Composite electrolyte diaphragm and lithium ion battery
By using composite electrolyte separators with high entropy polymer and high entropy lithium salt systems in lithium-ion batteries, the problem of low cycle life of lithium-ion batteries is solved, and higher battery performance and stability are achieved.
Patent Information
- Application Number
- CN202411036057.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-29
AI Technical Summary
The cycle life of lithium-ion batteries is low, mainly due to the instability of the interface between the organic-inorganic composite electrolyte and the electrode.
The composite electrolyte separator is adopted, and its raw material components include three or more polymers, lithium salts and oxide ceramic electrolytes to form a high-entropy polymer and high-entropy lithium salt system, which jointly participates in the formation of SEI films and improves the uniform transmission of lithium ions. and deposition, reduce interface impedance and enhance the cycling performance of the battery.
Through the synergy between high-entropy polymer and high-entropy lithium salt system, the cycle life and capacity retention rate of lithium-ion batteries are improved, the interface impedance and thermal shrinkage rate are reduced, and the mechanical strength and thermal stability of the battery are improved.
Smart Images

Figure CN119050461A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a composite electrolyte membrane and a lithium-ion battery. Background Art
[0002] Organic-inorganic composite electrolyte membranes have excellent electrochemical and mechanical properties and are very compatible with the current lithium-ion battery production process, and have extremely high commercial potential. Organic-inorganic composite electrolyte membranes combine electrolytes and membranes into one, achieving multiple functions of one material, simplifying battery structure, improving battery safety, further promoting the energy density of lithium-ion batteries, meeting the development of high-performance batteries, and accelerating the commercialization of solid-state batteries.
[0003] However, the interface between organic-inorganic composite electrolyte and electrode is unstable, which will reduce the cycle life of lithium-ion batteries to a certain extent. Summary of the invention
[0004] The present application provides a composite electrolyte membrane and a lithium-ion battery to solve the following technical problem: how to improve the cycle life of a lithium-ion battery.
[0005] In a first aspect, the present application provides a composite electrolyte membrane, wherein the raw material components of the composite electrolyte membrane include:
[0006] Three or more polymers, three or more lithium salts and oxide ceramic electrolytes; wherein:
[0007] The lithium salt comprises at least one inorganic lithium salt and at least two organic lithium salts;
[0008] The weight ratio of the polymer to the lithium salt is (3-12):1.
[0009] Optionally, the weight ratio of the polymer to the lithium salt is (4-10):1.
[0010] Optionally, the inorganic lithium salt includes at least one of the following: lithium perchlorate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium nitrate, and lithium difluorophosphate.
[0011] Optionally, the organic lithium salt includes at least two of the following: lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium difluorooxalatoborate, and lithium bis(oxalateborate).
[0012] Optionally, the weight ratio of the inorganic lithium salt to the organic lithium salt is 1:(1-3).
[0013] Optionally, the polymer includes at least three of the following: polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polycaprolactone, polypropylene polycarbonate, polyimide, polymethyl methacrylate, poly-1,2-dioxolane, polyvinylidene fluoride-hexafluoropropylene, and polyethylene glycol.
[0014] Optionally, the oxide ceramic electrolyte includes at least one of the following: lithium aluminum titanium phosphate, lithium lanthanum zirconate, tantalum-doped lithium lanthanum zirconate, lithium phosphosulfuric acid, and lithium germanium phosphosulfuric acid.
[0015] Optionally, the oxide ceramic electrolyte is 0.1 to 0.4 parts by weight relative to 1 part by weight of the raw material components of the composite electrolyte membrane.
[0016] Optionally, the composite electrolyte membrane is obtained by one of the following methods: melt hot pressing, electrostatic spinning, and hot solvent casting.
[0017] In a second aspect, the present application provides a lithium-ion battery, wherein the lithium-ion battery comprises the composite electrolyte membrane described in any one of the embodiments of the first aspect.
