In-situ double-layer structure polymer solid electrolyte and preparation method and application thereof
By using in-situ double-layer structure polymer solid electrolyte in lithium batteries, the problems of complex process and poor interface in the existing technology are solved, the electrochemical window is broadened, the ionic conductivity and interface compatibility are improved, and it is suitable for high performance Solid-state lithium battery.
Patent Information
- Application Number
- CN202411212478.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the preparation process of polymer solid electrolytes of solid state lithium batteries is complicated and has poor contact with positive and negative electrode materials, which limits its application in high-voltage lithium batteries, especially the single component in situ polymer ether electrolytes at voltage. It is prone to oxidation when it exceeds 3.9V, resulting in limited energy density and safety.
The polymer solid electrolyte with in-situ double-layer structure is used to form a polymer solid electrolyte with a double-layer structure by polymerizing acrylate monomer and ether monomer on the positive electrode side and the negative electrode side, combining a photoinitiator and lithium salt. Wide the electrochemical window and improve room temperature ionic conductivity, simplify the preparation process and improve interface compatibility with the electrodes.
The electrochemical stability window of polymer solid electrolyte is expanded to 4.92V, which improves room temperature ion conductivity, simplifies the preparation process, reduces production costs, and improves the interface contact with the positive electrode. It is suitable for high-performance solid lithium batteries. .
Smart Images

Figure CN118919840A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium battery materials, and in particular to an in-situ double-layer structure polymer solid electrolyte and a preparation method and application thereof. Background Art
[0002] With the rapid development of electric vehicles and portable electronic devices, people have put forward higher requirements for the energy density and safety of lithium-ion batteries. The energy density of traditional lithium-ion batteries using liquid electrolytes has reached its limit and there are safety issues such as flammability and explosion. Solid electrolytes are non-flammable and can also match high-voltage positive electrodes and metal lithium negative electrodes to improve the energy density of lithium-ion batteries.
[0003] Solid electrolytes can be divided into inorganic solid electrolytes and polymer solid electrolytes. Inorganic solid electrolytes have high room temperature ionic conductivity, but their difficult processing and large interface resistance limit their application. Polymer solid electrolytes have the advantages of good flexibility, easy processing and designable structure, and are widely used in solid-state lithium-ion batteries.
[0004] The traditional polymer solid electrolyte preparation method is cumbersome and the problem of poor contact with positive and negative electrode materials restricts its application in solid-state lithium metal batteries. Therefore, the selection of polymer solid electrolytes with simple structure, easy preparation and good interface contact with positive and negative electrodes is an important strategy for the development of solid-state lithium metal batteries. In-situ polymerized ether electrolytes have the advantages of simple manufacturing process, relatively high lithium ion conductivity, good anode stability, strong film-forming ability and good interface contact. However, single-component in-situ polymerized ether electrolytes will slowly oxidize when the voltage exceeds 3.9V, which limits their application in high-voltage batteries, and further limits their energy density and safety. The construction of in-situ double-layer polymer solid electrolytes is expected to solve the above problems.
[0005] Chinese patents CN 117038842 A, CN 117855579 A, and CN 112864458 B disclose methods for constructing a double-layer solid electrolyte by preparing a layer of solid electrolyte on the high-voltage positive electrode side and the lithium metal negative electrode side. However, the interface impedance between the double-layer solid electrolyte prepared by the above technology and the electrode is still relatively large, and the preparation process is complicated, which is incompatible with the existing lithium battery manufacturing process and cannot meet the needs of commercial applications of high-performance solid-state lithium batteries. Therefore, it is urgent to study a solid electrolyte with a simple preparation process and the ability to improve the interface compatibility between the solid electrolyte and the electrode. Summary of the invention
[0006] The purpose of the present invention is to provide an in-situ double-layer structure polymer solid electrolyte and its preparation method and application in order to overcome the defects of the above-mentioned prior art. By polymerizing acrylate monomers and ether monomers on the positive electrode side and the negative electrode side respectively to form a polymer solid electrolyte with a double-layer structure, the electrochemical window of the ether polymer solid electrolyte is broadened and the room temperature ionic conductivity of the polymer solid electrolyte is improved.
