the ball-milled powder may be subjected to an annealing treatment.

[0071] The above annealing treatment needs to be performed in an Ar or N2 inert atmosphere or in a vacuum. Preferably, a vacuum is used.

[0072] The annealing temperature is 200-500°C and the annealing time is 3h.

[0073] In the preparation of solid solution type solid electrolytes using the above scheme, the relative ratio of amorphous phase and crystalline phase, and the composition of crystalline phase are controlled by the synthesis conditions, including ball milling parameters (ball milling time, speed), raw material ratio, annealing conditions, etc. During the ball milling process, the residual raw material crystalline phase decreases until it disappears, and C e MB f Nanocrystals appear. Crystalline phase C e MB f The M content in the amorphous solid solution electrolyte gradually decreases and eventually evolves into CB. By optimizing the ball milling parameters, the composition and ionic conductivity of the amorphous solid solution electrolyte can be controlled. Figure 8 As shown in the figure, during the ball milling process of preparing Li2O-ZrCl4, when the ball milling speed is 600 rpm and the ball milling time is 20 h, the crystal phase of the obtained product is less, and the ionic conductivity is the highest at this time, which is 3.0×10 -3 S cm -1 When the ball milling time is 15h, the crystal phase of the obtained product is Li2ZrCl6; when the ball milling time is 80h, the crystal phase of the obtained product is LiCl. For example, in the process of preparing Li2O-ZrCl4 by ball milling, the crystal phase gradually evolves from Li2O to Li2ZrCl6 and finally to LiCl. The X-ray diffraction pattern evolution is shown in the attached figure. Figure 8 As shown in Figure 2, the nanocrystals with high Li content and low Zr content have larger electronic band gap and lower electronic conductivity. Fig.11 As shown in Figure 2, the reactivity with water molecules in humid air is weaker (better air stability). Therefore, by adjusting the ratio and composition of nanocrystals, the air stability and grain boundary electronic conductivity after powder cold pressing can be optimized.

[0074] The third aspect of the present invention discloses a solid-state battery, which is an all-solid-state lithium battery, wherein the all-solid-state lithium battery contains the above-mentioned solid solution type solid electrolyte. The all-solid-state lithium battery comprises a positive electrode sheet, a negative electrode sheet, and a solid electrolyte sheet between the positive and negative electrodes.

[0075] The solid electrolyte sheet is obtained by cold pressing a solid electrolyte material, wherein the solid electrolyte material is one of the above-mentioned solid solution type solid electrolytes or a solid electrolyte obtained according to the preparation method of the above-mentioned solid solution type solid electrolyte.

[0076] The positive electrode sheet is obtained by cold pressing or coating the positive electrode active material and the positive electrode filler. The positive electrode active material includes but is not limited to cobalt aluminum oxide, lithium iron phosphate, lithium-rich lithium manganese oxide, lithiated layered oxide, lithiated layered sulfide, or a combination thereof. The positive electrode filler is an ion conductor, a conductive agent, an adhesive, or a combination thereof; the ion conductor and the solid electrolyte between the positive and negative electrodes of the battery are the same material; the conductive agent may include graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or a combination thereof; the adhesive may include, for example, styrene-butadiene rubber, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, or a combination thereof. Cold pressing or coating methods are common methods for preparing positive electrode sheets in the art.

[0077] The negative electrode sheet is obtained by cold pressing or coating the negative electrode active material and the negative electrode filler. The negative electrode active material refers to the material that can store and release Li + Ionic materials include but are not limited to metal materials, graphite, and silicon; metal materials can be single metals or alloys; when metal materials are used as negative electrode active materials, negative electrode fillers can be omitted. Negative electrode fillers are ion conductors, conductive agents, adhesives, or combinations thereof; the ion conductors and the solid electrolytes between the positive and negative electrodes of the battery are of the same material; conductive agents may include graphite, carbon black, acetylene black, Ketjen black, carbon fibers, or combinations thereof; adhesives may include, for example, styrene-butadiene rubber, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, or combinations thereof. Cold pressing or coating methods are common methods for preparing negative electrode sheets in the art.

[0078] The following is further described in conjunction with specific embodiments.