[0018] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0019] The composite electrolyte membrane provided in the embodiment of the present application comprises raw materials including: three or more polymers, three or more lithium salts and oxide ceramic electrolyte; wherein the lithium salt comprises at least one inorganic lithium salt and at least two organic lithium salts; the weight ratio of the polymer to the lithium salt is (3-12):1. The three or more polymers can form a high entropy polymer system, which can reduce the crystallinity of the overall polymer, facilitate the migration of lithium ions in the amorphous region, thereby improving the ionic conductivity of the composite electrolyte membrane; the three or more polymers can form a lithium salt high entropy lithium salt system, which can participate in the formation of the negative electrode SEI film and reduce the consumption of active lithium in the positive electrode, thereby improving the reversible capacity of the battery cycle; wherein the inorganic lithium salt can form a lithium ion inorganic transmission interface, thereby ensuring the uniform deposition of lithium ions; the organic lithium salt can form a lithium ion organic transmission interface, thereby ensuring the stable efficiency of charge and discharge; the inorganic lithium salt and the organic lithium salt synergistically participate in the formation of the SEI film, thereby ensuring the uniform transfer of lithium ions. and deposition, and maintain stable efficiency during battery charging and discharging, produce mutual synergy and inhibit anion movement, and improve battery performance; the high entropy polymer system and the high entropy lithium salt system can form an organic solid electrolyte, participate in battery charging and discharging, and the organic solid electrolyte contains a high entropy polymer system and has good interface contact, thereby reducing interface impedance; the oxide ceramic electrolyte has good mechanical strength and thermal stability, thereby improving the mechanical strength and heat shrinkage resistance of the composite electrolyte membrane; the high entropy polymer system, the high entropy lithium salt system and the oxide ceramic electrolyte synergistically promote the composite electrolyte membrane to have higher ionic conductivity, good cycle performance and capacity retention rate, which is ultimately reflected in the improvement of the cycle life of the lithium-ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0021] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0022] Figure 1 A battery cycle test diagram provided in Example 1 of the present application;
[0023] Figure 2 A battery cycle test diagram provided in Example 2 of the present application;
[0024] Figure 3A battery cycle test diagram provided in Example 3 of the present application;
[0025] Figure 4 A battery cycle test diagram provided for comparative example 1 of the present application;
[0026] Figure 5 This is an interfacial impedance test diagram of a composite electrolyte membrane provided in Example 1 of the present application;
[0027] Figure 6 This is an interface impedance test diagram of a composite electrolyte membrane provided in Comparative Example 1 of the present application;
[0028] Figure 7 This is an appearance diagram of a composite electrolyte membrane provided in an embodiment of the present application;
[0029] Figure 8 This is an appearance diagram of a composite electrolyte membrane provided in an embodiment of the present application when heated to 200°C. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0031] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0032] In the present application, the terms "include", "comprising", etc. mean "including but not limited to". "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.
[0033] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0034] In a first aspect, the present application provides a composite electrolyte membrane, wherein the raw material components of the composite electrolyte membrane include:
[0035] Three or more polymers, three or more lithium salts and oxide ceramic electrolytes; wherein:
[0036] The lithium salt comprises at least one inorganic lithium salt and at least two organic lithium salts;
[0037] The weight ratio of the polymer to the lithium salt is (3-12):1.
[0038] In some embodiments, the weight ratio of the polymer to the lithium salt is (4-10):1.
[0039] In the embodiments of the present application, three or more polymers can form a high entropy polymer system, which can reduce the crystallinity of the overall polymer, which is beneficial to the migration of lithium ions in the amorphous region, thereby improving the ionic conductivity of the composite electrolyte membrane; three or more polymers can form a lithium salt high entropy lithium salt system, which can participate in the formation of the negative electrode SEI film and reduce the consumption of active lithium at the positive electrode, thereby improving the battery cycle reversible capacity; among them, the inorganic lithium salt can form a lithium ion inorganic transmission interface, thereby ensuring the uniform deposition of lithium ions; the organic lithium salt can form a lithium ion organic transmission interface, thereby ensuring the stable efficiency of charging and discharging; the inorganic lithium salt and the organic lithium salt synergistically participate in the formation of the SEI film, thereby ensuring the reversible capacity of the lithium ions. Uniform transfer and deposition, and maintaining stable efficiency during battery charging and discharging, produce mutual synergy and inhibit anion movement, and improve battery performance; the high entropy polymer system and the high entropy lithium salt system can form an organic solid electrolyte, participate in battery charging and discharging, and the organic solid electrolyte contains a high entropy polymer system and has good interface contact, thereby reducing interface impedance; the oxide ceramic electrolyte has good mechanical strength and thermal stability, thereby improving the mechanical strength and heat shrinkage resistance of the composite electrolyte membrane; the high entropy polymer system, the high entropy lithium salt system and the oxide ceramic electrolyte synergistically promote the composite electrolyte membrane to have higher ionic conductivity, good cycle performance and capacity retention rate, which is ultimately reflected in the improvement of the cycle life of the lithium-ion battery.