[0007] The purpose of the present invention can be achieved by the following technical solutions:
[0008] The invention provides an in-situ double-layer structure polymer solid electrolyte, which comprises a double-layer structure composed of acrylic ester monomers and ether monomers, an initiator and a lithium salt.
[0009] Furthermore, the molar ratio of the acrylic acid ester monomer, the ether monomer, the initiator and the lithium salt is (0.80-1.2):(1-2):(0.10-0.30):(1-2).
[0010] Furthermore, the acrylic ester monomer includes one or more of cyanoacrylate, pentafluoropropyl acrylate, hexafluorobutyl acrylate, and tetrafluoropropyl methacrylate.
[0011] Furthermore, the ether monomer includes one or more of 1,3-dioxolane, 1,3-dioxane, tetrahydrofuran or ethylene glycol diglycidyl ether.
[0012] Furthermore, the lithium salt includes one or more of lithium perchlorate, lithium hexafluorophosphate, lithium difluorooxalatoborate or lithium bis(trifluoromethanesulfonyl)imide.
[0013] Further, the initiator is a photoinitiator or a cationic initiator;
[0014] The photoinitiator includes one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexyl phenyl ketone, 2,4,6-trimethylbenzoyl diphenyl phosphine oxide, and isopropylthiocyanate;
[0015] The cationic initiator includes one or more of aluminum trifluoromethanesulfonate, aluminum chlorate, titanate chlorate, and lithium tetrafluoroborate.
[0016] The present invention also provides a method for preparing an in-situ double-layer structure polymer solid electrolyte, comprising the following steps:
[0017] S1: mixing an acrylic acid ester monomer, an initiator and a lithium salt, and stirring them evenly to obtain a first transparent mixed liquid;
[0018] S2: mixing the ether monomer, the initiator and the lithium salt, and stirring them evenly to obtain a second transparent mixed liquid;
[0019] S3: subjecting the first transparent mixed liquid in S1 to free radical polymerization under ultraviolet light to obtain a polymer solid electrolyte;
[0020] S4: The second transparent mixed liquid in S2 is uniformly coated on the surface of the polymer solid electrolyte obtained in S3 and allowed to stand to perform cationic polymerization to obtain an in-situ double-layer structured polymer solid electrolyte.
[0021] Furthermore, the stirring time of S1 and S2 is 6 to 8 h;
[0022] In S3, the UV light exposure time is 1h to 2h;
[0023] In S4, the standing time is 2 to 4 hours.
[0024] Furthermore, S1-S4 are all carried out in an inert atmosphere, and the inert atmosphere is argon.
[0025] The present invention also provides an application of an in-situ double-layer structure polymer solid electrolyte, wherein the solid electrolyte is used to prepare a solid-state lithium metal battery;
[0026] The solid-state lithium metal battery comprises a positive electrode, the prepared polymer solid electrolyte and a negative electrode which are stacked in sequence.
[0027] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0028] 1. The present invention polymerizes acrylate monomers and ether monomers on the positive electrode side and the negative electrode side respectively to form a polymer solid electrolyte with a double-layer structure, which broadens the electrochemical window of the ether polymer solid electrolyte and improves the room temperature ionic conductivity of the polymer solid electrolyte. The in-situ double-layer structure polymer solid electrolyte of the present invention has an ionic conductivity of up to 2.2×10 -4 S cm -1 The electrochemical stability window can reach 4.92V, which is a significant improvement compared to the 3.9V electrochemical stability window of traditional ether polymer solid electrolytes.
[0029] 2. The present invention applies the first transparent mixed liquid to the NCM811 positive electrode and directly performs ultraviolet polymerization on the positive electrode plate. The obtained solid electrolyte has good interface contact with the positive electrode plate.
