Integrated construction method of composite solid-state zinc ion battery

Through electrospinning technology, the dense metal organic frame fiber membrane and in-situ impregnation composite polar polymer is spun to build an integrated composite solid zinc ion battery, solving the challenges of solid zinc ion battery in terms of ion conductivity and mechanical strength. Efficient electrochemical performance and simplified preparation process are achieved.

CN118919879AActive Publication Date: 2024-11-08EAST CHINA UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411253924.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-08
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

Existing solid-state zinc ion batteries have challenges in ionic conductivity and mechanical strength, resulting in low zinc ion conductivity and complex assembly process, limiting their large-scale production.

Method used

The 'ans hole-type' skeleton structure fiber membrane with dense metal organic frame material is spun by electrospinning technology, and the polar polymer containing zinc salt is compounded through in-situ impregnation method to build an integrated composite solid zinc ion battery. Achieve close bonding between the electrode and the electrolyte to reduce the interface impedance.

Benefits of technology

It significantly improves zinc ion conductivity and mechanical strength, enhances the interface stability between the electrode and the electrolyte layer, simplifies the preparation process, improves production efficiency, and provides a more effective solution for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919879A_ABST
    Figure CN118919879A_ABST
Patent Text Reader

Abstract

The invention discloses an integrated construction method of a composite solid-state zinc ion battery, which comprises the following steps of: 1, spinning an ant-cave-shaped skeleton structure fiber membrane with a compact metal organic framework material by using a zinc foil as a receiver and adopting an electrostatic spinning technology; and the integrated composite solid-state zinc ion battery is constructed. According to the preparation method, an electrostatic spinning technology is adopted for spinning the ant-cave-shaped framework structure fiber membrane with a compact metal organic framework material on the surface, the mechanical meshing and chemical bonding effects between an electrode and an electrolyte layer are enhanced through the adhesion of nanofibers, and construction of an electrode / electrolyte layer integrated interface is really achieved. The ion transmission path is obviously shortened, the interface impedance is reduced, and the interface slippage in the stretching process is effectively prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of new energy materials, and in particular, relates to an integrated construction method of a composite solid-state zinc ion battery. Background Art

[0002] Zinc-ion batteries (AZIBs) are known for their inherent safety, abundant reserves, and low Zn / Zn ratio of -0.76 V relative to standard hydrogen electrode (SHE). 2+ It has attracted much attention due to its standard redox potential and simple manufacturing process. When zinc-ion batteries based on liquid electrolytes undergo various mechanical deformations, electrolyte leakage may endanger the battery's cycle performance. In addition, water-based liquid electrolytes can bring some thorny problems to the device, including the formation of zinc dendrites on the anode, hydrogen evolution reaction, the formation of by-products, and the dissolution of cathode materials, which leads to rapid decay of battery capacity. Solid-state zinc-ion batteries based on solid electrolytes do not contain active water molecules, and can alleviate the above problems to a certain extent by converting the solid-liquid interface between the electrodes into a solid-solid interface. Therefore, in recent years, more and more researchers have begun to develop new solid electrolytes that can act as both separators and electrolytes, thereby facilitating the battery preparation process and stabilizing the structure of flexible devices. Cui Guanglei from the Qingdao Institute of Bioenergy and Process Technology, Chinese Academy of Sciences, and Zhou Xinhong's team from Qingdao University of Science and Technology have disclosed a novel solid-state electrolyte based on Zn(TFSI) 2 The Zn 2+ Conductive solid electrolyte (ZCE), TFSI - Anions in TiO 2 The preferential adsorption of the Lewis acid surface of the nucleating agent weakens the ionic bonding, thus accelerating the Zn 2+ Migration (Angew.Chem.Int.Ed.2022,61,e202113086). A patent application with publication number CN114621408A discloses a polymer electrolyte that introduces a group capable of dynamically coordinating with zinc ions into a polyether-based polymer skeleton; a patent application with publication number CN113078372A discloses a sandwich structure hydrophilic zinc ion solid electrolyte and its application and preparation method in quasi-solid-state zinc ion batteries. Although the solid electrolytes prepared above all have certain flexibility, the slow reaction kinetics and poor interfacial compatibility at the interface between the electrode and the solid electrolyte result in low zinc ion conductivity. In addition, due to many problems such as low mechanical strength and complex assembly process, the large-scale production of zinc ion solid-state batteries is limited.

[0003] The patent application with publication number CN118040099A discloses an integrated structure of negative electrode and electrolyte, and its preparation method and application, wherein the integrated structure of negative electrode and electrolyte includes a zinc powder pole piece, an organic electrolyte and an aqueous electrolyte layer, wherein the organic electrolyte is distributed in the zinc powder pole piece, and the aqueous electrolyte layer is disposed on the surface of one side of the zinc powder pole piece. The integrated structure of negative electrode and electrolyte provided by the present application can effectively inhibit dendrite growth and reduce the probability of side reactions during the battery charge and discharge cycle, thereby improving the zinc utilization rate of the negative electrode and enhancing the structural stability of the integrated structure of negative electrode and electrolyte.

[0004] The patent application with publication number CN114628164A discloses a new strategy for the integrated in-situ construction of a flexible and stretchable supercapacitor. First, an integrated flexible and stretchable precursor fiber membrane with a "sandwich" structure is spun layer by layer using electrospinning technology, and then a conductive polymer is grown in situ on an electrode precursor fiber containing an oxidant by a gas phase polymerization method. Finally, an integrated flexible and stretchable supercapacitor is obtained by impregnating the fiber with an electrolyte and encapsulating the fiber. The integrated flexible and stretchable supercapacitor constructed by the present invention utilizes mechanical meshing and chemical bonding between nanofibers to achieve a strong interface bond and low interface impedance between the electrode / electrolyte, thereby giving the supercapacitor the ability to improve electrochemical stability during deformation.