[0040] The weight ratio of polymer to lithium salt can be (3-12):1, because: it can ensure that the lithium salt can be fully dissociated, increase the concentration of mobile lithium salt, help to increase the electrochemical reaction rate, and reduce polarization. If the weight ratio is too large, the polymer is excessive, the lithium ion concentration is too low, and the mobile ion concentration is low, which affects the battery performance; if the weight ratio is too small, the lithium salt is excessive, part of the lithium salt is not dissociated, and cannot participate in the electrochemical reaction, which affects the battery performance. Exemplarily, the weight ratio of the above polymer to lithium salt can be 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, etc.; further, the weight ratio of the polymer to lithium salt can be (4-10):1.
[0041] In some embodiments, the inorganic lithium salt includes at least one of the following: lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium nitrate (LiNO3), and lithium difluorophosphate (LiPO2F2).
[0042] In some embodiments, the organic lithium salt includes at least two of the following: lithium bis(trifluoromethanesulfonimide) (LiTFSI), lithium bis(fluorosulfonimide) (LiFSI), lithium difluorooxalatoborate (LiDFOB), and lithium bis(oxalateborate) (LiBOB).
[0043] In the embodiment of the present application, the combination of organic lithium salt and inorganic lithium salt can participate in the formation of SEI film. The organic lithium salt ensures the stability of charge and discharge efficiency in the SEI film, and the inorganic lithium salt component ensures the uniform deposition of lithium ions. The inorganic lithium salt can be at least one of the following: lithium perchlorate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium nitrate, lithium difluorophosphate; the organic lithium salt can be at least two of the following: lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium difluorooxalatoborate, lithium bis(oxalate borate); further, the combination of the lithium salt can be selected from LiClO4 / LiTFSI / LiBOB; LiFSI / LiDFOB / LiBF4;
[0044] Lithium salt combinations such as LiPF6 / LiBOB / LiTFSI; LiNO3 / LiFSI / LiDFOB.
[0045] In some embodiments, the weight ratio of the inorganic lithium salt to the organic lithium salt is 1:(1-3).
[0046] In the embodiments of the present application, inorganic lithium salts can form an inorganic lithium ion transmission interface, thereby ensuring uniform deposition of lithium ions; organic lithium salts can form an organic lithium ion transmission interface, thereby ensuring stable efficiency of charge and discharge; inorganic lithium salts and organic lithium salts synergistically participate in the formation of SEI film, thereby ensuring uniform transfer and deposition of lithium ions, and maintaining stable efficiency during battery charge and discharge, generating mutual synergy and inhibiting anion movement, and improving battery performance. Exemplarily, the weight ratio of the above-mentioned inorganic lithium salt to organic lithium salt is 1:1, 1:2, 1:3, etc. The lithium salt comprises an inorganic lithium salt and two organic lithium salts; the weight ratio (inorganic lithium salt: organic lithium salt: organic lithium salt) can be as low as 1:1:1, 2:1:1, 2:0.5:1.5, etc.
[0047] In some embodiments, the polymer includes at least three of the following: polyethylene oxide (PEO), polyacrylonitrile (PAN), polyvinylidene fluoride (PVDF), polycaprolactone (PCL), polypropylene polycarbonate (PPC), polyimide (PI), polymethyl methacrylate (PMMA), poly 1,2-dioxolane (PDOL), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), and polyethylene glycol (PEG).