[0030] 3. The present invention prepares solid electrolytes by in-situ polymerization of acrylate monomers and ether monomers by ultraviolet radiation free radical initiation and cation initiation. Compared with the traditional solution casting method and thermal initiation polymerization, the process of the present invention is simple and controllable, energy-saving and environmentally friendly, improves production efficiency and reduces production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 Schematic diagram of impedance test results of the solid electrolytes prepared in Examples 1-4 and Comparative Examples 1-2;
[0032] Figure 2 Schematic diagram of electrochemical stability test results of the solid electrolytes prepared in Examples 1-4 and Comparative Examples 1-2;
[0033] Figure 3 This is a cross-sectional electron microscope image of the first transparent mixed liquid after in-situ polymerization on the NCM811 positive electrode in Example 1;
[0034] Figure 4 This is a graph showing the electrochemical stability test results of a full battery assembled with a double-layer solid electrolyte prepared in Example 1;
[0035] Figure 5 This is a test result diagram of the electrochemical stability test of the full battery assembled based on the acrylic ester single-layer electrolyte in Comparative Example 1;
[0036] Figure 6 This is a graph showing the electrochemical stability test results of the full battery assembled based on the ether monolayer electrolyte in Comparative Example 2. DETAILED DESCRIPTION
[0037] The specific implementation methods of the present invention are described in detail below through examples. These examples are implemented on the premise of the scheme described in the present invention, and provide detailed implementation methods and specific operating processes, but the protection scope of the present invention is not limited to the following examples.
[0038] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments. Any features such as component models, material names, connection structures, preparation methods, materials, structures or composition ratios not clearly described in this technical solution are deemed to be common technical features disclosed in the prior art.
[0039] Example 1
[0040] This embodiment provides a method for preparing an in-situ double-layer structure polymer solid electrolyte, comprising the following steps:
[0041] S1: In an argon glove box, pentafluoropropyl acrylate, 2-hydroxy-2-methyl-1-phenyl-1-propanone and lithium bis(trifluoromethanesulfonyl)imide were added into a glass bottle according to mass of 1.2 g, 0.01 g and 0.30 g, respectively, and stirred for 6 hours to obtain a first transparent mixed liquid;
[0042] S2: In an argon glove box, 1,3-dioxolane, aluminum trifluoromethanesulfonate and lithium bis(trifluoromethanesulfonyl imide) were added into a glass bottle according to mass of 1 g, 0.015 g and 0.30 g, respectively, and stirred for 6 hours to obtain a second transparent mixed liquid;
[0043] S3: In an argon glove box, subjecting the transparent mixed liquid in S1 to free radical polymerization under the illumination of an ultraviolet lamp to obtain the polypentafluoropropyl acrylate polymer solid electrolyte;
[0044] S4: In an argon glove box, the liquid in S2 is coated on the polypentafluoropropyl acrylate polymer solid electrolyte obtained in S3, and ring-opening polymerization is carried out under cation initiation to obtain a double-layer structure polymer solid electrolyte.
[0045] Figure 3 This is a cross-sectional view of the first transparent mixed liquid in S1 after in-situ polymerization on the NCM811 positive electrode. It can be seen that the contact between the NCM811 positive electrode and the electrolyte is very close.
[0046] This embodiment also provides an application of an in-situ double-layer structure polymer solid electrolyte. In an argon glove box, the first transparent mixed liquid in S1 is evenly coated on the NCM811 positive electrode and subjected to ultraviolet polymerization. After the polymerization reaction is completed, the second transparent mixed liquid in S2 is coated thereon for cationic polymerization, and then stacked with the lithium metal negative electrode in sequence to assemble into a solid lithium metal battery. Figure 4 As shown, Figure 4 Figure 2 shows the cycling performance of the assembled battery at room temperature. The assembled battery exhibited a cycling performance of 175.2 mAh g after activation at a current density of 0.1 C. -1 The specific capacity is still 166.8 mAh g after 100 cycles. -1 The capacity retention rate is 95.2%, which shows that the solid electrolyte prepared in this embodiment has good cycle stability.
