Composite diaphragm and battery
By setting ceramic layers containing polymer microspheres and ceramic layers containing polymers on both sides of the substrate of the lithium-ion battery composite separator, the problem of thermal runaway in lithium-ion batteries is solved, and the safety and circulation of the battery are improved performance.
Patent Information
- Application Number
- CN202411185169.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-08
AI Technical Summary
Lithium-ion batteries have safety hazards at high temperatures. Inadequate heat resistance of the diaphragm leads to thermal runaway, which may cause fire or explosion, and the closed-cell temperature is too high to block the ion channel in time.
On both sides of the substrate of the composite separator, the first ceramic layer and the second ceramic layer are arranged, wherein the first ceramic layer contains the first polymer microspheres, the second ceramic layer does not contain polymer, and the polymer microspheres in the first ceramic layer The balls melt at high temperature to form an ion barrier layer, reduce the closed-cell temperature, and improve the heat resistance and permeability of the membrane by controlling the particle size of the ceramic and the adhesion of the coating.
It effectively reduces the risk of thermal runaway in lithium-ion batteries, improves the safety performance and long-cycle performance of the battery, while taking into account low-temperature performance.
Smart Images

Figure CN118920023A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery separators, and in particular to a composite separator and a battery. Background Art
[0002] In recent years, lithium-ion batteries have been widely used in smart phones, tablet computers, smart wearables, power tools, electric vehicles, etc. With the widespread application of lithium-ion batteries, consumers' demands for the service life and application environment of lithium-ion batteries are constantly increasing, which requires lithium-ion batteries to have both low-temperature performance and good safety performance.
[0003] At present, there are safety hazards in the use of lithium-ion batteries. For example, when the battery temperature increases to a certain level, the internal temperature is out of control, which is prone to serious safety accidents, fires, or even explosions. The main reason for the thermal runaway problem of batteries is that the diaphragm is not heat-resistant enough, which causes the diaphragm to shrink or even rupture at high temperatures, and cannot isolate the positive and negative electrodes of the battery; on the other hand, the diaphragm closed-cell temperature is too high (the diaphragm closed-cell temperature refers to the temperature at which the diaphragm closes when heated. If the diaphragm closed-cell temperature is too high, the diaphragm will only close when it is subjected to high heat), which causes the diaphragm to be unable to close before thermal runaway, and unable to immediately block the ion channels inside the battery.
[0004] Based on this situation, there is an urgent need to develop lithium-ion batteries with separators with high safety performance. Summary of the invention
[0005] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a composite diaphragm and a battery. The present invention provides a first ceramic layer containing first polymer microspheres on one side of a substrate and a first ceramic layer without first polymer microspheres on the other side of the substrate. The composite diaphragm prepared can be used in a battery to improve the safety performance of the battery while taking into account the low temperature performance of the battery and having excellent long cycle performance.
[0006] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a composite diaphragm, which includes a substrate. Along the thickness direction of the substrate, the substrate has a first surface and a second surface arranged opposite to each other, a first ceramic layer is arranged on the first surface of the substrate, and a second ceramic layer is arranged on the second surface of the substrate; a first coating is arranged on the side of the first ceramic layer away from the substrate, and a second coating is arranged on the side of the second ceramic layer away from the substrate; the first ceramic layer includes a first ceramic powder and a first polymer microsphere, and the second ceramic layer includes a second ceramic powder.
[0007] The second aspect of the present invention provides a battery, which includes a positive electrode sheet, a negative electrode sheet, a composite diaphragm and an electrolyte. The composite diaphragm is the composite diaphragm described in the first aspect, the first coating of the composite diaphragm is adjacent to the negative electrode sheet, and the second coating of the composite diaphragm is adjacent to the positive electrode sheet.
[0008] Optionally, the adhesion force between the first coating layer and the negative electrode sheet is F1, 0.2N / M≤F1≤5N / M.
[0009] Optionally, the bonding force between the second coating layer and the positive electrode sheet is F2, 5N / M≤F2≤20N / M.
[0010] Optionally, the electrolyte contains propyl propionate; preferably, the content of propyl propionate is 5wt%-30wt%.
[0011] The present invention adopts the above technical solution to achieve the following beneficial effects:
[0012] The present invention arranges the first ceramic layer and the second ceramic layer on both sides of the substrate, respectively, so that the first ceramic layer contains the first polymer microspheres, and the second ceramic layer does not contain the polymer. The first polymer microspheres in the first ceramic layer can be melted under high temperature conditions to form multiple continuous ion barrier layers, reduce the closed-cell temperature of the composite diaphragm, and prevent the occurrence of further thermal runaway of the lithium-ion battery, thereby improving the safety performance of the battery; the second ceramic layer does not contain the polymer, so that the ceramic particles in the second ceramic layer can be in close contact, which is beneficial to improving the heat resistance of the composite diaphragm. Therefore, the composite diaphragm of the present invention can improve the safety performance of the battery and also improve the long cycle performance of the battery.
[0013] The endpoints and any values of the range disclosed in this article are not limited to the precise range or value, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 Shown is a schematic diagram of the cross-sectional structure of the composite diaphragm.
[0015] Description of Figure Numbers
[0016] 1. Substrate; 21. First ceramic layer; 22. Second ceramic layer; 23. First polymer microspheres; 31. First coating layer; 32. Second coating layer; 4. Negative electrode sheet; 5. Positive electrode sheet. DETAILED DESCRIPTION
[0017] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0018] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.