[0079] Example 1

[0080] This embodiment provides a solid solution type solid electrolyte Li2O-ZrCl4, and the specific preparation method is as follows:

[0081] In an argon atmosphere glove box without water or oxygen, Li2O and ZrCl4 were mixed in a molar ratio of 1:1 and hand-ground with an agate mortar for 10 min to mix them thoroughly.

[0082] The mixed powder (about 2g) was transferred to a 75mL ball mill, and 60g of grinding beads with a diameter of 3mm were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 550 rpm for 20h. The ball mill was cooled with circulating water during the ball milling process. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized Li2O-ZrCl4 solid solution solid electrolyte.

[0083] Example 2

[0084] This embodiment provides solid solution type solid electrolytes Li2O-HfCl4, Li2S-HfCl4 and Li3N-HfCl4, and the specific preparation methods are as follows:

[0085] In an argon atmosphere glove box without water or oxygen, Li2O and HfCl4 were mixed at a molar ratio of 1:1 and hand-ground using an agate mortar for 10 min to mix thoroughly.

[0086] The mixed powder (about 2 g) was transferred to a 75 mL ball mill, and 60 g of grinding beads with a diameter of 3 mm were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 550 rpm for 20 h. The ball mill was cooled with circulating water during the ball milling process. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized Li2O-HfCl4 solid solution solid electrolyte.

[0087] According to the above steps, Li2S-HfCl4 and Li3N-HfCl4 solid solution type solid electrolytes are synthesized respectively, the difference being that the raw material Li2O is replaced by Li2S and Li3N respectively.

[0088] Example 3

[0089] This embodiment provides solid electrolytes Li2SO4-HfCl4 and 2 / 3Li3PO4-HfCl4, and the specific preparation methods are as follows:

[0090] In an anhydrous and oxygen-free argon atmosphere glove box, Li2SO4 and HfCl4 were mixed in a substance ratio of 1:1 and hand-ground using an agate mortar for 10 min to fully mix.

[0091] The mixed powder (about 1g) was transferred to a 75mL ball mill, and 40g of grinding beads with a diameter of 3mm were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600 rpm for 1.5h. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized Li2SO4-HfCl4 solid electrolyte.

[0092] According to the above steps, a 2 / 3Li3PO4-HfCl4 solid electrolyte is synthesized, the difference being that the raw material Li2SO4 is replaced by Li3PO4, and the molar ratio is replaced by 2 / 3:1.

[0093] Example 4

[0094] This embodiment provides a solid electrolyte Li2SO4-ZrCl4, and the specific preparation method is as follows:

[0095] In an anhydrous and oxygen-free argon atmosphere glove box, Li2SO4 and ZrCl4 were mixed in a substance ratio of 1:1 and hand-ground using an agate mortar for 10 min to fully mix.

[0096] The mixed powder (about 1g) was transferred to a 75mL ball mill, and 40g of grinding beads with a diameter of 3mm were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600 rpm for 1.5h. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized Li2SO4-ZrCl4 solid electrolyte.

[0097] Example 5

[0098] This embodiment provides solid electrolytes Li2SO4-TaCl5 and 2 / 3Li3PO4-TaCl5. The specific preparation method is as follows:

[0099] In an anhydrous and oxygen-free argon atmosphere glove box, Li2SO4 and TaCl5 were mixed in a substance ratio of 1:1 and hand-ground using an agate mortar for 10 min to fully mix.

[0100] The mixed powder (about 1g) was transferred to a 75mL ball mill, and 40g of grinding beads with a diameter of 3mm were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600 rpm for 1h. After the ball milling was completed, the ball mill was transferred to a glove box, opened, and the powder in the jar was taken out, which was the synthesized Li2SO4-TaCl5 solid electrolyte.

[0101] According to the above steps, 2 / 3Li3PO was synthesized 4- TaCl5 solid electrolyte, the difference is that the raw material Li2SO4 is replaced by Li3PO4, and the molar ratio is replaced by 2 / 3:1.

[0102] Example 6

[0103] This embodiment provides a solid electrolyte Li3PO4-SiI4. The specific preparation method is as follows:

[0104] In an anhydrous and oxygen-free argon atmosphere glove box, Li3PO4 and SiI4 were mixed in a substance ratio of 1:1 and hand-ground using an agate mortar for 10 min to fully mix.