[0047] Example 2
[0048] This embodiment provides a method for preparing an in-situ double-layer structure polymer solid electrolyte, comprising the following steps:
[0049] S1: In an argon glove box, hexafluorobutyl acrylate, 2-hydroxy-2-methyl-1-phenyl-1-propanone and lithium difluorooxalatoborate were added into a glass bottle according to the mass of 1.34 g, 0.01 g and 0.12 g, respectively, and stirred for 6 hours to obtain a transparent mixed liquid;
[0050] S2: In an argon glove box, 1,3-dioxane, aluminum trifluoromethanesulfonate and lithium difluorooxalatoborate were added into a glass bottle according to mass of 1 g, 0.015 g and 0.12 g, respectively, and stirred for 6 hours to obtain a transparent mixed liquid;
[0051] S3: In an argon glove box, the liquid in S1 is subjected to free radical polymerization under the illumination of an ultraviolet lamp to obtain a poly(hexafluorobutyl acrylate) polymer solid electrolyte;
[0052] S4: In an argon glove box, the liquid in S2 is applied to the poly(hexafluorobutyl acrylate) polymer solid electrolyte obtained in S3, and ring-opening polymerization is carried out under cation initiation to obtain the double-layer structure polymer solid electrolyte.
[0053] Example 3
[0054] This embodiment provides a method for preparing an in-situ double-layer structure polymer solid electrolyte, comprising the following steps:
[0055] S1: In an argon glove box, hexafluorobutyl acrylate, 2,2-dimethoxy-2-acetophenone and lithium bis(trifluoromethanesulfonyl)imide were added into a glass bottle according to the mass of 1.34 g, 0.015 g and 0.3 g, respectively, and stirred for 6 hours to obtain a transparent mixed liquid;
[0056] S2: In an argon glove box, 1,3-dioxane, boron trifluoride and lithium bis(trifluoromethanesulfonyl)imide were added into a glass bottle according to mass of 1 g, 0.01 g and 0.3 g, respectively, and stirred for 6 hours to obtain a transparent mixed liquid;
[0057] S3: In an argon glove box, the liquid in S1 is subjected to free radical polymerization under the illumination of an ultraviolet lamp to obtain a poly(hexafluoropropyl)acrylate) polymer solid electrolyte;
[0058] S4: In an argon glove box, the liquid in S2 is applied to the poly(hexafluorobutyl acrylate) polymer solid electrolyte obtained in S3, and ring-opening polymerization is carried out under cation initiation to obtain a double-layer structured polymer solid electrolyte.
[0059] Example 4
[0060] This embodiment provides a method for preparing an in-situ double-layer structure polymer solid electrolyte, comprising the following steps:
[0061] S1: In an argon glove box, tetrafluoropropyl methacrylate, 2,2-dimethoxy-2-acetophenone and lithium hexafluorophosphate were added into a glass bottle according to the mass of 1.25 g, 0.015 g and 0.25 g, respectively, and stirred for 6 hours to obtain a transparent mixed liquid;
[0062] S2: In an argon glove box, 1,3-dioxolane, lithium tetrafluoroborate and lithium hexafluorophosphate were added into a glass bottle according to mass of 1 g, 0.01 g and 0.25 g, respectively, and stirred for 6 hours to obtain a transparent mixed liquid;
[0063] S3: In an argon glove box, subjecting the liquid in S1 to free radical polymerization under the illumination of an ultraviolet lamp to obtain the polytetrafluoropropyl methacrylate polymer solid electrolyte;
[0064] S4: In an argon glove box, the liquid in S2 is applied to the polytetrafluoropropyl methacrylate polymer solid electrolyte obtained in S3, and ring-opening polymerization is carried out under cation initiation to obtain a double-layer structure polymer solid electrolyte.