[0048] In the embodiment of the present application, the polymer may include at least three of the following: polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polycaprolactone, polypropylene polycarbonate, polyimide, polymethyl methacrylate, poly 1,2-dioxolane, polyvinylidene fluoride-hexafluoropropylene, polyethylene glycol; the above polymers are widely available, low-priced, mechanically flexible, and have good contact and wetting functions. At the same time, the polymer chain segments contain highly electronegative elements (N, O, S, F), which are conducive to the dissociation of lithium salts and promote lithium ion migration. Further, the combination of the polymer can be PEO-PAN-PPC; PCL-PMMA-PVDF; PEG-PI-PDOL; PEO-PCL-PVDF, etc.
[0049] In some embodiments, the oxide ceramic electrolyte includes at least one of lithium aluminum titanium phosphate (LATP), lithium lanthanum zirconate (LLZO), tantalum-doped lithium lanthanum zirconate (LLZTO), lithium phosphosulfuryl chloride (LPSCl), and lithium germanium phosphosulfur (LGPS).
[0050] In an embodiment of the present application, the oxide ceramic electrolyte may include at least one of the following: lithium aluminum titanium phosphate, lithium lanthanum zirconate, tantalum-doped lithium lanthanum zirconate, lithium phosphorus sulfur chlorine, and lithium germanium phosphorus sulfur. The above oxide ceramic electrolyte has high mechanical strength and excellent heat shrinkage resistance, and the oxide ceramic electrolyte has a lithium ion transmission channel, which can further improve the lithium ion transmission efficiency and alleviate the polarization effect caused by the slow ion migration rate.
[0051] In some embodiments, the oxide ceramic electrolyte is present in an amount of 0.1 to 0.4 parts by weight relative to 1 part by weight of the raw material components of the composite electrolyte separator.
[0052] In the embodiment of the present application, relative to 1 part by weight of the raw material components of the composite electrolyte diaphragm, the oxide ceramic electrolyte can be 0.1 to 0.4 parts by weight, which can make the composite electrolyte diaphragm have the characteristics of both rigidity and flexibility, and have good heat shrinkage resistance. Exemplarily, relative to 1 part by weight of the raw material components of the composite electrolyte diaphragm, the oxide ceramic electrolyte can be 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, etc.
[0053] In some embodiments, the composite electrolyte membrane is obtained by one of the following methods: melt hot pressing, electrostatic spinning, and hot solvent casting.
[0054] In the embodiments of the present application, the composite electrolyte membrane can be obtained by one of the following methods: melt hot pressing, electrostatic spinning, hot solvent casting, and the method of obtaining is simple.
[0055] In addition, the raw material components of the above-mentioned composite electrolyte membrane also include: a solvent, which can be N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), and dimethyl carbonate (DMC). The above-mentioned solvent has a large polarity and is conducive to dissolving polymers and lithium salts.
[0056] In a second aspect, the present application provides a lithium-ion battery, wherein the lithium-ion battery comprises the composite electrolyte membrane described in any one of the embodiments of the first aspect.
[0057] The lithium-ion battery is realized based on the above-mentioned composite electrolyte membrane. The specific raw material components of the composite electrolyte membrane can refer to the above-mentioned embodiments. Since the lithium-ion battery adopts part or all of the technical solutions of the above-mentioned embodiments, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be described one by one here.
[0058] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0059] Example 1
[0060] A composite electrolyte membrane, the raw material components of the composite electrolyte membrane include:
[0061] PEO-PAN-PPC (weight ratio 1:1:1), LiClO4 / LiTFSI / LiBOB (weight ratio 1:1:1) polymer and lithium salt weight ratio is 4:1, LLZTO is 30% of the raw material components of the composite electrolyte membrane.
[0062] A preparation method of a composite electrolyte diaphragm comprises: using a ternary material (Ni83), an adhesive PVDF, and a conductive agent in a ratio of 95:3:2, mixing them evenly, coating them on a current collector aluminum foil, and drying them for use; using a graphite negative electrode as a negative electrode, using PEO-PAN-PPC (weight ratio of 1:1:1) as a composite electrolyte diaphragm, adding LiClO4 / LiTFSI / LiBOB (weight ratio of 1:1:1), and the polymer to lithium salt ratio is 4:1 by weight, weighing the polymer and the lithium salt in proportion, putting them into a mixer for internal mixing, mixing them evenly, adding 30% LLZTO (30% of the total mass), mixing them evenly, and hot pressing them to obtain a composite electrolyte diaphragm.