[0019] The first aspect of the present invention provides a composite membrane, the composite membrane comprises a substrate, along the thickness direction of the substrate, the substrate has a first surface and a second surface arranged opposite to each other, a first ceramic layer is arranged on the first surface of the substrate, and a second ceramic layer is arranged on the second surface of the substrate; a first coating is arranged on the side of the first ceramic layer away from the substrate, and a second coating is arranged on the side of the second ceramic layer away from the substrate; the first ceramic layer comprises a first ceramic powder and a first polymer microsphere, and the second ceramic layer comprises a second ceramic powder. Figure 1 As shown, the first ceramic layer 21 contains first polymer microspheres 23. The first polymer microspheres added in the first ceramic layer are conducive to reducing the closed-cell temperature of the composite diaphragm. When the temperature of the first ceramic layer reaches the closed-cell temperature or above, the morphology and structure of the first polymer microspheres will change, and they will melt to form multiple continuous ion barrier layers. The formed ion barrier layers block the current inside the battery to prevent further thermal runaway of the lithium-ion battery, thereby improving the safety performance of the battery. The absence of a polymer in the second ceramic layer is conducive to making the ceramic particles stacked more closely, further improving the thermal stability of the composite diaphragm, and maintaining good insulation at high temperatures to avoid contact between the positive and negative electrodes, thereby improving the safety performance of the battery.
[0020] In some embodiments, a first coating is disposed on a side of the first ceramic layer away from the substrate, and a second coating is disposed on a side of the second ceramic layer away from the substrate. Figure 1 As shown, a first ceramic layer 21 is arranged on one side of the substrate 1, a second ceramic layer 22 is arranged on the other side of the substrate, a first coating 31 is arranged on the first ceramic layer, and a second coating 32 is arranged on the second ceramic layer.
[0021] In some embodiments, the first ceramic layer includes a first ceramic powder and a first polymer microsphere.
[0022] In some embodiments, the first ceramic layer includes a first binder.
[0023] In some embodiments, in the first ceramic layer, the content of the first polymer microspheres is 30wt%-80wt%, for example, 30wt%, 40wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt% and 80wt%. Preferably, it is 50wt%-75wt%. When the content of the first polymer microspheres is within the above range, it is beneficial for the first polymer microspheres to melt under high temperature conditions to form multiple dense ion barrier layers, reduce the closed-pore temperature of the composite diaphragm, and prevent the occurrence of further thermal runaway of the lithium-ion battery, thereby improving the safety performance of the battery. It can also enable lithium ions to be better transmitted through the composite diaphragm, inhibit lithium precipitation, and improve the long cycle performance of the battery. When the content of the first polymer microspheres is small, a dense barrier layer cannot be formed at high temperature, resulting in a side reaction of the battery at high temperature to generate a large amount of heat until the battery fails; when the content of the first polymer microspheres is large, it is not conducive to the passage of lithium ions, resulting in local lithium precipitation at the negative electrode position, affecting the long cycle performance of the battery.
[0024] In some embodiments, in the first ceramic layer, the content of the first ceramic powder is 15wt%-60wt%, for example, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt% and 60wt%.
[0025] In some embodiments, in the first ceramic layer, the content of the first binder is 1 wt %-10 wt %.
[0026] In some embodiments, the ratio of the Dv50 particle size of the first polymer microsphere to the thickness of the first ceramic layer is (0.1-0.8):1, for example, it can be 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1 and 0.8:1. The test method for the Dv50 particle size is GB / T 15445.2-2006. When the ratio of the Dv50 particle size of the first polymer microsphere to the thickness of the first ceramic layer is (0.1-0.8):1, it is beneficial for the first polymer microsphere to melt under high temperature conditions to form multiple dense ion barrier layers, reduce the closed-cell temperature of the composite diaphragm, prevent the occurrence of further thermal runaway of the lithium-ion battery, thereby improving the safety performance of the battery, and can also enable lithium ions to be better transmitted through the composite diaphragm, inhibit lithium precipitation, and improve the long cycle performance of the battery. When the particle size of the first polymer microspheres is less than 0.1 times the thickness of the first ceramic layer, due to the small particle size of the first polymer microspheres, a dense barrier layer cannot be formed at high temperature, which causes the battery to undergo side reactions at high temperatures and generate a large amount of heat until the battery fails; when the particle size of the first polymer microspheres is greater than 0.8 times the thickness of the first ceramic layer, due to the large particle size of the polymer microspheres, lithium ions cannot be effectively transported under normal battery conditions, resulting in local lithium deposition at the negative electrode position, affecting the long cycle performance of the battery.
[0027] In some embodiments, the Dv50 particle size of the first polymer microspheres is 0.1 μm-3 μm, for example, 0.1 μm, 0.2 μm, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm and 3 μm.
[0028] In some embodiments, the thickness of the first ceramic layer is 1 μm-5 μm, for example, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm and 5 μm.
[0029] In some embodiments, the melting point of the first polymer microsphere is 80° C.-120° C., for example, it can be 80° C., 85° C., 90° C., 95° C., 100° C., 105° C., 110° C., 115° C. and 120° C., preferably 90° C.-115° C. When the melting point of the first polymer microsphere is 80° C.-120° C., it is beneficial for the first polymer microsphere to melt under high temperature conditions to form multiple dense ion barrier layers, reduce the closed-cell temperature of the composite diaphragm, and prevent the occurrence of further thermal runaway of the lithium-ion battery, thereby improving the safety performance and cycle performance of the battery. When the melting point of the first polymer microspheres is lower than 80°C, during the subsequent baking process of the battery cell, the first polymer microspheres melt at a relatively low temperature, resulting in pore blockage in the diaphragm, affecting the low-temperature discharge performance and long cycle performance of the battery; when the melting point of the first polymer microspheres is higher than 120°C, the closed-pore temperature of the composite diaphragm is high, and when the battery cell is at 120°C, a side reaction occurs between the electrolyte and the negative electrode to generate a large amount of heat, and the high closed-pore temperature cannot timely block the ion transmission between the positive and negative electrodes to effectively improve the safety performance.