[0005] Based on the above background, preparing an integrated composite solid-state zinc-ion battery and evolving the overall structure from a three-dimensional stacking structure to a two-dimensional dense film is one of the most effective strategies to achieve energy storage devices that simultaneously improve both ionic conductivity and deformation capacity. Summary of the invention

[0006] The purpose of the present invention is to provide a novel integrated construction method for a composite solid-state zinc ion battery. First, an "ant-hole-type" skeleton structure fiber membrane with a dense metal organic framework material is spun on a zinc foil by electrospinning technology, and then a polar polymer containing a zinc salt is compounded by an in-situ impregnation method to construct an integrated composite solid-state zinc ion battery, thereby achieving close integration between the components, significantly reducing the interface impedance, and effectively solving the challenges of current solid-state zinc ion batteries in terms of ionic conductivity and mechanical strength.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] The first aspect of the present invention provides an integrated construction method of a composite solid-state zinc ion battery, comprising the following steps:

[0009] In the first step, zinc foil is used as a receiver and electrospinning technology is used to spin an "ant nest type" skeleton structure fiber membrane with dense metal organic framework materials:

[0010] Dissolving a metal salt in a first organic solvent, dissolving an organic ligand in a first organic solvent, mixing the two solutions, wherein the molar ratio of the metal salt to the organic ligand is 1:1 to 8 (preferably 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:8), and after the reaction is complete, washing to obtain a metal organic framework material;

[0011] The metal salt is selected from at least one of zinc nitrate hexahydrate, cobalt nitrate hexahydrate and zirconium tetrachloride.

[0012] The organic ligand is selected from at least one of terephthalic acid and 2-methylimidazole.

[0013] The metal organic framework material is uniformly dispersed in a mixed organic solvent, wherein the mixed organic solvent is made of a second organic solvent and a third organic solvent in a mass ratio of 1:1 to 4 (preferably 1:1, 1:2, 1:3, 1:4), a fluorine-containing elastic polymer is added, and a cross-linking agent is added to the above solution, and the mass ratio of the fluorine-containing elastic polymer to the entire mixed solution is controlled to be 5wt% to 10wt% (preferably 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%). ), the mass ratio of the fluorinated elastic polymer to the metal organic framework material is 1:0.03-0.2 (preferably 1:0.04, 1:0.05, 1:0.06, 1:0.1, 1:0.15, 1:0.2), and the mass ratio of the fluorinated elastic polymer to the cross-linking agent is 1:0.02-0.06 (preferably 1:0.02, 1:0.03, 1:0.04, 1:0.05, 1:0.06), to obtain an "ant nest type" fiber membrane precursor spinning solution A;

[0014] The fluorine-containing elastic polymer is selected from at least one of fluorine rubber and polyvinylidene fluoride.

[0015] The cross-linking agent is at least one selected from hexamethylenediamine, tetraethylenetriamine and triethylenetetramine.

[0016] Using zinc foil as a receiver, spinning solution A is subjected to electrospinning technology to obtain zinc foil covered with an "ant-hole type" fiber membrane with metal organic framework material, and the membrane thickness is controlled at 20 to 70 microns (preferably 20, 30, 40, 50, 60, 70 microns).

[0017] The second step is to use an in-situ impregnation method to compound a polar polymer containing zinc salt to construct an integrated composite solid-state zinc ion battery

[0018] Dissolving a zinc salt in a fourth organic solvent, adding a polar polymer, wherein the mass percentage of the polar polymer in the fourth organic solvent is 3-7 wt% (preferably 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%), and the mass ratio of the zinc salt to the polar polymer is 1:1-5 (preferably 1:1, 1:2, 1:3, 1:4, 1:5), to obtain an impregnation solution B;

[0019] The zinc salt is selected from at least one of zinc trifluoromethanesulfonate, zinc sulfate, zinc chloride and zinc bromide.

[0020] The polar polymer is selected from at least one of polyethylene oxide, poly(vinylidene fluoride-co-hexafluoropropylene), and polyacrylonitrile.

[0021] Casting the impregnation solution B on the zinc foil covered with the "ant nest type" fiber membrane with the metal organic framework material, and drying it at a temperature of 40 to 70° C. (preferably 40° C., 50° C., 60° C., 70° C.) for 4 to 12 hours (preferably 4, 5, 6, 7, 12 hours) to obtain an integrated composite solid zinc ion electrolyte;

[0022] The positive electrode active material, conductive carbon black and binder in a mass ratio of 1 to 10:1 to 3:1 (preferably 7:2:1) are mixed and stirred into a uniform slurry, and the slurry is cast on a titanium foil by a doctor blade method. After drying, it is used as a positive electrode material. The effective mass loading of the positive electrode material is 0.3 to 0.8 mg / cm 2 (preferably 0.3, 0.4, 0.5, 0.6, 0.7, 0.8); combine and package the integrated composite solid-state zinc ion electrolyte and the positive electrode material of the same size to obtain an integrated composite solid-state zinc ion battery.

[0023] The first organic solvent is selected from at least one of methanol, ethanol, acetone, butanone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, acetonitrile, ethylene glycol, and propylene glycol.

[0024] The second organic solvent is selected from at least one of acetone and butanone.

[0025] The third organic solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone.

[0026] The mass ratio of the metal organic framework material ZIF-8 to the mixed organic solvent is 1:20 to 800 (preferably 1:190, 1:473.5, 1:263.5, 1:259, 1:99.6, 1:58.7).

[0027] The conditions for the electrospinning are: voltage 12-20 kV (preferably 12, 13, 14, 16, 18, 19, 20 kV), humidity 10-30% (preferably 10, 20, 30%), and the distance from the spinning needle to the receiver is 9-21 cm (preferably 9, 10, 12, 15, 17, 19, 20 cm).