[0063] After assembling the solid-state battery containing the composite electrolyte membrane of Example 1 by stacking, the battery was placed in a 60° C. constant temperature box for 2 hours and then subjected to performance testing. The test results are shown in Table 1 for the battery cycle performance.
[0064] Table 1 Battery cycle performance
[0065]
[0066]
[0067] Example 2
[0068] A composite electrolyte membrane, the raw material components of the composite electrolyte membrane include:
[0069] PCL-PMMA-PVDF (weight ratio 1:1:1), LiFSI / LiDFOB / LiBF4 (weight ratio 1:1:1) polymer and lithium salt weight ratio is 8:1, LLZTO is 30% of the raw material components of the composite electrolyte membrane.
[0070] A preparation method of a composite electrolyte diaphragm comprises: using a ternary material (Ni83), an adhesive PVDF, and a conductive agent in a ratio of 95:3:2, mixing them evenly and coating them on a current collector aluminum foil, and drying them for use; using a graphite negative electrode as a negative electrode, using PCL-PMMA-PVDF (weight ratio of 1:1:1) as a composite electrolyte diaphragm, adding LiFSI / LiDFOB / LiBF4 (weight ratio of 1:1:1), and the polymer to lithium salt ratio is 8:1 by weight, weighing the polymer and the lithium salt in proportion, putting them into a mixer for internal mixing, mixing evenly and adding 30% LLZTO (30% of the total mass), mixing evenly and hot pressing to obtain a composite electrolyte diaphragm.
[0071] After assembling the solid-state battery containing the composite electrolyte membrane of Example 2 by stacking, the battery was placed in a 60° C. constant temperature box for 2 hours and then subjected to performance testing. The test results are shown in Table 2 for the battery cycle performance.
[0072] Table 2 Battery cycle performance
[0073] positive electrode Cycle rate Cycle number Capacity retention rate Ni83 1C 100 94.94%
[0074] Example 3
[0075] A composite electrolyte membrane, the raw material components of the composite electrolyte membrane include:
[0076] PEG-PI-PDOL (weight ratio 1:1:1), LiPF6 / LiBOB / LiTFSI (weight ratio 1:1:1) were added, the weight ratio of polymer to lithium salt was 10:1, and LLZTO was 30% of the raw material components of the composite electrolyte membrane.
[0077] A preparation method of a composite electrolyte diaphragm comprises: using a ternary material (Ni83), an adhesive PVDF, and a conductive agent in a ratio of 95:3:2, mixing them evenly, coating them on a current collector aluminum foil, and drying them for use; using a graphite negative electrode as a negative electrode, using PEG-PI-PDOL (weight ratio of 1:1:1) as a composite electrolyte diaphragm, adding LiPF6 / LiBOB / LiTFSI (weight ratio of 1:1:1), and the polymer to lithium salt ratio is 10:1 by weight, weighing the polymer and the lithium salt in proportion, putting them into a mixer for internal mixing, mixing them evenly, adding 30% LLZTO (30% of the total mass), mixing them evenly, and hot pressing them to obtain a composite electrolyte diaphragm.
[0078] After assembling the solid-state battery containing the composite electrolyte membrane of Example 3 by stacking, the battery was placed in a 60° C. constant temperature box for 2 hours and then subjected to performance testing. The test results are shown in Table 3 for the battery cycle performance.
[0079] Table 3 Battery cycle performance
[0080] positive electrode Cycle rate Cycle number Capacity retention rate Ni83 1C 100 97.04%
[0081] Comparative Example 1
[0082] A composite electrolyte membrane, the raw material components of the composite electrolyte membrane include:
[0083] PEO-PAN (weight ratio 1:1:1), add LiClO4 / LiBOB (weight ratio 1:1)
[0084] The weight ratio of polymer to lithium salt is 10:1, and LLZTO accounts for 30% of the raw material components of the composite electrolyte separator.
[0085] A preparation method of a composite electrolyte diaphragm comprises: using a ternary material (Ni83), an adhesive PVDF, and a conductive agent in a ratio of 95:3:2, mixing them evenly and coating them on a current collector aluminum foil, and drying them for use; using a graphite negative electrode as a negative electrode, using PEO-PAN (weight ratio 1:1) as a composite electrolyte diaphragm, adding LiClO4 / LiBOB (weight ratio 1:1), and the polymer to lithium salt ratio is 10:1 by weight, weighing the polymer and the lithium salt in proportion, putting them into a mixer for internal mixing, mixing them evenly and adding 30% LLZTO (30% of the total mass), mixing them evenly and hot pressing them to obtain a composite electrolyte diaphragm.