[0030] In some embodiments, the thermal shrinkage of the composite membrane at 150°C is ≤5%. The thermal shrinkage test method is as follows: the composite membrane is cut into a 100mm*100mm square pattern, and marks A1 / A2 are made at intervals of 80mm in the width TD direction, and the distance between A1 and A2 is recorded as L1; then the pattern is placed in an oven at 150°C±2°C and baked for 1 hour, and after baking, the distance between A1 and A2 is measured and recorded as L2, and the thermal shrinkage of the composite membrane can be calculated, thermal shrinkage (%) = (L1-L2) / L1×100%.
[0031] In some embodiments, the molecular weight of the first polymer microspheres is 50,000-400,000, for example, 50,000, 100,000, 150,000, 200,000, 250,000, 300,000, 350,000 and 400,000, preferably 80,000-300,000.
[0032] In some embodiments, the ratio of the particle size of the first ceramic powder Dv50 to the particle size of the second ceramic powder Dv50 is 1:(0.2-0.8), for example, it can be 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7 and 1:0.8. When the ratio of the particle size of the first ceramic powder Dv50 to the particle size of the second ceramic powder Dv50 is within the above range, the heat resistance of the composite diaphragm is better (when the heat resistance of the diaphragm is good, the diaphragm is not easy to shrink and break when heated, which helps to better isolate the positive and negative electrodes), and it is beneficial to improve the transmission efficiency of lithium ions, thereby improving the safety performance and cycle performance of the battery. When the particle size of the second ceramic powder Dv50 is smaller than 0.2 times the particle size of the first ceramic powder Dv50, the pores of the second ceramic layer are too small due to the small particle size of the second ceramic powder, which is not conducive to the transmission of lithium ions and affects the low-temperature performance of the battery; when the particle size of the second ceramic powder Dv50 is larger than 0.8 times the particle size of the first ceramic powder Dv50, the particle size of the second ceramic powder Dv50 is too large, which causes the ceramic powders to be not stacked tightly enough and the heat resistance of the composite diaphragm is insufficient, resulting in poor insulation of the composite diaphragm at high temperature, leading to a short circuit between the positive and negative electrodes, and causing high-temperature failure of the battery.
[0033] In some embodiments, the ratio of the Dv50 particle size of the first polymer microspheres to the Dv50 particle size of the first ceramic powder is 1:(0.05-3), for example, it can be 1:0.05, 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.5, 1:2, 1:2.5 and 1:3.
[0034] In some embodiments, the particle size Dv50 of the first ceramic powder is 0.8-3 μm, for example, 0.8 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm and 3 μm.
[0035] In some embodiments, the second ceramic layer includes a second ceramic powder.
[0036] In some embodiments, the second ceramic layer includes a second binder.
[0037] In some embodiments, in the second ceramic layer, the content of the second ceramic powder is 80wt%-99wt%, for example, it can be 80wt%, 82wt%, 84wt%, 86wt%, 88wt%, 90wt%, 91wt%, 92wt%, 93wt%, 94wt%, 95wt%, 97wt% and 99wt%.
[0038] In some embodiments, the content of the second binder is 1 wt %-20 wt %.
[0039] In some embodiments, the particle size Dv50 of the second ceramic powder is 0.1-0.6 μm, for example, 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm and 0.6 μm.
[0040] In some embodiments, the first coating layer includes a second polymer and a third binder. The second polymer is spherical and has a melting point of 130°C-160°C.
[0041] In some embodiments, the first coating includes a thickener.
[0042] In some embodiments, in the first coating, the content of the second polymer is 85wt%-95wt%, for example, it can be 85wt%, 86wt%, 87wt%, 88wt%, 89wt%, 90wt%, 91wt%, 92wt%, 93wt%, 94wt% and 95wt%.
[0043] In some embodiments, in the first coating layer, the content of the third binder is 1 wt %-10 wt %.
[0044] In some embodiments, in the first coating layer, the thickener is present in an amount of 1 wt % to 5 wt %.
[0045] In some embodiments, the ratio of the Dv50 particle size of the first polymer microsphere to the Dv50 particle size of the second polymer is (0.25-5):1, for example, it can be 0.25:1, 0.5:1, 0.8:1, 1:1, 1.2:1, 1.5:1, 2:1, 3:1, 4:1 and 5:1. Preferably, the ratio of the Dv50 particle size of the first polymer microsphere to the Dv50 particle size of the second polymer is (0.5-1.5):1. When the ratio of the Dv50 particle size of the first polymer microsphere to the Dv50 particle size of the second polymer is (0.25-5):1, the first polymer microsphere and the first ceramic powder can form a dense barrier layer at high temperature, isolating the ion transmission between the positive and negative electrodes, reducing side reactions, and thus improving the safety performance of the battery cell. When the ratio of the Dv50 particle size of the first polymer microsphere to the Dv50 particle size of the second polymer is less than 0.25, due to the small particle size of the first polymer microsphere, a dense barrier layer cannot be formed at high temperature, which causes the battery to undergo side reactions at high temperature and generate a large amount of heat, causing the battery to fail; when the ratio of the Dv50 particle size of the first polymer microsphere to the Dv50 particle size of the second polymer is greater than 5, due to the excessively large particle size of the first polymer microsphere, lithium ions cannot be effectively transported under normal battery conditions, resulting in local lithium deposition at the negative electrode position, affecting the long cycle performance of the battery.
[0046] In some embodiments, the ratio of the Dv50 particle size of the second polymer to the thickness of the first coating is (0.1-3):1, for example, it can be 0.1:1, 0.3:1, 0.5:1, 0.8:1, 1:1, 1.2:1, 1.5:1, 2:1 and 3:1. Preferably, the ratio of the Dv50 particle size of the second polymer to the thickness of the first coating is (0.5-2):1. When the ratio of the Dv50 particle size of the second polymer to the thickness of the first coating is (0.1-3):1, it is beneficial to improve the long cycle performance and battery energy density of the battery. When the ratio of the Dv50 particle size of the second polymer to the thickness of the first coating is less than 0.1, the second polymer particles are too small, resulting in easy pore blocking of the diaphragm, affecting the long cycle performance of the battery. When the ratio of the Dv50 particle size of the second polymer to the thickness of the first coating is greater than 3, the polymer particles are too large, resulting in excessive thickness of the first coating, affecting the battery energy density.