[0065] Comparative Example 1
[0066] This comparative example provides a method for preparing an acrylate single-layer electrolyte, comprising the following steps:
[0067] S1: In an argon glove box, tetrafluoropropyl methacrylate, 2,2-dimethoxy-2-acetophenone and lithium hexafluorophosphate were added into a glass bottle according to the mass of 1.25 g, 0.015 g and 0.25 g, respectively, and stirred for 6 hours to obtain a transparent mixed liquid;
[0068] S2: In an argon glove box, the liquid in S1 is subjected to free radical polymerization under the illumination of an ultraviolet lamp to obtain the polytetrafluoropropyl methacrylate polymer solid electrolyte.
[0069] Figure 5 The cycling performance diagram of the solid-state lithium metal button battery assembled with the acrylic ester single-layer electrolyte prepared in this comparative example, with NCM811 as the positive electrode and a lithium metal sheet as the negative electrode at room temperature.
[0070] like Figure 5 As shown in Figure 2, the solid-state lithium metal battery assembled with acrylic monolayer electrolyte exhibited a charge and discharge rate of 158.8 mAh g at a current density of 0.1 C after activation. -1 The discharge specific capacity decays rapidly during the cycle. This is because the ionic conductivity of the acrylate monolayer electrolyte is low, which leads to excessive internal resistance of the battery, thus causing the specific capacity to decay rapidly.
[0071] Comparative Example 2
[0072] This comparative example provides a method for preparing an ether monolayer electrolyte, comprising the following steps:
[0073] S1: In an argon glove box, 1,3-dioxolane, lithium tetrafluoroborate and lithium hexafluorophosphate were added into a glass bottle according to mass of 1 g, 0.01 g and 0.25 g, respectively, and stirred for 6 hours to obtain a transparent mixed liquid;
[0074] S2: In an argon glove box, the liquid in S1 is subjected to ring-opening polymerization under cation initiation to obtain a polymer solid electrolyte.
[0075] Figure 6The cycling performance diagram of the solid-state lithium metal button battery assembled with the ether single-layer electrolyte prepared in this comparative example, with NCM811 as the positive electrode and a lithium metal sheet as the negative electrode at room temperature.
[0076] like Figure 6 As shown in Figure 2, the lithium metal battery assembled with ether monolayer electrolyte exhibited a high efficiency of 179.7 mAh g at a current density of 0.1 C after activation. -1 The specific capacity is 67.1 mAh g after 100 cycles. -1 The capacity retention rate is 37.2%. It can be seen that the oxidation resistance of the ether monolayer electrolyte is relatively poor, which causes the ether electrolyte to continuously react with the NCM811 positive electrode, resulting in a rapid decrease in specific capacity.
[0077] Test Example 1
[0078] In an argon glove box, the polymer solid electrolytes prepared in Examples 1 to 4 and Comparative Examples 1 and 2 were assembled into button batteries with NCM811 as the positive electrode and lithium metal as the negative electrode, and AC impedance tests were performed at 25° C. The test conditions were a frequency range of 1 MHz to 0.1 Hz, an AC amplitude of 10 mV, and ionic conductivity was measured. The results are shown in Tables 1 and Figure 1 As shown in Table 1 and Figure 1 It can be seen that the ionic conductivity of acrylate polymer solid electrolyte is lower than that of ether polymer solid electrolyte. Therefore, acrylate electrolyte alone is difficult to be applied to lithium batteries. The polymer solid electrolyte that combines it with ether polymer solid electrolyte has higher ionic conductivity and can be used in lithium batteries.
[0079] Table 1 Ionic conductivity of polymer solid electrolytes prepared in various embodiments and comparative examples
[0080]
[0081] Test Example 2
[0082] The polymer solid electrolytes prepared in Examples 1 to 4 and Comparative Examples 1 and 2 were subjected to linear sweep voltammetry tests. The test conditions were: in the voltage range of 0-6 V, 1 mV s -1 The response current changes of different polymer solid electrolytes at a scan rate of Figure 2 As shown in Table 2, Figure 2 It can be seen that the oxidation resistance of acrylate polymer solid electrolyte is better than that of ether polymer solid electrolyte, and it can stabilize the high-voltage positive electrode. Therefore, combining acrylate polymer solid electrolyte with ether polymer solid electrolyte can promote the application of ether electrolyte in high-voltage positive electrode battery systems.