[0105] The mixed powder (about 1g) was transferred to a 75mL ball mill, and 40g of grinding beads with a diameter of 3mm were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600 rpm for 1h. After the ball milling was completed, the ball mill was transferred to a glove box, opened, and the powder in the jar was taken out, which was the synthesized Li3PO4-SiI4 solid electrolyte.

[0106] The ball milling speed can be 500 rpm, and the ball milling time can be 5 h.

[0107] Example 7

[0108] This embodiment provides a solid electrolyte 2 / 3Li3PO4-(AlCl3) 1 / 5 (ZrCl4) 1 / 5 (HfCl4) 1 / 5 (TaCl5) 1 / 5 (NbCl5) 1 / 5 The specific preparation method is as follows:

[0109] In an anhydrous and oxygen-free argon atmosphere glove box, Li3PO4, AlCl3, ZrCl4, HfCl4, TaCl5, and NbCl5 were mixed in a molar ratio of 2 / 3:1 / 5:1 / 5:1 / 5:1 / 5:1 / 5, and hand-ground using an agate mortar for 10 min to mix thoroughly.

[0110] The mixed powder (about 1g) was transferred to a 75mL ball mill, and 40g of 3mm diameter grinding beads were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600 rpm for 2h. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized 2 / 3Li3PO4-(AlCl3) 1 / 5 (ZrCl4) 1 / 5 (HfCl4) 1 / 5 (TaCl5) 1 / 5 (NbCl5) 1 / 5 Solid electrolyte.

[0111] The ball milling speed can be 400 rpm or 800 rpm, and the corresponding ball milling time can be 30 h and 0.5 h.

[0112] Example 8

[0113] This embodiment provides solid electrolytes 0.2Li2CO3-HfCl4, 0.5Li2CO3-HfCl4, 0.8Li2CO3-HfCl4, Li2CO3-HfCl4, 1.5Li2CO3-HfCl4, 2Li2CO3-HfCl4, and the specific preparation method is as follows:

[0114] In an anhydrous and oxygen-free argon atmosphere glove box, Li2CO3 and HfCl4 were mixed in a substance ratio of 1:1 and hand-ground using an agate mortar for 10 min to fully mix.

[0115] The mixed powder (about 1 g) was transferred to a 75 mL ball mill, and 40 g of grinding beads with a diameter of 3 mm were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600 rpm for 1.5 h. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized Li2CO3-HfCl4 solid electrolyte.

[0116] According to the above steps, 0.2Li2CO3-HfCl4 solid electrolyte is synthesized, except that the molar ratio is replaced by 0.2:1. According to the above steps, 0.5Li2CO3-HfCl4 solid electrolyte is synthesized, except that the molar ratio is replaced by 0.5:1. According to the above steps, 0.8Li2CO3-HfCl4 solid electrolyte is synthesized, except that the molar ratio is replaced by 0.8:1. According to the above steps, 1.5Li2CO3-HfCl4 solid electrolyte is synthesized, except that the molar ratio is replaced by 1.5:1. According to the above steps, 2Li2CO3-HfCl4 solid electrolyte is synthesized, except that the molar ratio is replaced by 2:1.

[0117] Example 9

[0118] This embodiment provides a solid electrolyte (Li2CO3)1 / 3(Li3PO4)1 / 3(Li2SO4)1 / 3-HfCl4.

[0119] Specifically, the (Li2CO3)1 / 3(Li3PO4)1 / 3(Li2SO4)1 / 3-HfCl4 solid electrolyte is synthesized according to the preparation method provided in Example 6, with the difference that the raw materials and their amounts are replaced by Li2CO3, Li3PO4, Li2SO4 and HfCl4 mixed in a material ratio of 1 / 3:1 / 3:1 / 3:1.

[0120] Example 10

[0121] This embodiment provides a composite halide solid electrolyte Ag2O-ZrCl4.

[0122] Specifically, the Ag2O-ZrCl4 halide solid electrolyte was synthesized according to the preparation method provided in Example 1, except that the raw material Li2O was replaced by Ag2O.