[0047] In some embodiments, the Dv50 particle size of the second polymer is 0.1 μm-2 μm, for example, 0.1 μm, 0.5 μm, 1 μm, 1.5 μm and 2 μm.
[0048] In some embodiments, the first coating layer has a thickness of 0.5 μm-5 μm.
[0049] In some embodiments, the second coating layer includes a third polymer and a third ceramic powder. The shape of the third polymer is not specifically limited and may be spherical or non-spherical. The third ceramic powder is beneficial for further reducing the static electricity generated by the battery.
[0050] In some embodiments, in the second coating, the content of the third polymer is 20wt%-80wt%, for example, it can be 20wt%, 30wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt% and 80wt%.
[0051] In some embodiments, in the second coating, the content of the third ceramic powder is 20wt%-80wt%, for example, it can be 20wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 70wt% and 80wt%.
[0052] In some embodiments, the particle size of the third ceramic powder Dv50 is 0.5-1.5 μm, for example, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm and 1.5 μm. When the particle size of the third ceramic powder Dv50 is 0.5-1.5 μm, it is beneficial to improve the heat resistance of the diaphragm and reduce the thermal shrinkage of the diaphragm.
[0053] In some embodiments, the first polymer microspheres are selected from at least one of polyethylene, polymethacrylic acid, polymethacrylate, polypropylene and polyvinylidene fluoride.
[0054] In some embodiments, the first ceramic powder, the second ceramic powder and the third ceramic powder are each independently selected from at least one of aluminum oxide, boehmite, magnesium oxide, magnesium hydroxide, barium sulfate, barium titanate, zinc oxide, calcium oxide, silicon dioxide, silicon carbide and nickel oxide.
[0055] In some embodiments, the second polymer and the third polymer are each independently selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene modification and copolymers thereof, polyimide, polyacrylonitrile, polymethyl methacrylate and polyacrylic acid.
[0056] In some embodiments, the first binder, the second binder and the third binder are each independently selected from at least one of polymethacrylic acid, polymethyl methacrylate, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyimide, polyacrylonitrile, polymethyl acrylate, aramid resin, polyacrylic acid, styrene-butadiene rubber, polyvinyl alcohol, polyvinyl acetate, carboxymethyl cellulose, sodium carboxymethyl cellulose and carboxyethyl cellulose.
[0057] In some embodiments, the thickener is selected from at least one of carboxymethyl cellulose, sodium carboxymethyl cellulose and lithium carboxymethyl cellulose.
[0058] In some embodiments, the preparation method of the composite membrane is:
[0059] Disposing a first ceramic layer on a first surface of the substrate, and disposing a second ceramic layer on a second surface of the substrate;
[0060] A first coating layer is disposed on a side of the first ceramic layer away from the substrate, and a second coating layer is disposed on a side of the second ceramic layer away from the substrate.
[0061] A first ceramic slurry is prepared, and the first ceramic slurry is coated on a first surface of a substrate to obtain a first ceramic layer.
[0062] A second ceramic slurry is prepared, and the second ceramic slurry is coated on the second surface of the substrate to obtain a second ceramic layer.
[0063] A first coating slurry is prepared, and the first coating slurry is applied to the surface of the dried first ceramic layer to obtain a first coating.
[0064] A second coating slurry is prepared, and the second coating slurry is applied to the surface of the dried second ceramic layer to obtain a second coating.
[0065] In some embodiments, the first ceramic layer slurry includes a first ceramic powder and a first polymer microsphere.
[0066] In some embodiments, the first ceramic layer slurry further includes a first binder.
[0067] In some embodiments, the second ceramic layer slurry includes a second ceramic powder.
[0068] In some embodiments, the second ceramic layer slurry further includes a second binder.
[0069] In some embodiments, the first coating slurry includes a second polymer, an aqueous solvent, and a third binder. When the second polymer in the first coating is insoluble in the aqueous solvent, the third binder can make the second polymer and the aqueous solvent uniformly mixed, and the third binder will form a hydrophilic layer on the surface of the second polymer, so that the second polymer is uniformly dispersed in water.
[0070] In some embodiments, the first coating slurry further includes a thickener.
[0071] In some embodiments, the second coating slurry includes a third polymer, an oil-based solvent, and a third ceramic powder.
[0072] The specific materials for preparing the first ceramic layer slurry, the second ceramic layer slurry, the first coating slurry and the second coating slurry can refer to the materials contained in the aforementioned first ceramic layer, the second ceramic layer, the first coating and the second coating, which will not be described one by one here.
[0073] In some embodiments, the aqueous solvent is selected from at least one of water, methanol and ethanol. When the solvent in the first coating is an aqueous solvent, the first coating is in contact with the negative electrode active layer, and the heat generated by the high-temperature negative electrode can be transferred to the first ceramic layer in a timely manner when the negative electrode adhesion is weak. When the temperature of the first ceramic layer reaches the closed-cell temperature and above, the morphology and structure of the first polymer microspheres will change, and the first polymer microspheres will melt to form multiple continuous ion barrier layers, and the coating will form a current blockage, forming an internal blockage inside the battery to prevent further thermal runaway of the lithium-ion battery, thereby improving the safety performance of the battery.
[0074] In some embodiments, the oily solvent is selected from at least one of N,N-dimethylacetamide (DMAc), acetone, tetrahydrofuran, dichloromethane, chloroform, dimethylformamide, N-methyl-2-pyrrolidone and cyclohexane. When the binder in the second coating is an oily solvent, the coating prepared by using a polar oily solvent has good adhesion. The second coating is in contact with the positive electrode active layer, and the adhesion between the composite diaphragm and the positive electrode sheet is improved, so that the interface between the composite diaphragm and the positive electrode active layer side can be kept in a good state, and the side reaction on the positive electrode active layer side can be reduced, thereby improving the long cycle performance of the battery.