[0028] The fourth organic solvent is selected from at least one of acetonitrile, ethylene glycol, and propylene glycol.

[0029] The binder is selected from PVDF.

[0030] The positive electrode active material is at least one of vanadium-based oxides, manganese-based oxides, polyaniline, and activated carbon.

[0031] The vanadium-based oxide is selected from vanadium oxide and vanadium pentoxide.

[0032] The manganese-based oxide is selected from manganese dioxide.

[0033] Due to the adoption of the above technical solution, the present invention has the following advantages and beneficial effects:

[0034] The present invention uses electrospinning technology to spin an "ant-hole-type" skeleton-structured fiber membrane with a dense metal organic framework material on the surface. The adhesion of the nanofibers enhances the mechanical meshing and chemical bonding between the electrode and the electrolyte layer, and truly achieves the construction of an integrated electrode / electrolyte layer interface. It not only significantly shortens the ion transmission path and reduces the interface impedance, but also effectively prevents the interface slippage that occurs during the stretching process.

[0035] The metal organic framework material prepared by the present invention has a unique pore structure and can form additional single ion fast channels. The fluorine in the fluorine-containing elastic polymer can regulate the electron distribution along the porous channels, thereby enhancing the capture and dissociation of anions. The two synergistically promote the migration kinetics of zinc ions and greatly improve the ionic conductivity.

[0036] The strategy proposed in the present invention of combining electrospinning and in-situ impregnation on the electrode to construct an integrated composite solid-state zinc ion battery not only provides support and stability for the electrode material, prevents the electrode material from deformation or peeling during the charging and discharging process, but also simplifies the preparation process and improves production efficiency, providing more effective solutions and innovative technologies for the large-scale production of integrated flexible energy storage devices.

[0037] The new strategy for the integrated construction of composite solid-state zinc ion batteries proposed in this invention first uses zinc foil as a receiver and uses electrospinning technology to spin a fiber skeleton with an "ant nest" structure. The dense metal organic framework material on the skeleton surface can construct Zn 2+The fiber skeleton is immersed in a polymer containing zinc salt, and the ion migration is accelerated by polar group coordination. Finally, the positive electrode material is configured and encapsulated to obtain an integrated composite solid-state zinc ion battery. The ultra-high mechanical strength of the fiber skeleton and the fast ion transport mechanism of the active group locking the anion enable the integrated composite solid-state zinc ion battery of the present invention to have higher ion conductivity and specific capacity retention rate during the cycle. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 The present invention is a schematic diagram of the integrated construction process of the composite solid-state zinc ion battery.

[0039] Figure 2 This is a schematic diagram of a field emission scanning electron microscope photograph of an "ant-hive-type" skeleton structure fiber membrane with a dense metal organic framework material constructed in Example 1.

[0040] Figure 3 This is a schematic diagram of the ionic conductivity of the integrated composite solid-state zinc ion electrolyte constructed in Example 1 at different temperatures.

[0041] Figure 4 Schematic diagram of the specific capacity and coulombic efficiency of the integrated composite solid-state zinc ion battery constructed in Example 1 during the charge and discharge cycle. DETAILED DESCRIPTION

[0042] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0043] Example 1

[0044] The construction method of integrated composite solid-state zinc ion battery is as follows Figure 1 As shown, Figure 1 The schematic diagram of the integrated construction process of the composite solid-state zinc ion battery of the present invention comprises the following steps:

[0045] In the first step, zinc foil is used as a receiver and electrospinning technology is used to spin an "ant nest type" skeleton structure fiber membrane with dense metal organic framework materials:

[0046] 0.008 mol of zinc nitrate hexahydrate was dissolved in 30 mL of methanol, and 0.064 mol of 2-methylimidazole was dissolved in 60 mL of methanol. The two solutions were mixed, and the molar ratio of zinc nitrate hexahydrate to 2-methylimidazole was 1:8. The mixture was reacted for 24 h, and centrifuged and washed with 40 mL of methanol each time. Washing was performed three times to obtain 0.65 g of metal organic framework material ZIF-8.

[0047] 0.096g of metal organic framework material ZIF-8 is uniformly dispersed in 18.256g of mixed organic solvent, which is made of acetone and N,N-dimethylformamide in a mass ratio of 1:2, and then 1.6g of fluororubber is dissolved in the above solution, and finally 0.048g of hexamethylenediamine is added to the above solution, and the mass ratio of fluororubber to the whole mixed solution is controlled to be 8wt%, the mass ratio of fluororubber to metal organic framework material ZIF-8 is 1:0.06, and the mass ratio of fluororubber to hexamethylenediamine is 1:0.03, to obtain 20g of "ant nest type" fiber membrane precursor spinning solution A.

[0048] Using zinc foil as a receiver, spinning solution A was electrospinned to produce zinc foil covered with an "ant-hole-shaped" fiber membrane of metal organic framework material ZIF-8, and the thickness of the membrane layer was controlled at 40 microns. Electrospinning conditions: voltage of 18 kV, humidity of 10%, and the distance from the spinning needle to the receiver was 17 cm.

[0049] The results were characterized by field emission scanning electron microscopy. Figure 2 As shown, Figure 2 This is a schematic diagram of a field emission scanning electron microscope photo of an "ant-hole-type" skeleton structure fiber membrane with a dense metal organic framework material constructed in Example 1. As can be seen from the figure, the nanofibers are intertwined or staggered. This structure increases the flexibility and strength of the fiber and ensures the stable operation of the electrochemical performance during the deformation process. At the same time, an "ant-hole" structure with well-developed pores is formed, which provides natural favorable conditions for subsequent in-situ impregnation. More importantly, the metal organic framework material evenly distributed on the surface has a unique pore structure, which can form additional zinc single ion fast channels.