[0086] After assembling the solid-state battery containing the composite electrolyte membrane of Comparative Example 1 by stacking, the battery was placed in a 60° C. constant temperature box for 2 hours and then subjected to performance testing. The test results are shown in Table 4 for the battery cycle performance.
[0087] Table 4 Battery cycle performance
[0088] positive electrode Cycle rate Cycle number Capacity retention rate Ni83 1C 100 62.68%
[0089] Figure 1 A battery cycle test diagram provided in Example 1 of the present application; Figure 2 A battery cycle test diagram provided in Example 2 of the present application; Figure 3 A battery cycle test diagram provided in Example 3 of the present application; see Figures 1 to 3 , and combined with Tables 1 to 3, it is shown that the battery still has a capacity retention rate of more than 94% after 100 cycles; Figure 4 A battery cycle test diagram provided for comparative example 1 of this application; see Figure 4 , combined with Table 4, it is shown that the capacity retention rate of the battery after 100 cycles is much lower than that of Examples 1 to 3.
[0090] In addition, the interface impedance test and conductivity calculation of the electrolyte of case 1 and the comparative electrolyte were carried out by electrochemical impedance spectroscopy (EIS). Figure 5 This is an interfacial impedance test diagram of a composite electrolyte membrane provided in Example 1 of the present application;
[0091] Figure 6 This is a graph of the interfacial impedance test of a composite electrolyte membrane provided in Comparative Example 1 of the present application; see Figures 5-6 ; Among them, the impedance of the composite electrolyte membrane of Example 1 is 1.83Ω, and the conductivity is 7.14*10 -4 S / cm; the impedance of the composite electrolyte membrane of Comparative Example 1 is 58.59Ω, and the conductivity is 2.23*10 -5 In summary, the battery cycle test and the interface impedance test indicate that the interface impedance of the composite electrolyte membrane of the embodiment of the present application is smaller and more stable, and the corresponding battery has a higher capacity retention rate.
[0092] Figure 7 This is an appearance diagram of a composite electrolyte membrane provided in an embodiment of the present application; Figure 8 This is an appearance diagram of a composite electrolyte membrane provided in an embodiment of the present application heated to 200°C; see Figures 7-8 , indicating that the shrinkage rate of the composite electrolyte membrane provided in the embodiment of the present application after being heated to 200°C is extremely low, which can be less than 5%. Please refer to the thermal shrinkage rate of the composite electrolyte membrane heated to 200°C shown in Table 5.
[0093] Table 5 Thermal shrinkage of composite electrolyte membrane heated to 200°C
[0094] Serial number Thermal shrinkage% Example 2 1.3 Example 3 1.5 Example 4 1.1 Comparative Example 1 54.8
[0095] As shown in Table 5, the thermal shrinkage of the composite electrolyte membranes provided in Examples 1 to 3 of the present application when heated to 200°C is not higher than 1.5%, and the high entropy polymer system contributes to the flexible matrix; the high entropy lithium salt system can ensure the stability of the interface and the rapid transmission of lithium ions, and the inorganic lithium salt therein can also improve the thermal shrinkage performance of the electrolyte membrane; and the ceramic oxide electrolyte with excellent thermal stability is used to further improve the thermal shrinkage performance, which is ultimately reflected in the extremely low shrinkage of the composite electrolyte membranes of the present application after being heated to 200°C, which can be less than 5%. The thermal shrinkage of the composite electrolyte membrane in Comparative Example 1 when heated to 200°C is much higher than 5%.