[0075] The second aspect of the present invention provides a battery, the battery comprising a positive electrode sheet, a negative electrode sheet, a composite diaphragm and an electrolyte, the composite diaphragm is the composite diaphragm described in the first aspect, the first coating of the composite diaphragm is adjacent to the negative electrode sheet, and the second coating of the composite diaphragm is adjacent to the positive electrode sheet. Figure 1 As shown, the first coating layer 31 is in contact with the negative electrode sheet 4 , and the second coating layer 32 is in contact with the positive electrode sheet 5 .
[0076] In some embodiments, the adhesion force between the first coating and the negative electrode sheet is F1, 0.2N / M≤F1≤5N / M, for example, it can be 0.2N / M, 0.4N / M, 0.6N / M, 0.8N / M, 1N / M, 1.2N / M, 1.4N / M, 1.6N / M, 1.8N / M, 2N / M, 3N / M, 4N / M and 5N / M. Preferably, the adhesion force between the first coating and the negative electrode sheet is 0.5N / M≤F1≤5N / M. Please refer to the test part for the test method of the adhesion force. When the first coating layer contacts the negative electrode sheet, the bonding force is relatively small, and the heat generated by the high-temperature negative electrode can be transferred to the first ceramic layer in a timely manner. When the temperature of the first ceramic layer reaches the closed-cell temperature or above, the morphology and structure of the first polymer microspheres will change, and they will melt to form multiple continuous ion barrier layers. The formed ion barrier layers block the current inside the battery, preventing the lithium-ion battery from further thermal runaway, thereby improving the safety performance of the battery.
[0077] In some embodiments, the bonding force between the second coating and the positive electrode sheet is F2, 5N / M≤F2≤20N / M, for example, 5N / M, 8N / M, 10N / M, 12N / M, 14N / M, 16N / M, 18N / M and 20N / M. The bonding force between the second coating and the positive electrode sheet is relatively large, which is conducive to maintaining a good interface effect of the battery, reducing the occurrence of positive electrode side reactions, and improving the safety performance of the battery.
[0078] In some embodiments, the electrolyte contains propyl propionate; preferably, the content of propyl propionate is 5wt%-30wt%, for example, 5wt%, 10wt%, 15wt%, 20wt%, 25wt% and 30wt%. When the content of propyl propionate in the electrolyte is greater than 30wt%, the safety performance of the battery deteriorates.
[0079] In the present invention, the materials of the positive electrode sheet and the negative electrode sheet are not specifically limited as long as they can meet the actual needs. The following is a schematic description.
[0080] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on one side or both sides of the positive electrode current collector, and the positive electrode active material layer includes a positive electrode active material, a conductive agent, and a binder.
[0081] In some embodiments, the positive electrode active material is selected from ternary materials, lithium iron phosphate, or ternary materials or lithium iron phosphate coated with materials containing impurity elements, and the impurities include at least two elements of Al, Mg, Mn, Cr, Ti and Zr.
[0082] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer coated on one side or both sides of the negative electrode current collector, and the negative electrode active material layer includes a negative electrode active material, a conductive agent, and a binder.
[0083] In some embodiments, the negative electrode active material is selected from graphite, SiOx / C and Si / C graphite composite materials.
[0084] In some embodiments, the electrolyte includes ethyl methyl carbonate EMC, diethyl carbonate DEC, propyl propionate PP, and ethylene carbonate EC.
[0085] In some embodiments, the content H of PP in the electrolyte and the Dv50 particle size of the first polymer satisfy 10≤100×H / D50 particle size of the first polymer≤50, for example, it can be 10, 20, 30, 40 and 50.
[0086] In some embodiments, in the electrolyte, the content of EMC is 10wt%-70wt%, the content of DEC is 10wt%-40wt%, the content of PP is 5wt%-30wt%, and the content of EC is 15wt%-40wt%.
[0087] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0088] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0089] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.
[0090] Example 1
[0091] (1) Preparation of composite diaphragm
[0092] The first polymer microspheres prepared from polyethylene, the first ceramic powder alumina and the first binder polymethacrylic acid were prepared in a ratio of 50:45:5, which was recorded as solution A; the second ceramic powder alumina and the second binder polymethyl methacrylate were prepared in a ratio of 95:5, which was recorded as solution B; the second polymer polyvinylidene fluoride-hexafluoropropylene, the third binder polymethyl methacrylate, and the thickener sodium carboxymethyl cellulose were dissolved in water in a ratio of 93:5:2, which was recorded as solution C; the third polymer polyvinylidene fluoride-hexafluoropropylene copolymer and the third ceramic powder were dissolved in DMAc in a ratio of 40:60, which was recorded as solution D;
[0093] Solution A was coated on one side of a polyethylene substrate (PE substrate) with a thickness of 7 μm by using a gravure roller, and after drying, a diaphragm with a first ceramic layer of 2 μm was obtained, which was recorded as diaphragm E, and the content of the first polymer microspheres in the first ceramic layer was 50 wt%; Solution B was coated on the other side of the substrate by using a gravure roller, and after drying, a diaphragm with a first ceramic layer of 2 μm and a second ceramic layer of 2 μm was obtained, which was recorded as diaphragm F;
[0094] Solution D was coated on the second ceramic layer of diaphragm F by gravure roller coating, and after water drying, a diaphragm having a first ceramic layer of 2 μm, a second ceramic layer of 2 μm, and a second coating layer of 1 μm was obtained, which was recorded as diaphragm G;
[0095] The solution C is coated on the first ceramic layer of the diaphragm G by using a gravure roller, and after drying, a diaphragm having a first ceramic layer of 2 μm, a first coating layer of 1 μm, a second ceramic layer of 2 μm, and a second coating layer of 1 μm is obtained to obtain a diaphragm H;
[0096] Wherein: the first polymer type, the first polymer ratio, the first polymer melting point, the first ceramic powder Dv50 particle size, and the second ceramic powder Dv50 particle size in the ceramic layer are detailed in Table 1 and Table 2.