[0050] The second step is to use an in-situ impregnation method to compound a polar polymer containing zinc salt to construct an integrated composite solid-state zinc ion battery

[0051] 0.5 g of zinc trifluoromethanesulfonate was dissolved in 18.5 g of acetonitrile, and 1 g of polyethylene oxide was added. The mass percentage of polyethylene oxide in the whole mixed solution was 5 wt %, and the mass ratio of zinc trifluoromethanesulfonate to polyethylene oxide was 1:2, to obtain 20 g of impregnation solution B.

[0052] 5 mL of impregnation solution B was cast on the zinc foil (size 3 cm × 3 cm) covered with the above-mentioned "ant-hole-type" fiber membrane with the metal organic framework material ZIF-8, dried at 60°C for 12 hours, and cut into a disc with a diameter of 12 mm to achieve the integration of the negative electrode and the composite solid electrolyte to obtain a composite solid zinc ion electrolyte.

[0053] 0.14 g vanadium oxide, 0.04 g conductive carbon black, and 0.02 g binder PVDF were mixed and stirred into a uniform slurry. 5 mL of the slurry was cast on a titanium foil (size 10 cm × 10 cm) by a scraper method. After drying, it was cut into a disk with a diameter of 12 mm as the positive electrode material. The effective mass loading of the positive electrode material was 0.5 mg / cm 2 The integrated composite solid-state zinc ion electrolyte and the positive electrode material of the same size are combined and packaged to obtain an integrated composite solid-state zinc ion battery.

[0054] The conductivity test and charge-discharge cycle test of the constructed integrated composite solid-state zinc ion battery were carried out at different temperatures. Figure 3 As shown, Figure 3 This is a schematic diagram of the ionic conductivity of the integrated composite solid zinc ion electrolyte constructed in Example 1 at different temperatures. It can be seen from the figure that when the temperature is 30°C, the conductivity of the integrated composite solid zinc ion electrolyte can reach 1.62×10 -4 S / cm. The results are as follows Figure 4 As shown, Figure 4 The capacity and coulombic efficiency schematic diagram of the integrated composite solid-state zinc ion battery constructed in Example 1 during the charge and discharge cycle. As can be seen from the figure, the integrated composite solid-state zinc ion battery has a charge and discharge specific capacity of up to 348mAh / g at a current density of 0.05A / g, and a capacity retention rate of about 95.7% after 50 cycles. The coulombic efficiency is close to 100%, indicating that the battery can still maintain a high energy utilization rate after multiple charge and discharge cycles. This shows that the method of the present invention enhances the interface stability between the electrode and the electrolyte, promotes the kinetics of ion migration, enables the device to operate efficiently and stably, and exhibits excellent electrochemical performance.

[0055] Example 2

[0056] The method for constructing an integrated composite solid-state zinc ion battery comprises the following steps:

[0057] In the first step, zinc foil is used as a receiver and electrospinning technology is used to spin an "ant nest type" skeleton structure fiber membrane with dense metal organic framework materials:

[0058] 0.008 mol of cobalt nitrate hexahydrate was dissolved in 30 mL of ethanol, and 0.032 mol of 2-methylimidazole was dissolved in 60 mL of ethanol. The two solutions were mixed, and the molar ratio of cobalt nitrate hexahydrate to 2-methylimidazole was 1:4. The reaction was carried out for 24 hours, and the mixture was centrifuged and washed with 40 mL of ethanol each time. Washing was performed three times to obtain 0.5 g of metal organic framework material ZIF-67.

[0059] 0.04g of metal organic framework material ZIF-67 is uniformly dispersed in 18.94g of mixed organic solvent, which is made of acetone and N,N-dimethylacetamide in a mass ratio of 1:1, and then 1g of polyvinylidene fluoride is dissolved in the above solution, and finally 0.02g of tetraethylenetriamine is added to the above solution, and the mass ratio of polyvinylidene fluoride to the whole mixed solution is controlled to be 5wt%, the mass ratio of polyvinylidene fluoride to metal organic framework material ZIF-67 is 1:0.04, and the mass ratio of polyvinylidene fluoride to tetraethylenetriamine is 1:0.02, and 20g of "ant nest type" fiber membrane precursor spinning solution A is obtained.

[0060] Using zinc foil as a receiver, spinning solution A was electrospinned to produce zinc foil covered with an "ant-hole-shaped" fiber membrane of metal organic framework material ZIF-67, with a membrane thickness of 30 microns. Electrospinning conditions: voltage of 19 kV, humidity of 10%, and a distance of 15 cm from the spinning needle to the receiver.

[0061] The second step is to use an in-situ impregnation method to compound a polar polymer containing zinc salt to construct an integrated composite solid-state zinc ion battery

[0062] 0.3 g of zinc sulfate was dissolved in 18.5 g of acetonitrile, and 1.2 g of polyethylene oxide was added, wherein the mass percentage of polyethylene oxide in the whole mixed solution was 6 wt %, and the mass ratio of zinc sulfate to polyethylene oxide was 1:4, and 20 g of impregnation solution B was obtained.

[0063] 5 mL of impregnation solution B was cast on the zinc foil (size 3 cm × 3 cm) covered with the "ant-hole-type" fiber membrane with the metal organic framework material ZIF-67, dried at 50 ° C for 7 hours, and cut into a disc with a diameter of 12 mm to achieve the integration of the negative electrode and the composite solid electrolyte to obtain a composite solid zinc ion electrolyte.

[0064] 0.14 g of vanadium-based oxide vanadium pentoxide, 0.04 g of conductive carbon black, and 0.02 g of binder PVDF were mixed and stirred into a uniform slurry. 5 mL of the slurry was cast on a titanium foil (size 10 cm × 10 cm) by a scraper method. After drying, it was cut into a disk with a diameter of 12 mm as the positive electrode material. The effective mass loading of the positive electrode material was 0.5 mg / cm 2 The integrated composite solid-state zinc ion electrolyte and the positive electrode material of the same size are combined and packaged to obtain an integrated composite solid-state zinc ion battery.