[0123] Embodiment 11

[0124] This embodiment provides a solid electrolyte Li2CO3-AlCl3, and the specific preparation method is as follows:

[0125] In an anhydrous and oxygen-free argon atmosphere glove box, Li2CO3 and AlCl3 were mixed in a substance ratio of 1:1 and hand-ground using an agate mortar for 10 min to fully mix.

[0126] The mixed powder (about 1g) was transferred to a 75mL ball mill, and 40g of grinding beads with a diameter of 3mm were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600 rpm for 20h. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized Li2CO3-AlCl3 solid electrolyte.

[0127] Example 12

[0128] This embodiment provides a solid electrolyte 0.5Li4SiO4-MoCl6, and the specific preparation method is as follows:

[0129] In an anhydrous and oxygen-free argon atmosphere glove box, Li4SiO4 and MoCl6 were mixed at a molar ratio of 0.5:1 and hand-ground using an agate mortar for 10 min to fully mix.

[0130] The mixed powder (about 1g) was transferred to a 75mL ball mill, and 40g of 3mm diameter grinding beads were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600 rpm for 20h. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized 0.5Li4SiO4-MoCl6 solid electrolyte.

[0131] Example 13

[0132] This embodiment provides a solid electrolyte 0.5Li4SiO4-NbCl5, and the specific preparation method is as follows:

[0133] In an anhydrous and oxygen-free argon atmosphere glove box, Li4SiO4 and NbCl5 were mixed at a molar ratio of 0.5:1 and hand-ground using an agate mortar for 10 min to fully mix.

[0134] The mixed powder (about 1g) was transferred to a 75mL ball mill, and 40g of grinding beads with a diameter of 3mm were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600 rpm for 20h. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized 0.5Li4SiO4-NbCl5 solid electrolyte.

[0135] Embodiment 14

[0136] This embodiment provides a solid electrolyte 0.5Li2CO3-NbOCl3, and the specific preparation method is as follows:

[0137] In an anhydrous and oxygen-free argon atmosphere glove box, Li2CO3 and NbOCl3 were mixed at a molar ratio of 0.5:1 and hand-ground using an agate mortar for 10 min to fully mix.

[0138] The mixed powder (about 1g) was transferred to a 75mL ball mill, and 40g of 3mm diameter grinding beads were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600 rpm for 20h. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized 0.5Li2CO3-NbOCl3 solid electrolyte.

[0139] Embodiment 15

[0140] This embodiment provides a solid electrolyte 0.5Li2CO3-AlOCl, and the specific preparation method is as follows:

[0141] In an anhydrous and oxygen-free argon atmosphere glove box, Li2CO3 and NbOCl3 were mixed at a molar ratio of 0.5:1 and hand-ground using an agate mortar for 10 min to fully mix.

[0142] The mixed powder (about 1g) was transferred to a 75mL ball mill, and 40g of 3mm diameter grinding beads were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600 rpm for 20h. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized 0.5Li2CO3-NbOCl3 solid electrolyte.

[0143] Example 16

[0144] This embodiment provides an all-solid-state lithium battery, which is assembled using the solid solution type solid electrolyte 2 / 3Li3PO4-HfCl4 provided in Example 1. The specific assembly process is as follows:

[0145] Step 1: Weigh 120 mg of the solid solution solid electrolyte 2 / 3Li3PO4-HfCl4 powder synthesized in Example 1, and cold press it into a solid electrolyte sheet with a diameter of 10 mm at a pressure of 100 MPa for 2 minutes.

[0146] Step 2: Weigh the commercially available lithiated layered oxide LiNi 0.88 Co 0.06 Mn 0.06O2 (as positive electrode active material) and 2 / 3Li3PO4-HfCl4 (as ion conductor) with a mass ratio of 7:3 are manually ground in a mortar for 10 minutes until uniformly mixed; 10 mg of the mixed powder is weighed and evenly spread on one side of the solid electrolyte sheet prepared in step 1, and cold pressed at a pressure of 350 MPa for 2 minutes to form a double-layer structure of "positive electrode sheet-solid electrolyte sheet".

[0147] Step 3: Use a commercially available indium sheet (10 mm in diameter and 200 μm in thickness) as the negative electrode active material, and stick it on the other surface of the solid electrolyte sheet in the double-layer structure prepared in step 2 to form a three-layer structure of "positive electrode sheet-solid electrolyte sheet-negative electrode sheet". Apply a pressure of 75 MPa to the whole structure, and complete the assembly to obtain an all-solid-state lithium battery.