[0097] Wherein: the second polymer type in the coating, the first coating solvent, the third polymer type, and the second coating solvent are detailed in Table 1 and Table 2.
[0098] (2) Preparation of positive electrode
[0099] The positive electrode active material lithium iron phosphate (LFP), the binder polyvinylidene fluoride (PVDF), and the conductive agent acetylene black are mixed in a weight ratio of 97:1:2, and N-methylpyrrolidone (NMP) is added, and stirred under the action of a vacuum mixer until the mixed system becomes a positive electrode slurry with uniform fluidity; the positive electrode slurry is evenly coated on an aluminum foil with a thickness of 10 μm; the coated aluminum foil is baked in an oven with 5 different temperature gradients, and then dried in an oven at 120°C for 8 hours, and then rolled and cut to obtain the required positive electrode sheet.
[0100] (3) Negative electrode preparation
[0101] 96% by weight of artificial graphite negative electrode material, 0.2% by weight of single-walled carbon nanotube (SWCNT) conductive agent, 1% by weight of conductive carbon black (SP) conductive agent, 1% by weight of sodium carboxymethyl cellulose (CMC) binder and 1.8% by weight of styrene-butadiene rubber (SBR) binder were made into slurry by a wet process, coated on the surface of the negative electrode current collector copper foil, and dried (temperature: 85°C, time: 5h), rolled and die-cut to obtain the negative electrode sheet.
[0102] (4) Preparation of non-aqueous electrolyte
[0103] In a glove box filled with argon (water <10ppm, oxygen <1ppm), ethylene carbonate (EC), propylene carbonate (PC), and propyl propionate (PP) were mixed at a mass ratio of 2:1.5:2 to obtain a mixed solution 1, 10wt% of EP was added to the mixed solution 1 to obtain a mixed solution 2, and 14% of LiPF6 based on the total mass of the non-aqueous electrolyte was slowly added to the mixed solution 2, and the non-aqueous electrolyte was obtained by stirring. The EP content in the electrolyte is shown in Table 2.
[0104] The specific different characteristics of Example 1 group to Example 10 group are shown in Table 1.
[0105] Example 2 group: refer to Example 1, except that the ratio of Dv50 of the first polymer microspheres to the thickness of the first ceramic layer is different.
[0106] Example 3 group: refer to Example 1, except that the melting point of the first polymer microsphere is different.
[0107] Example 4 group: refer to Example 1, except that the content of the first polymer microspheres is different.
[0108] Example 5 group: refer to Example 1, except that the ratio of the Dv50 particle size of the first ceramic powder and the second ceramic powder is different.
[0109] Example 6 group: refer to Example 1, except that the first polymer microspheres are selected differently.
[0110] Example 6-1: The first polymer microsphere is polymethacrylic acid.
[0111] Example 6-2: The first polymer microsphere is polyvinylidene fluoride-hexafluoropropylene copolymer.
[0112] Example 7 group: refer to Example 1, except that the solvents for the first coating and the second coating are different.
[0113] Example 7-1 was carried out according to the method of Example 1, except that the solvent of solution C was DMAc.
[0114] Example 7-2 is carried out according to the method of Example 1, except that the solvent of solution D is water.
[0115] Example 8: The method was carried out in accordance with Example 1, except that the ratio of the Dv50 of the second polymer to the thickness of the first coating layer was different.
[0116] Example 9: The method was carried out in accordance with Example 1, except that the content of the third polymer in the third coating layer was different.
[0117] Example 10 group: refer to Example 1, except that the PP content in the electrolyte is different.
[0118] Comparative Example 1: The method is carried out in accordance with Example 1, except that neither the first ceramic layer nor the second ceramic layer contains the first polymer microspheres, but only contains ceramic powder.
[0119] Comparative Example 2: The method is carried out in accordance with Example 1, except that both the first ceramic layer and the second ceramic layer contain first polymer microspheres.
[0120] Comparative Example 3: The method is carried out with reference to Example 1, except that the first ceramic layer does not contain the first polymer microspheres, and the second ceramic layer contains the first polymer microspheres.
[0121] Table 1
[0122]
[0123] Table 2
[0124]
[0125] The electrochemical performance of the batteries obtained in the above comparative examples and embodiments was tested. The test data are shown in Table 3. The relevant descriptions are as follows:
[0126] (1) 25℃ cycle test: The batteries obtained in the above embodiments and comparative examples were placed in a (25±2)℃ environment and left to stand for 2-3 hours. When the battery body reached (25±2)℃, the battery was charged at a constant current of 3C until the cut-off current was 0.05C. After the battery was fully charged, it was left for 5 minutes and then discharged at a constant current of 3C until the cut-off voltage was 3.0V. The highest discharge capacity of the first three cycles was recorded as the initial capacity Q. When the cycle reached 1000 times, the last discharge capacity Q of the battery was recorded. The recorded results are shown in Table 3. The calculation formula used is as follows: Capacity retention rate (%) = Q1 / Q×100%.
[0127] (2) Room-temperature capacity retention rate and low-temperature capacity retention rate: The batteries obtained in the above embodiments and comparative examples were first discharged at 0.2C to 3.0V at an ambient temperature of (25±3)°C and left for 5 min. They were then charged at 0.7C. When the battery terminal voltage reached the charge limit voltage, constant voltage charging was performed until the charging current ≤ the cutoff current. Charging was stopped and left for 5 min. The batteries were then discharged at 0.2C to 3.0V. The discharge capacity was recorded as the room-temperature capacity Q4.