[0065] The constructed integrated composite solid-state zinc-ion battery was subjected to conductivity tests and charge-discharge cycle tests at different temperatures.

[0066] Example 3

[0067] The method for constructing an integrated composite solid-state zinc ion battery comprises the following steps:

[0068] In the first step, zinc foil is used as a receiver and electrospinning technology is used to spin an "ant nest type" skeleton structure fiber membrane with dense metal organic framework materials:

[0069] 0.008 mol of zinc nitrate hexahydrate was dissolved in 30 mL of N, N-dimethylformamide, and 0.024 mol of terephthalic acid was dissolved in 60 mL of N, N-dimethylformamide. The two solutions were mixed, and the molar ratio of zinc nitrate hexahydrate to terephthalic acid was 1:3. The mixture was reacted for 24 hours, and centrifuged and washed three times with 40 mL of N, N-dimethylformamide each time to obtain 0.75 g of metal organic framework material MOF-5.

[0070] 0.07g of metal organic framework material MOF-5 was uniformly dispersed in 18.446g of mixed organic solvent, which was made of butanone and N-methylpyrrolidone in a mass ratio of 1:3, and then 1.4g of polyvinylidene fluoride was dissolved in the above solution, and finally 0.084g of hexamethylenediamine was added to the above solution, and the mass ratio of polyvinylidene fluoride to the whole mixed solution was controlled to be 7wt%, the mass ratio of polyvinylidene fluoride to metal organic framework material MOF-5 was 1:0.05, and the mass ratio of polyvinylidene fluoride to hexamethylenediamine was 1:0.06, and 20g of "ant hole type" fiber membrane precursor spinning solution A was obtained.

[0071] Using zinc foil as a receiver, spinning solution A was electrospinned to produce zinc foil covered with an "ant-hole-shaped" fiber membrane of metal organic framework material MOF-5, and the thickness of the membrane layer was controlled at 50 microns. Electrospinning conditions: voltage of 16 kV, humidity of 20%, and the distance from the spinning needle to the receiver was 17 cm.

[0072] The second step is to use an in-situ impregnation method to compound a polar polymer containing zinc salt to construct an integrated composite solid-state zinc ion battery

[0073] 0.8 g of zinc chloride was dissolved in 18.4 g of ethylene glycol, and 0.8 g of polyacrylonitrile was added, the mass percentage of polyacrylonitrile in the whole mixed solution was 4 wt %, and the mass ratio of zinc chloride to polyacrylonitrile was 1:1, to obtain 20 g of impregnation solution B.

[0074] 5 mL of impregnation solution B was cast on the zinc foil (size 3 cm × 3 cm) covered with the above-mentioned "ant-hole-type" fiber membrane with the metal organic framework material MOF-5, dried at 40°C for 12 hours, and cut into a disc with a diameter of 12 mm to achieve the integration of the negative electrode and the composite solid electrolyte to obtain a composite solid zinc ion electrolyte.

[0075] 0.14 g of manganese dioxide, 0.04 g of conductive carbon black, and 0.02 g of binder PVDF were mixed and stirred into a uniform slurry. 5 mL of the slurry was cast on a titanium foil (size 10 cm × 10 cm) by a scraper method. After drying, it was cut into a disk with a diameter of 12 mm as the positive electrode material. The effective mass loading of the positive electrode material was 0.7 mg / cm 2 The integrated composite solid-state zinc ion electrolyte and the positive electrode material of the same size are combined and packaged to obtain an integrated composite solid-state zinc ion battery.

[0076] The constructed integrated composite solid-state zinc-ion battery was subjected to conductivity tests and charge-discharge cycle tests at different temperatures.

[0077] Example 4

[0078] The method for constructing an integrated composite solid-state zinc ion battery comprises the following steps:

[0079] In the first step, zinc foil is used as a receiver and electrospinning technology is used to spin an "ant nest type" skeleton structure fiber membrane with dense metal organic framework materials:

[0080] 0.008 mol of zirconium tetrachloride was dissolved in 30 mL of N, N-dimethylformamide, and 0.008 mol of terephthalic acid was dissolved in 60 mL of N, N-dimethylformamide. The two solutions were mixed, with a molar ratio of zirconium tetrachloride to terephthalic acid of 1:1. The reaction was carried out for 24 hours, and centrifuged and washed with 40 mL of N, N-dimethylformamide each time. Wash three times to obtain 0.6 g of the metal organic framework material Uio-66.

[0081] 0.072g of metal organic framework material Uio-66 is uniformly dispersed in 18.68g of mixed organic solvent, which is made of acetone and N-methylpyrrolidone in a mass ratio of 1:2. Then 1.2g of fluororubber is dissolved in the above solution, and finally 0.048g of triethylenetetramine is added to the above solution. The mass ratio of fluororubber to the whole mixed solution is controlled to be 6wt%, the mass ratio of fluororubber to metal organic framework material Uio-66 is 1:0.06, and the mass ratio of fluororubber to triethylenetetramine is 1:0.04, to obtain 20g of "ant nest type" fiber membrane precursor spinning solution A.

[0082] Using zinc foil as a receiver, spinning solution A was electrospinned to produce zinc foil covered with an "ant-hole-shaped" fiber membrane of metal organic framework material Uio-66, with a membrane thickness of 20 microns. Electrospinning conditions: voltage of 14 kV, humidity of 30%, and a distance of 20 cm from the spinning needle to the receiver.