[0083] Table 2 Electrochemical stability window of polymer solid electrolytes prepared in various embodiments and comparative examples
[0084]
[0085] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. An in-situ double-layer polymer solid electrolyte, characterized in that: The solid electrolyte comprises a double-layer structure formed by an acrylate monomer and an ether monomer, an initiator and a lithium salt, wherein the initiator is used for initiating polymerization of the acrylate monomer and the ether monomer.
2. The in-situ double-layer polymer solid electrolyte according to claim 1, characterized in that: The molar ratio of the acrylic acid ester monomer, the ether monomer, the initiator and the lithium salt is (0.80-1.2):(1-2):(0.10-0.30):(1-2).
3. The in-situ double-layer polymer solid electrolyte according to claim 1, characterized in that: The acrylic ester monomers include one or more of cyanoacrylate, pentafluoropropyl acrylate, hexafluorobutyl acrylate, and tetrafluoropropyl methacrylate.
4. The in-situ double-layer polymer solid electrolyte according to claim 1, characterized in that: The ether monomer includes one or more of 1,3-dioxolane, 1,3-dioxane, tetrahydrofuran or ethylene glycol diglycidyl ether.
5. The in-situ double-layer polymer solid electrolyte according to claim 1, characterized in that: The lithium salt includes one or more of lithium perchlorate, lithium hexafluorophosphate, lithium difluorooxalatoborate or lithium bis(trifluoromethanesulfonyl)imide.
6. The in-situ double-layer polymer solid electrolyte according to claim 1, characterized in that: The initiator is a photoinitiator or a cationic initiator; The photoinitiator includes one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexyl phenyl ketone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, isopropylthiocyanate, and 2,2-dimethoxy-2-acetophenone; The cationic initiator includes one or more of aluminum trifluoromethanesulfonate, aluminum chlorate, titanate chlorate, and lithium tetrafluoroborate.
7. A method for preparing an in-situ double-layer polymer solid electrolyte according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1: mixing an acrylic acid ester monomer, an initiator and a lithium salt, and stirring them evenly to obtain a first transparent mixed liquid; S2: mixing the ether monomer, the initiator and the lithium salt, and stirring them evenly to obtain a second transparent mixed liquid; S3: subjecting the first transparent mixed liquid in S1 to free radical polymerization under ultraviolet light to obtain a polymer solid electrolyte; S4: The second transparent mixed liquid in S2 is uniformly coated on the surface of the polymer solid electrolyte obtained in S3 and allowed to stand to perform cationic polymerization to obtain an in-situ double-layer structured polymer solid electrolyte.
8. The method for preparing an in-situ double-layer polymer solid electrolyte according to claim 1, characterized in that: The stirring time of S1 and S2 is 6 to 8 h; In S3, the UV light exposure time is 1h to 2h; In S4, the standing time is 2 to 4 hours.
9. The method for preparing an in-situ double-layer polymer solid electrolyte according to claim 1, characterized in that: S1-S4 are all carried out in an inert atmosphere, which is argon.
10. An application of an in-situ double-layer structure polymer solid electrolyte, characterized in that: The solid electrolyte is used to prepare a solid-state lithium metal battery; The solid-state lithium metal battery comprises a positive electrode, a polymer solid electrolyte according to any one of claims 1 to 6, and a negative electrode stacked in sequence.
Citation Information
Patent Citations
A bilayer composite solid electrolyte material, its preparation method, and its application
CN112864458B
Pole piece with multiple layers of solid electrolyte, preparation method of pole piece, solid-state battery and preparation method of solid-state battery
CN117038842A
Janus composite solid electrolyte and preparation method and application thereof
CN117855579A
Cited By
Preparation method of polysulfone-polyether double-layer solid electrolyte
CN120809946A
A solid-state lithium battery using an in-situ cured polymer solid electrolyte and a method of manufacturing the same
CN122868667A