[0128] Then the battery is charged at 0.7C. When the battery terminal voltage reaches the charging limit voltage, it is changed to constant voltage charging until the charging current is less than or equal to the cut-off current, and the charging is stopped; the fully charged battery is placed at (-20±2)℃ for 4h, and then discharged at 0.25C current to the cut-off voltage of 3.0V, and the discharge capacity Q5 is recorded. The low-temperature discharge capacity retention rate can be calculated, and the recorded results are shown in Table 3. The calculation formula used is as follows: Low-temperature discharge capacity retention rate (%) = Q5 / Q4×100%.
[0129] (3) Thermal shrinkage test method: Cut the composite diaphragm into 100mm*100mm square patterns, mark A1 / A2 at intervals of 80mm in the width TD direction, and the distance between A1 and A2 is recorded as L1; then place the pattern in an oven at 150℃±2℃ and bake for 1 hour. After baking, measure the distance between A1 and A2 and record it as L2. The thermal shrinkage of the composite diaphragm can be calculated. The results are recorded as shown in Table 3, where the calculation formula used is as follows: Thermal shrinkage (%) = (L1-L2) / L1×100%. Thermal shrinkage is used to indicate the heat resistance of the battery.
[0130] (4) Method for measuring the adhesion between the first coating and the negative electrode sheet: The batteries obtained in the above embodiments and comparative examples are placed in an environment of (25±2)°C and left to stand for 2-3 hours. When the battery body reaches (25±2)°C, the battery is charged at a constant current of 0.7C with a cut-off current of 0.05C. When the battery terminal voltage reaches the charging limit voltage, constant voltage charging is performed until the charging current ≤ the cut-off current. Charging is stopped and left for 5 minutes. The fully charged battery is dissected. A composite diaphragm and a negative electrode integral sample with a length of 30 mm and a width of 15 mm is selected along the direction of the ear. The composite diaphragm and the negative electrode are tested at an angle of 180 degrees on a universal stretching machine at a speed of 100 mm / min and a test displacement of 50 mm. The test result is recorded as the adhesion between the composite diaphragm and the negative electrode N (unit: N / m).
[0131] (5) Method for measuring the adhesion between the second coating and the positive electrode sheet: The batteries obtained in the above embodiments and comparative examples are placed in an environment of (25±2)°C and left to stand for 2-3 hours. When the battery body reaches (25±2)°C, the battery is charged at a constant current of 0.7C with a cut-off current of 0.05C. When the battery terminal voltage reaches the charging limit voltage, constant voltage charging is performed until the charging current ≤ the cut-off current. Charging is stopped and left for 5 minutes. The fully charged battery is dissected, and a composite diaphragm and a positive electrode integral sample with a length of 30mm*width of 15mm is selected along the direction of the pole ear. The composite diaphragm and the negative electrode are tested at an angle of 180 degrees on a universal stretching machine at a speed of 100mm / min and a test displacement of 50mm. The test result is recorded as the adhesion between the composite diaphragm and the positive electrode sheet N (unit: N / m).
[0132] (6) 150°C thermal shock test (150°C 1H furnace temperature test): The batteries obtained in the above examples and comparative examples were heated by convection or circulating hot air oven at a starting temperature of (25±3)°C, a temperature change rate of (5±2)°C / min, and the temperature was raised to (150±2)°C. The test was terminated after maintaining for 1h, and the battery status results were recorded as shown in Table 3. The test result A / B means that the total number of tests was B times, and the number of times the test was passed was A times. The 150°C thermal shock test is used to illustrate the safety performance of the battery.
[0133] (7) Air permeability of the diaphragm after baking at 130°C for 1 min: Refer to the test method for air permeability of the diaphragm in 3.2 of the national standard G / B 363-2018. The air permeability of the diaphragm after baking at 130°C for 1 min is used to illustrate the furnace temperature performance of the battery.
[0134] Table 3
[0135]
[0136]
[0137] The composite diaphragm of the present invention is provided with a first ceramic layer and a second ceramic layer on both sides of the substrate, so that the first ceramic layer contains first polymer microspheres and the second ceramic layer does not contain polymers. The first polymer microspheres in the first ceramic layer can be melted under high temperature conditions to form multiple continuous ion barrier layers, thereby reducing the closed-pore temperature of the composite diaphragm and preventing further thermal runaway of the lithium-ion battery, thereby improving the safety performance of the battery; the second ceramic layer does not contain polymers, so that the ceramic particles in the second ceramic layer can be in close contact, which is beneficial to improving the heat resistance of the composite diaphragm. By designing the particle size of the first ceramic particles and the particle size and temperature of the first polymer microspheres, the first ceramic layer can achieve the effect of rapid closed pores; by controlling the first ceramic and the second ceramic particles, it is ensured that the composite diaphragm maintains excellent permeability and heat resistance.
[0138] Furthermore, the first ceramic layer of the composite diaphragm corresponds to the negative electrode end in the battery, and the second ceramic layer of the composite diaphragm corresponds to the positive electrode end in the battery, which is beneficial for the timely transfer of heat energy to the first ceramic layer when the battery is in thermal runaway, so that the first polymer microspheres in the first ceramic layer can be melted in time, thereby helping to reduce the closed-cell temperature of the composite diaphragm, prevent the occurrence of further thermal runaway of the lithium-ion battery, and improve the safety performance of the battery.