[0083] The second step is to use an in-situ impregnation method to compound a polar polymer containing zinc salt to construct an integrated composite solid-state zinc ion battery

[0084] 0.16 g of zinc bromide was dissolved in 19.04 g of propylene glycol, and 0.8 g of poly(vinylidene fluoride-co-hexafluoropropylene) was added, the mass percentage of poly(vinylidene fluoride-co-hexafluoropropylene) in the whole mixed solution was 4 wt %, and the mass ratio of zinc bromide to poly(vinylidene fluoride-co-hexafluoropropylene) was 1:5, and 20 g of impregnation solution B was obtained.

[0085] 5 mL of impregnation solution B was cast on the zinc foil (size 3 cm × 3 cm) covered with the "ant-hole-type" fiber membrane with the metal organic framework material Uio-66, dried at 60 ° C for 12 hours, and cut into a disc with a diameter of 12 mm to achieve the integration of the negative electrode and the composite solid electrolyte to obtain a composite solid zinc ion electrolyte.

[0086] 0.14 g polyaniline, 0.04 g conductive carbon black, and 0.02 g binder PVDF were mixed and stirred into a uniform slurry. 5 mL of the slurry was cast on a titanium foil (size 10 cm × 10 cm) by a scraper method. After drying, it was cut into a disk with a diameter of 12 mm as the positive electrode material. The effective mass loading of the positive electrode material was 0.3 mg / cm 2 The integrated composite solid-state zinc ion electrolyte and the positive electrode material of the same size are combined and packaged to obtain an integrated composite solid-state zinc ion battery.

[0087] The constructed integrated composite solid-state zinc-ion battery was subjected to conductivity tests and charge-discharge cycle tests at different temperatures.

[0088] Example 5

[0089] The method for constructing an integrated composite solid-state zinc ion battery comprises the following steps:

[0090] In the first step, zinc foil is used as a receiver and electrospinning technology is used to spin an "ant nest type" skeleton structure fiber membrane with dense metal organic framework materials:

[0091] 0.008 mol of zinc nitrate hexahydrate was dissolved in 30 mL of ethanol, and 0.048 mol of 2-methylimidazole was dissolved in 60 mL of ethanol. The two solutions were mixed, and the molar ratio of zinc nitrate hexahydrate to 2-methylimidazole was 1:6. The mixture was reacted for 24 h, and centrifuged and washed with 40 mL of ethanol each time. Washing was performed three times to obtain 0.55 g of metal organic framework material ZIF-8.

[0092] 0.18g of metal organic framework material ZIF-8 is uniformly dispersed in 17.93g of mixed organic solvent, which is made of acetone and N,N-dimethylacetamide in a mass ratio of 1:4, and then 1.8g of fluororubber is dissolved in the above solution, and finally 0.09g of tetraethylenetriamine is added to the above solution, and the mass ratio of fluororubber to the whole mixed solution is controlled to be 9wt%, the mass ratio of fluororubber to metal organic framework material ZIF-8 is 1:0.1, and the mass ratio of fluororubber to tetraethylenetriamine is 1:0.05, to obtain 20g of "ant nest type" fiber membrane precursor spinning solution A.

[0093] Using zinc foil as a receiver, spinning solution A was electrospinned to produce zinc foil covered with an "ant-hole-shaped" fiber membrane of metal organic framework material ZIF-8, and the thickness of the membrane layer was controlled at 60 microns. Electrospinning conditions: voltage of 13 kV, humidity of 30%, and the distance from the spinning needle to the receiver was 12 cm.

[0094] The second step is to use an in-situ impregnation method to compound a polar polymer containing zinc salt to construct an integrated composite solid-state zinc ion battery

[0095] 0.47 g of zinc bromide was dissolved in 18.13 g of ethylene glycol, and 1.4 g of polyacrylonitrile was added, wherein the content of polyacrylonitrile was 7 wt % of the total mixed solution, and the mass ratio of zinc bromide to polyacrylonitrile was 1:3, to obtain 20 g of impregnation solution B.

[0096] 5 mL of impregnation solution B was cast on the zinc foil (size 3 cm × 3 cm) covered with the above-mentioned "ant-hole-type" fiber membrane with the metal organic framework material ZIF-8, dried at 70°C for 6 hours, and cut into a disc with a diameter of 12 mm to achieve the integration of the negative electrode and the composite solid electrolyte to obtain a composite solid zinc ion electrolyte.

[0097] 0.14 g of activated carbon, 0.04 g of conductive carbon black, and 0.02 g of binder PVDF were mixed and stirred into a uniform slurry. 5 mL of the slurry was cast on a titanium foil (size 10 cm × 10 cm) by a scraper method. After drying, it was cut into a disk with a diameter of 12 mm as the positive electrode material. The effective mass loading of the positive electrode material was 0.8 mg / cm 2 The integrated composite solid-state zinc ion electrolyte and the positive electrode material of the same size are combined and packaged to obtain an integrated composite solid-state zinc ion battery.

[0098] The constructed integrated composite solid-state zinc-ion battery was subjected to conductivity tests and charge-discharge cycle tests at different temperatures.

[0099] Example 6

[0100] The method for constructing an integrated composite solid-state zinc ion battery comprises the following steps:

[0101] In the first step, zinc foil is used as a receiver and electrospinning technology is used to spin an "ant nest type" skeleton structure fiber membrane with dense metal organic framework materials:

[0102] 0.008 mol of zirconium tetrachloride was dissolved in 30 mL of N, N-dimethylformamide, and 0.016 mol of terephthalic acid was dissolved in 60 mL of N, N-dimethylformamide. The two solutions were mixed, with a molar ratio of zirconium tetrachloride to terephthalic acid of 1:2. The mixture was reacted for 24 h, and centrifuged and washed with 40 mL of N, N-dimethylformamide each time. Washing was performed three times to obtain 0.72 g of the metal organic framework material Uio-66.