[0148] The steps 1 to 3 are all carried out in a glove box with an anhydrous and oxygen-free argon atmosphere.

[0149] At room temperature, the all-solid-state battery was tested for cycle performance using a Blue Electric battery testing system with a voltage range of 2.5V to 4.3V (voltage relative to Li+ / Li). The first three cycles were activated at a rate of 0.3C, and from the fourth cycle onwards a rate of 1C was used.

[0150] Embodiment 17

[0151] The method described in Example 11 was used to assemble the all-solid-state LiIn-LiNi 0.88 Co 0.06 Mn 0.06 O2 (LiIn-NMC88) battery, the difference is: the solid electrolyte used is the 2 / 3Li3PO4-ZrCl4 solid electrolyte synthesized in the embodiment, and the process of preparing the composite positive electrode is carried out in a drying room with a dew point of -50°C.

[0152] Embodiment 18

[0153] The method described in Example 12 was used to assemble all-solid-state LiIn-LiNi 0.88 Co 0.06 Mn 0.06 O2 (LiIn-NMC88) battery, the difference is that the solid electrolyte used is the Li2ZrCl6 electrolyte of Comparative Example 1.

[0154] Embodiment 19

[0155] In this embodiment, the powder in the jar after ball milling is subjected to vacuum annealing treatment in an Ar atmosphere, with an annealing temperature of 300° C. and an annealing time of 3 h.

[0156] Embodiment 20

[0157] In this embodiment, the powder in the jar after ball milling is subjected to vacuum annealing treatment in an Ar atmosphere, with an annealing temperature of 200° C. and an annealing time of 3 h.

[0158] Embodiment 21

[0159] In this embodiment, the powder in the jar after ball milling is subjected to vacuum annealing treatment in an Ar atmosphere, with an annealing temperature of 500° C. and an annealing time of 3 h.

[0160] Comparative Example 1

[0161] This case provides a solid electrolyte, and the specific preparation method is as follows:

[0162] In an anhydrous and oxygen-free argon atmosphere glove box, LiCl and ZrCl4 were mixed at a molar ratio of 2:1 and hand-ground using an agate mortar for 10 min to fully mix.

[0163] The mixed powder (about 2g) was transferred to a 75mL ball mill, and 60g of grinding beads with a diameter of 3mm were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 550 rpm for 20h. The ball mill was cooled with circulating water during the ball milling process. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized Li2ZrCl6 halide solid electrolyte.

[0164] The materials obtained in the examples and their corresponding properties are analyzed below.

[0165] 1. Characterization of ionic conductivity

[0166] (1) Characterization methods

[0167] In a water-free and oxygen-free argon atmosphere glove box, the amorphous solid solution solid electrolyte powder prepared in the example was filled into a cylindrical tablet pressing mold (with a diameter of 10 mm); and cold pressed at a pressure of 375 MPa for 2 min to obtain a solid electrolyte sheet with a thickness of 0.5 to 1.5 mm and a diameter of 10 mm; after gold plating on the upper and lower surfaces of the solid electrolyte sheet, two stainless steel blocking electrodes were used to clamp the upper and lower surfaces, and the electrochemical workstation was connected to test the electrochemical impedance spectrum at room temperature; room temperature Li + Ionic conductivity, test results are shown in Table 1.

[0168] (2) Characterization results

[0169] Carrier Salt C a A b The ionic conductivity is less than 10 -7 S cm -1 , and van der Waals crystal MB yThe ionic conductivity of the amorphous solid solution electrolyte prepared after mixing is greater than 10 -3 S cm -1 .

[0170] 2. Local structure analysis

[0171] (1) Characterization methods

[0172] The Li2O-ZrCl4 and Li2SO4-ZrCl4 solid electrolytes synthesized in the examples were characterized using Fourier transform infrared spectroscopy, X-ray absorption spectroscopy and pair distribution function.

[0173] (2) Characterization results

[0174] Figure 2 is the pair distribution function of Li2O-ZrCl4 solid electrolyte. After local structure analysis, it can be determined that the local structure is: the Cl part of the [ZrCl6] octahedron is replaced by O, and multiple [ZrCl6] polyhedra are connected by O, such as Figure 3 shown.