[0139] Furthermore, a first coating is provided on the side of the first ceramic layer away from the substrate, and a second coating is provided on the side of the second ceramic layer away from the substrate. By controlling the adhesion of the first coating and the second coating, the good interface of the battery cell is ensured while reducing damage to the negative electrode active layer. The first coating and the second coating can provide good adhesion between the composite diaphragm and the positive and negative electrode sheets, preventing the positive electrode active layer and the negative electrode active layer from falling off. The first coating contains an aqueous solvent. Under aqueous solvent conditions, the adhesion of the first coating is poor. The second coating contains an oily solvent. Under oily solvent conditions, the second coating has good adhesion. The first coating is in contact with the negative electrode sheet, and the second coating is in contact with the positive electrode sheet. The adhesion between the first coating and the negative electrode sheet is small, which is beneficial when thermal runaway occurs in the battery. The heat at the negative end can be transferred to the first ceramic layer through the first coating in time, thereby avoiding further thermal runaway, and also helping to reduce damage to the negative electrode active layer. There is a strong adhesion between the second coating and the positive electrode sheet, which can keep the interface between the composite separator and the positive electrode sheet in a good state, reduce side reactions on the positive electrode side, and thus improve the long cycle performance of the battery.
[0140] Furthermore, by controlling the particle size Dv50 of the first polymer microspheres and the content of PP in the electrolyte, the prepared battery can take both low temperature performance and safety performance into consideration.
[0141] The solution of the present invention reasonably designs the ceramic layer and coating in the battery composite diaphragm, and the composite diaphragm prepared can effectively improve the safety performance of the battery while taking into account the low-temperature performance of the battery, and at the same time has excellent long-cycle performance.
[0142] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.
[0143] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A composite diaphragm, characterized in that: The composite diaphragm comprises a substrate, wherein along the thickness direction of the substrate, the substrate has a first surface and a second surface which are arranged opposite to each other, a first ceramic layer is arranged on the first surface of the substrate, and a second ceramic layer is arranged on the second surface of the substrate; a first coating is arranged on a side of the first ceramic layer away from the substrate, and a second coating is arranged on a side of the second ceramic layer away from the substrate; The first ceramic layer includes first ceramic powder and first polymer microspheres, and the second ceramic layer includes second ceramic powder.
2. The composite diaphragm according to claim 1, characterized in that: The ratio of the Dv50 particle size of the first polymer microsphere to the Dv50 particle size of the first ceramic powder is 1:(0.05-3); and / or, The ratio of the Dv50 particle size of the first polymer microsphere to the thickness of the first ceramic layer is (0.1-0.8):1; and / or, The Dv50 particle size of the first polymer microsphere is 0.1 μm-3 μm; and / or, The thickness of the first ceramic layer is 1 μm-5 μm; and / or, In the first ceramic layer, the content of the first polymer microspheres is 30wt%-80wt%.
3. The composite diaphragm according to claim 1 or 2, characterized in that: The melting point of the first polymer microsphere is 80°C-120°C, preferably 90°C-115°C; and / or, The molecular weight of the first polymer microspheres is 50,000-400,000, preferably 80,000-300,000.
4. The composite diaphragm according to claim 1, characterized in that: The ratio of the particle size Dv50 of the first ceramic powder to the particle size Dv50 of the second ceramic powder is 1:(0.2-0.8); and / or, The first ceramic powder has a particle size Dv50 of 0.8-3 μm; and / or, The second ceramic powder has a Dv50 particle size of 0.1-0.6 μm.
5. The composite diaphragm according to claim 1, characterized in that: The first coating comprises a second polymer and a third binder; and / or, The second coating layer includes a third polymer and a third ceramic powder; and / or, the first ceramic layer further includes a first binder; and / or, The second ceramic layer also includes a second binder.
6. The composite diaphragm according to claim 5, characterized in that: The ratio of the Dv50 particle size of the first polymer microsphere to the Dv50 particle size of the second polymer is (0.25-5):1; and / or, The ratio of the Dv50 particle size of the second polymer to the thickness of the first coating is (0.1-3):1; and / or, The Dv50 particle size of the second polymer is 0.1 μm-2 μm; and / or, The third ceramic powder has a particle size Dv50 of 0.5-1.5 μm.
7. The composite diaphragm according to any one of claims 1 to 6, characterized in that: The first polymer microspheres are selected from at least one of polyethylene, polymethacrylic acid, polymethacrylate, polypropylene and polyvinylidene fluoride; and / or, The first ceramic powder, the second ceramic powder and the third ceramic powder are each independently selected from at least one of aluminum oxide, boehmite, magnesium oxide, magnesium hydroxide, barium sulfate, barium titanate, zinc oxide, calcium oxide, silicon dioxide, silicon carbide and nickel oxide; and / or, The second polymer and the third polymer are each independently selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene modification and copolymers thereof, polyimide, polyacrylonitrile, polymethyl methacrylate and polyacrylic acid.
8. The composite diaphragm according to any one of claims 5 to 7, characterized in that: The first binder, the second binder and the third binder are each independently selected from at least one of polymethacrylic acid, polymethyl methacrylate, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyimide, polyacrylonitrile, polymethyl acrylate, aramid resin, polyacrylic acid, styrene-butadiene rubber, polyvinyl alcohol, polyvinyl acetate, carboxymethyl cellulose, sodium carboxymethyl cellulose and carboxyethyl cellulose.
9. A battery, characterized in that: The battery comprises a positive electrode sheet, a negative electrode sheet, a composite diaphragm and an electrolyte, wherein the composite diaphragm is the composite diaphragm according to any one of claims 1 to 8, wherein the first coating of the composite diaphragm is adjacent to the negative electrode sheet, and the second coating of the composite diaphragm is adjacent to the positive electrode sheet.
10. The battery according to claim 9, wherein The bonding force between the first coating and the negative electrode sheet is F1, 0.2N / M≤F1≤5N / M; and / or, The bonding force between the second coating and the positive electrode sheet is F2, 5N / M≤F2≤20N / M; and / or, The electrolyte contains propyl propionate; preferably, the content of propyl propionate is 5wt%-30wt%.
Citation Information
Patent Citations
Lithium ion battery composite diaphragm and preparation method and application thereof
CN104157811A
Composite diaphragm as well as preparation method and application thereof
CN113178663A
Diaphragm and battery containing diaphragm
CN114006024A
Battery
CN114024035A
Composite diaphragm and lithium ion battery containing same
CN116053707A