[0096] One or more technical solutions provided in the embodiments of the present application also have at least the following beneficial effects or advantages:
[0097] (1) To address the problems of high polymer crystallinity, unstable interface and short life in organic-inorganic composite solid electrolytes, the high entropy of the polymer system is increased, three or more polymers are used as the polymer matrix, the disorder of the system is increased, the crystallinity of the polymer is reduced, the proportion of non-crystalline regions is increased, and the migration rate of lithium ions is increased;
[0098] (2) The lithium salt uses a combination of three or more lithium salts, and adopts an organic-inorganic lithium salt composite method. Under the action of the electric field, the organic lithium salt and the inorganic lithium salt will adhere to the negative electrode to form a layer that acts as an artificial SEI film, thereby reducing the consumption of active lithium;
[0099] (3) Through the synergistic effect of the high entropy polymer system and the high entropy lithium salt system, not only can the crystallinity of the polymer be reduced, but also the stability of the interface can be ensured and the electrochemical performance of the electrolyte can be improved, thereby extending the cycle life of the solid-state battery;
[0100] (4) The raw materials provided in the embodiments of the present application are easily available and inexpensive, which is conducive to planned promotion and application;
[0101] (5) The high entropy polymer system contributes to the flexible matrix; the high entropy lithium salt system can ensure the interface stability and the rapid transmission of lithium ions, and the inorganic lithium salt therein can also improve the thermal shrinkage performance of the electrolyte membrane; and the ceramic oxide electrolyte with excellent thermal stability is coordinated to further improve the thermal shrinkage performance, which is ultimately reflected in the composite electrolyte membrane of the embodiment of the present application having an extremely low shrinkage rate after heating to 200°C, which can be less than 5%;
[0102] (6) By introducing oxide ceramic electrolytes into the high entropy polymer system and the high entropy lithium salt system, the composite solid electrolyte membrane has good interface stability, extremely low thermal shrinkage and long cycle life.
[0103] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A composite electrolyte membrane, characterized in that: The raw material components of the composite electrolyte membrane include: Three or more polymers, three or more lithium salts and oxide ceramic electrolytes; wherein, The lithium salt comprises at least one inorganic lithium salt and at least two organic lithium salts; The weight ratio of the polymer to the lithium salt is (3-12):
1.
2. The composite electrolyte membrane according to claim 1, characterized in that The weight ratio of the polymer to the lithium salt is (4-10):
1.
3. The composite electrolyte membrane according to claim 1, characterized in that: The inorganic lithium salt includes at least one of the following: lithium perchlorate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium nitrate, and lithium difluorophosphate.
4. The composite electrolyte membrane according to claim 1, characterized in that: The organic lithium salt includes at least two of the following: lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium difluorooxalatoborate, and lithium bis(oxalateborate).
5. The composite electrolyte membrane according to claim 1, characterized in that: The weight ratio of the inorganic lithium salt to the organic lithium salt is 1:(1-3).
6. The composite electrolyte membrane according to any one of claims 1 to 5, characterized in that: The polymer includes at least three of the following: polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polycaprolactone, polypropylene polycarbonate, polyimide, polymethyl methacrylate, poly-1,2-dioxolane, polyvinylidene fluoride-hexafluoropropylene, and polyethylene glycol.
7. The composite electrolyte membrane according to claim 1, characterized in that: The oxide ceramic electrolyte includes at least one of the following: lithium aluminum titanium phosphate, lithium lanthanum zirconate, tantalum-doped lithium lanthanum zirconate, lithium phosphosulfuryl chloride, and lithium germanium phosphosulfuryl chloride.
8. The composite electrolyte membrane according to claim 1, characterized in that: The oxide ceramic electrolyte is present in an amount of 0.1 to 0.4 parts by weight relative to 1 part by weight of the raw material components of the composite electrolyte separator.
9. The composite electrolyte membrane according to claim 1, characterized in that: The composite electrolyte membrane is obtained by one of the following methods: melt hot pressing, electrostatic spinning, and hot solvent casting.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the composite electrolyte membrane according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method and application of incombustible composite-based solid electrolyte membrane
CN114583252A
Composite solid electrolyte membrane and preparation method thereof
CN116130748A
Solid electrolyte membrane and preparation method and application thereof
CN116646594A
Composite solid electrolyte diaphragm and preparation method thereof
CN116937068A
Ternary functional lithium salt-based cross-linked network structure solid polymer electrolyte, preparation method thereof and solid lithium secondary battery
CN118336106A
Cited By
High-entropy alloy composite solid electrolyte and preparation method thereof
CN120999092A