[0175] Figure 4 is the pair distribution function of Li2SO4-ZrCl4 solid electrolyte, Figure 5 The X-ray absorption spectrum of Li2SO4-ZrCl4 solid electrolyte is shown in Figure 2. After local structure analysis, it can be determined that the local structure is: the Cl part of the [ZrCl6] octahedron is replaced by O, and multiple ZrCl6 polyhedrons are connected by multiple O of SO4 tetrahedron, such as Figure 6 This local structure constitutes an open framework structure with a cross-linked network skeleton and three-dimensional channels running through it, in which the Li ions fill the vacancies.

[0176] 3. Crystal structure characterization and analysis

[0177] (1) Characterization methods

[0178] The solid electrolyte prepared in the example was characterized using an X-ray diffractometer.

[0179] (2) Characterization results

[0180] like Figure 7 As shown, the X-ray diffraction spectra of solid electrolytes Li2CO3-HfCl4, Li2SO4-HfCl4, Li2CO3-ZrCl4, Li2SO4-ZrCl4, Li2O-TaCl5, 2 / 3Li3PO4-ZrCl4, and Li2C2O4-TaCl5 lithium salt-van der Waals crystal solid solution type solid electrolytes are characterized respectively. The results show that none of the 7 solid electrolytes have obvious diffraction peaks, indicating that the above 7 solid solution type solid electrolytes are disordered amorphous phases.

[0181] Figure 8 The crystal structure of Li2O-ZrCl4 solid electrolyte evolves with ball milling time. During the whole ball milling process, the diffraction peak is broad and the intensity is low, indicating that Li2O-ZrCl4 electrolyte is a mostly amorphous material with a small amount of nanocrystalline. The change of nanocrystalline is: the raw material Li2O phase gradually disappears, then the Li2ZrCl6 crystal phase appears, and finally turns into LiCl.

[0182] 4. Microstructure characterization and analysis

[0183] (1) Characterization methods

[0184] The microstructure of the solid solution-type solid electrolyte synthesized in the example was characterized using high-resolution cryo-transmission electron microscopy.

[0185] (2) Characterization results

[0186] The characterization results are as follows Fig. 9 As shown, the results show that the Li2O-ZrCl4 solid solution electrolyte is mostly disordered amorphous phase, the crystalline phase is LiCl, the grain size is about 10nm, and the crystalline phase is enriched on the particle surface.

[0187] Crystal structure characterization analysis and microstructure characterization analysis show that lithium salts with different anions react with van der Waals crystals to obtain materials with similar crystal structures and microstructures, and have high ionic conductivity. This solid-phase reaction behavior is similar to the dissociation behavior of salts in solution, and can be understood as the dissociation behavior of lithium salts (solutes) in van der Waals crystals (solid solvents).

[0188] Fig.10 The core-shell structure of the crystalline phase and amorphous phase in the Ag2O-ZrCl4 solid electrolyte is shown. The crystalline phase is AgCl. Fig.10 This indicates that the outer layer is enriched with Ag and Cl elements, and that the AgCl crystal phase is wrapped on the surface of the amorphous phase to form a core-shell structure.

[0189] 5. First principles calculation

[0190] (1) Characterization methods

[0191] The band gaps of the crystalline phases at various stages during the synthesis of the Li2O-ZrCl4 solid electrolyte were calculated using first-principles calculations.

[0192] (2) Characterization results

[0193] During the ball milling process, the residual raw material crystal phase decreases and eventually disappears, accompanied by LixZr (1-0.25x) Cl4 nanocrystals appear. Crystalline phase LixZr (1-0.25x)The Zr content in Cl4 gradually decreases and eventually evolves into LiCl. The band gap of nanocrystals with different values ​​of x was calculated by first principles. Fig.11 It shows that as x increases, that is, the Li content increases and the Zr content decreases, LixZr (1-0.25x) The band gap of Cl4 gradually increases, indicating that its electronic conductivity gradually decreases.