[0103] 0.3g of the metal organic framework material Uio-66 is uniformly dispersed in 17.62g of a mixed organic solvent, wherein the mixed organic solvent is made of butanone and N,N-dimethylformamide in a mass ratio of 1:1, and then 2g of polyvinylidene fluoride is dissolved in the above solution, and finally 0.08g of triethylenetetramine is added to the above solution, and the mass ratio of polyvinylidene fluoride to the entire mixed solution is controlled to be 10wt%, the mass ratio of polyvinylidene fluoride to the metal organic framework material Uio-66 is 1:0.15, and the mass ratio of polyvinylidene fluoride to triethylenetetramine is 1:0.04, to obtain 20g of "ant nest type" fiber membrane precursor spinning solution A.

[0104] Using zinc foil as a receiver, spinning solution A was electrospinned to obtain zinc foil covered with an "ant-hole-shaped" fiber membrane of metal organic framework material Uio-66, and the thickness of the membrane layer was controlled at 70 microns. Electrospinning conditions: voltage of 20 kV, humidity of 20%, and the distance from the spinning needle to the receiver was 9 cm.

[0105] The second step is to use an in-situ impregnation method to compound a polar polymer containing zinc salt to construct an integrated composite solid-state zinc ion battery

[0106] 0.3 g of zinc trifluoromethanesulfonate was dissolved in 19.1 g of propylene glycol, and 0.6 g of polyethylene oxide was added, the mass percentage of polyethylene oxide in the whole mixed solution was 3 wt %, and the mass ratio of zinc trifluoromethanesulfonate to polyethylene oxide was 1:2, to obtain 20 g of impregnation solution B.

[0107] 5 mL of impregnation solution B was cast on the zinc foil (size 3 cm × 3 cm) covered with the "ant-hole-type" fiber membrane with the metal organic framework material Uio-66, dried at 50°C for 10 hours, and cut into a disc with a diameter of 12 mm to achieve the integration of the negative electrode and the composite solid electrolyte to obtain a composite solid zinc ion electrolyte.

[0108] 0.14 g of manganese dioxide, 0.04 g of conductive carbon black, and 0.02 g of binder PVDF were mixed and stirred into a uniform slurry. 5 mL of the slurry was cast on a titanium foil (size 10 cm × 10 cm) by a scraper method. After drying, it was cut into a disk with a diameter of 12 mm as the positive electrode material. The effective mass loading of the positive electrode material was 0.4 mg / cm 2 The integrated composite solid-state zinc ion electrolyte and the positive electrode material of the same size are combined and packaged to obtain an integrated composite solid-state zinc ion battery.

[0109] The constructed integrated composite solid-state zinc-ion battery was subjected to conductivity tests and charge-discharge cycle tests at different temperatures.

[0110] Comparative Example 1

[0111] The method for constructing a composite solid-state zinc ion battery comprises the following steps:

[0112] In the first step, a polymer skeleton membrane with a dense metal organic framework material on the surface was constructed by glass plate casting method.

[0113] 0.008 mol of zinc nitrate hexahydrate was dissolved in 30 mL of methanol, and 0.064 mol of 2-methylimidazole was dissolved in 60 mL of methanol. The two solutions were mixed, and the molar ratio of zinc nitrate hexahydrate to 2-methylimidazole was 1:8. The mixture was reacted for 24 h, and centrifuged and washed with 40 mL of methanol each time. Washing was performed three times to obtain 0.65 g of metal organic framework material ZIF-8.

[0114] 0.096g of metal organic framework material ZIF-8 is uniformly dispersed in 18.256g of mixed organic solvent, wherein the mixed organic solvent is made of acetone and N,N-dimethylformamide in a mass ratio of 1:2, and then 1.6g of fluororubber is dissolved in the above solution, and finally 0.048g of hexamethylenediamine is added to the above solution, and the mass ratio of fluororubber to the entire mixed solution is controlled to be 8wt%, the mass ratio of fluororubber to metal organic framework material ZIF-8 is 1:0.06, and the mass ratio of fluororubber to hexamethylenediamine is 1:0.03, to obtain 20g of casting liquid A.

[0115] 10g of casting liquid A was uniformly cast on a flat glass plate (size 6cm×6cm) to form a film, and then vacuum dried for 8h. After the solvent was completely evaporated, the glass plate was removed to obtain a polymer skeleton film with a dense metal organic framework material on the surface, and the film thickness was controlled to be 40 microns.

[0116] The second step is to immerse in a polar polymer containing zinc salt and encapsulate it to construct a composite solid-state zinc ion battery.

[0117] 0.5 g of zinc trifluoromethanesulfonate was dissolved in 18.5 g of acetonitrile, and 1 g of polyethylene oxide was added. The mass percentage of polyethylene oxide in the whole mixed solution was 5 wt %, and the mass ratio of zinc trifluoromethanesulfonate to polyethylene oxide was 1:2, to obtain 20 g of impregnation solution B.

[0118] The prepared polymer skeleton membrane (size 6 cm×6 cm) with a dense metal organic framework material on the surface was immersed in 10 g of impregnation solution B for 3 minutes, taken out, dried at 60° C. for 12 hours, and cut into a disc with a diameter of 19 mm to obtain a composite solid zinc ion electrolyte.

[0119] 0.14 g vanadium oxide, 0.04 g conductive carbon black, and 0.02 g binder PVDF were mixed and stirred into a uniform slurry. 5 mL of the slurry was cast on a titanium foil (size 10 cm × 10 cm) by a scraper method. After drying, it was cut into a disk with a diameter of 12 mm as the positive electrode material. The effective mass loading of the positive electrode material was 0.5 mg / cm 2 The composite solid-state zinc ion electrolyte, zinc foil negative electrode (cut into a disc with a diameter of 12 mm) and positive electrode material are packaged together to obtain a composite solid-state zinc ion battery.

[0120] Table 1 Test results of the integrated composite solid-state zinc ion battery constructed by Examples 1 to 6 and Comparative Example 1

[0121]

[0122]

[0123] The electrochemical performance of the integrated composite solid-state zinc ion battery constructed in Examples 1 to 6 and Comparative Example 1 was tested under dynamic and static conditions. The specific test results are shown in Table 1. It can be found that the specific capacity of the entire device is basically positively correlated with the size of the ionic conductivity. Compared with Comparative Example 1, the electrospinning method forms an "ant hole" structure with well-developed pores, which is conducive to the rapid segment movement of zinc ions, thereby having a higher specific capacity and better cycle stability in the charge and discharge cycle.

[0124] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modify the technical contents suggested above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the solution of the present invention.

Claims

1. A method for constructing an integrated composite solid-state zinc ion battery, characterized in that: The following steps are involved: The first step is to dissolve the metal salt in the first organic solvent, dissolve the organic ligand in the first organic solvent, mix the two solutions, and the molar ratio of the metal salt to the organic ligand is 1:1 to 8. After the reaction is complete, washing is performed to obtain a metal organic framework material; The metal salt is selected from at least one of zinc nitrate hexahydrate, cobalt nitrate hexahydrate, and zirconium tetrachloride; The organic ligand is selected from at least one of terephthalic acid and 2-methylimidazole; The metal organic framework material is uniformly dispersed in a mixed organic solvent, wherein the mixed organic solvent is made of a second organic solvent and a third organic solvent in a mass ratio of 1:1-4, a fluorine-containing elastic polymer is added, and a cross-linking agent is added to the above solution, wherein the mass ratio of the fluorine-containing elastic polymer to the whole mixed solution is controlled to be 5wt%-10wt%, the mass ratio of the fluorine-containing elastic polymer to the metal organic framework material is 1:0.03-0.2, and the mass ratio of the fluorine-containing elastic polymer to the cross-linking agent is 1:0.02-0.06, to obtain an "ant nest type" fiber membrane precursor spinning solution A; The fluorine-containing elastic polymer is selected from at least one of fluororubber and polyvinylidene fluoride; The cross-linking agent is selected from at least one of hexamethylenediamine, tetraethylenetriamine and triethylenetetramine; Using zinc foil as a receiver, spinning solution A is electrospinned to produce zinc foil covered with "ant nest type" fiber membrane with metal organic framework material, and the thickness of the membrane layer is controlled at 20 to 70 microns; The second step is to dissolve the zinc salt in the fourth organic solvent, add the polar polymer, the content of the polar polymer in the fourth organic solvent is 3-7wt% by weight, and the mass ratio of the zinc salt to the polar polymer is 1:1-5, to obtain an impregnation solution B; The zinc salt is selected from at least one of zinc trifluoromethanesulfonate, zinc sulfate, zinc chloride and zinc bromide; The polar polymer is selected from at least one of polyethylene oxide, poly(vinylidene fluoride-co-hexafluoropropylene), and polyacrylonitrile; Casting the impregnation solution B on the zinc foil covered with the "ant nest type" fiber membrane with the metal organic framework material, and drying it at a temperature of 40 to 70° C. for 4 to 12 hours to obtain an integrated composite solid zinc ion electrolyte; The positive electrode active material, conductive carbon black and binder with a mass ratio of 1 to 10:1 to 3:1 are mixed and stirred into a uniform slurry, and the slurry is cast on a titanium foil by a doctor blade method. After drying, it is used as a positive electrode material. The effective mass loading of the positive electrode material is 0.3 to 0.8 mg / cm 2 ; Combine and package the integrated composite solid-state zinc ion electrolyte and positive electrode material of the same size to obtain an integrated composite solid-state zinc ion battery.

2. The integrated construction method of the composite solid-state zinc ion battery according to claim 1, characterized in that: The first organic solvent is selected from at least one of methanol, ethanol, acetone, butanone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, acetonitrile, ethylene glycol, and propylene glycol.

3. The integrated construction method of the composite solid-state zinc ion battery according to claim 1, characterized in that: The second organic solvent is selected from at least one of acetone and butanone.

4. The integrated construction method of the composite solid-state zinc ion battery according to claim 1, characterized in that: The third organic solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone.

5. The integrated construction method of the composite solid-state zinc ion battery according to claim 1, characterized in that: The mass ratio of the metal organic framework material ZIF-8 to the mixed organic solvent is 1:20-800.

6. The integrated construction method of the composite solid-state zinc ion battery according to claim 1, characterized in that: The conditions for the electrostatic spinning are: voltage 12-20 kV, humidity 10-30%, and a distance from the spinning needle to the receiver of 9-21 cm.

7. The integrated construction method of the composite solid-state zinc ion battery according to claim 1, characterized in that: The fourth organic solvent is selected from at least one of acetonitrile, ethylene glycol, and propylene glycol.

8. The integrated construction method of the composite solid-state zinc ion battery according to claim 1, characterized in that: The binder is selected from PVDF.

9. The integrated construction method of the composite solid-state zinc ion battery according to claim 1, characterized in that: The positive electrode active material is at least one of vanadium-based oxides, manganese-based oxides, polyaniline, and activated carbon.

10. The integrated construction method of a composite solid-state zinc ion battery according to claim 9, characterized in that: The vanadium-based oxide is selected from vanadium oxide and vanadium pentoxide; The manganese-based oxide is selected from manganese dioxide.

Citation Information

Patent Citations

  • Solid electrolyte / electrode integrated material for solid-state lithium battery as well as preparation method and application of solid electrolyte / electrode integrated material

    CN115084448A

  • All-solid-state lithium-sulfur battery based on three-dimensional metal organic framework nanofiber composite solid electrolyte

    CN117810525A

  • Class of cathode materials and secondary ion batteries containing these cathode materials

    US20230246189A1

  • In-situ preparation and application of solid polymer electrolyte

    WO2023109659A1