[0194] 5. Constant current charge and discharge test

[0195] (1) Test method

[0196] At room temperature, the BlueDian battery test system was used to perform constant current charge and discharge tests on the all-solid-state battery provided in Example 1. The voltage range was 2.5V to 4.3V (relative to the voltage of Li+ / Li) and the cycle rate was 0.1C.

[0197] (2) Test results

[0198] The test results are as follows Fig.12 shown.

[0199] The all-solid-state battery provided in Application Example 1 has a reversible capacity of 196.80 mAh g-1 at a rate of 0.1C, and the cycle efficiencies of the first and second cycles are 88.23% and 98.74% respectively.

[0200] Table 1 Ionic conductivity of solid electrolytes

[0201]

[0202]

[0203] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. Amorphous solid solution type solid electrolyte, characterized in that: The general formula is (C a A b ) x -MB y , the (C a A b ) x -MB y It is a frame structure; Among them, C a A b is the carrier salt, a and b are the atomic numbers of cation C and anion A in the carrier salt, respectively. y is a van der Waals crystal, y is the number of atoms of element B, x is the number of atoms of element C a A b and MB y The stoichiometric ratio; The B element in the van der Waals crystal is C a A b The anion A in the cation is partially replaced, and the dissociated cation C is in the framework structure; the C is attached to the outside of the framework structure. e MB f and CB, C e MB f Where e and f are the stoichiometric numbers of cations C and MB, respectively.

2. The amorphous solid solution type solid electrolyte according to claim 1, characterized in that: The van der Waals crystals are one or more of halide van der Waals crystals, sulfide van der Waals crystals or oxide van der Waals crystals; The carrier salt is one or more of lithium salt, sodium salt, silver salt, copper salt or potassium salt.

3. The amorphous solid solution type solid electrolyte according to claim 1, characterized in that: The C a A b C in the + 、Na + 、Ag + , Cu + or K + ; A is a simple anion, a polyanion or a mixture of the two; the simple anion is a halogen, OH - NH2 - 、O2 2- , O 2- , S 2- or N 3- One or more of; the polyanion is XO m n- or X m O 3m+1 n- , X is one or more of B, S, C, P, Si, As, Mo, W or C; MB y Wherein M is one or more of Zr, Hf, Ta, Nb, Al, Fe, Ga, In, Mo, W, Y, Ti, Si, B and Sb, and B is one or more of halogen, S or O.

4. The amorphous solid solution type solid electrolyte according to claim 3, characterized in that: When A is a polyanion, the B element in the van der Waals crystal is replaced by XO m n- or X m O 3m+1 n- The O element in is substituted.

5. The amorphous solid solution type solid electrolyte according to claim 1, characterized in that: The C e MB f and CB are nanocrystals, and the content of nanocrystals in the amorphous solid solution type solid electrolyte is less than 30wt.%; Frame structure (C a A b ) x -MB y Granular, C e MB f or CB on the surface of the particles.

6. The amorphous solid solution type solid electrolyte according to claim 1, characterized in that: The range of x is 0.2 to 2, and the range of y is 3 to 6.

7. The method for preparing the amorphous solid solution type solid electrolyte according to claim 1, characterized in that: The following steps are involved: In an inert atmosphere without water or oxygen, mix C a A b Powder and MB y The powders were mixed and solid-phase reacted by mechanical ball milling to obtain the target product (C a A b ) c -MB y .

8. The preparation method according to claim 7, characterized in that: The ball milling time is 1 h to 30 h, and the ball milling speed is 400 rpm to 800 rpm.

9. The preparation method according to claim 7, characterized in that: After ball milling, the powder is annealed; the annealing temperature is 200-500° C., and the annealing environment is an inert atmosphere or a vacuum environment.

10. A solid-state battery, characterized in that: The invention is an all-solid-state lithium battery, comprising a positive electrode sheet, a negative electrode sheet, and a solid electrolyte sheet between the positive electrode sheet and the negative electrode sheet, wherein the material of the solid electrolyte sheet is the amorphous solid solution solid electrolyte according to any one of claims 1 to 6.

Citation Information

Cited By

  • Polyanion solid electrolyte, preparation method thereof and solid-state battery

    CN119560625A

  • Solid electrolyte material with composite structure and battery manufactured by using material

    CN120221770A

  • Solid electrolyte and preparation method therefor, and battery

    WO2026026595A1