Method for realizing integration of perovskite single crystal and CMOS (Complementary Metal-Oxide-Semiconductor Transistor) by using ionic liquid as connecting layer
By reacting with perovskite single crystals as a connecting layer, the integration of perovskite single crystals and CMOS substrates is achieved, solving the high-temperature instability and cumbersome steps of the integration of perovskite single crystals and CMOS, and improving X-ray The sensitivity and stability of the detector are suitable for commercial applications.
Patent Information
- Application Number
- CN202411007181.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
AI Technical Summary
The high temperature instability of perovskite single crystals and CMOS substrates leads to the damage of the crystals or substrates in the traditional flip welding method, limiting its application in commercial equipment, and the existing ionic liquid methods are complicated and inconvenient, limiting the perovskite single Commercial application of crystal integration with CMOS.
Using ionic liquid as the connecting layer, the ionic liquid is converted into liquid through hygroscopic action and reacts with perovskite single crystals to form a new interface layer, achieving strong adhesion between perovskite single crystals and CMOS substrate, avoiding high temperature damage and Simplify the steps.
It improves the sensitivity and stability of the X-ray detector, provides good mechanical and electrical performance, is suitable for commercial applications, and extends to other halide perovskite materials, achieving the integrated manufacturing of high-performance X-ray detectors.
Smart Images

Figure CN118922035A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of X-ray detector integrated manufacturing, and relates to a method for realizing the integration of a perovskite single crystal and a CMOS by using an ionic liquid as a connecting layer. Background Art
[0002] X-ray detection technology plays a key supporting role in medical diagnosis, industrial flaw detection, safety monitoring and other fields. However, due to the potential damage of X-rays to human cells, high-dose exposure will increase the risk of cancer. Emerging perovskite single crystal detectors are expected to achieve highly sensitive X-ray detection and reduce the X-ray working dose, thereby reducing the risks for doctors and patients in clinical practice. For example, reducing the X-ray working dose can extend the safe time of X-ray imaging, which is very critical for imaging in some key scenarios, such as guiding interventional surgery.
[0003] The practical application of perovskite single crystal X-ray imaging relies on the integration of perovskite single crystals with large-area CMOS chips. However, due to the instability of perovskite single crystals and CMOS chip substrates at high temperatures, the traditional "flip-chip" method will cause damage to the perovskite crystals or the substrate, and is not suitable for the integration of perovskite crystals with CMOS / TFT circuits, limiting its application in commercial devices.
[0004] Ionic liquids refer to salts that are liquid at room temperature or close to room temperature and are composed entirely of anions and cations. They are generally composed of organic cations and inorganic or organic anions. They are a new generation of electrolyte materials and are environmentally friendly. Therefore, they are widely used in the optoelectronic field.
[0005] Reference 1 discloses a method of preparing an X-ray detector by soaking MAPbI3 single crystals in ionic liquids. The photoelectric performance of the detector is significantly improved. However, this method requires power to be applied during soaking, and the soaked single crystal must be further combined with a substrate, which results in cumbersome steps and inconvenient operation, limiting its commercial application.
[0006] Reference 2 discloses a method for integrating a perovskite single crystal and an ITO substrate using an ionic liquid. The X-ray detector prepared using the perovskite single crystal and the ITO substrate obtained by the method has excellent stability and sensitivity. An ITO substrate generally refers to a substrate constructed on an ITO (Indium Tin Oxide) film. ITO is a transparent conductive material widely used in the fields of electronics and optoelectronics, especially in the fields of thin-film solar cells, touch screen technology, and OLED display technology.
[0007] CMOS, the full name of which is Complementary Metal-Oxide-Semiconductor, is an important chip inside a computer system. The manufacturing technology of CMOS chips is similar to that of general computer chips. It mainly uses semiconductors made of silicon and germanium, which allow semiconductors with N (negatively charged) and P (positively charged) levels to coexist on CMOS. The current generated by these two complementary effects can be recorded and interpreted into images by the processing chip. CMOS not only plays a key role in computer systems, but also plays an important role in digital photography as an image sensor.
[0008] The surface of CMOS chip is mainly made of silicon and other metal materials. When integrated with perovskite single crystal as a substrate, on the one hand, it will show completely different material properties. On the other hand, due to the manufacturing process and packaging design, CMOS often has a complex surface structure, rather than the completely flat surface of ITO substrate. Therefore, the method of integrating perovskite single crystal with ITO cannot be taken for granted that it is also applicable to the integration of perovskite single crystal with CMOS.
[0009] Reference 1: CN117858586A;
[0010] Cited literature 2: Min Kyu Kim, et al. Integration of Large-Area HalidePerovskite Single Crystals and Substrates via Chemical Welding Using an IonicLiquid for Applications in X-ray Detection[J]. ACS Applied Materials AndInterfaces, 2023, 15(49): 57404-57414. Summary of the invention
[0011] Problem that the invention aims to solve
[0012] In view of the above problems, the present invention aims to provide a method for integrating perovskite single crystal with CMOS using ionic liquid as a connecting layer. The method can achieve strong bonding of large-area halide perovskite single crystal with CMOS substrate through chemical reaction, improve the sensitivity and stability of X-ray detectors, and provide a new solution for the integrated manufacturing of high-performance X-ray detectors based on CMOS.
[0013] Solutions for solving problems
[0014] [1] A method for integrating a perovskite single crystal with a CMOS using an ionic liquid as a connecting layer, comprising the following steps:
[0015] (1) Placing ionic liquid powder on a CMOS substrate, the ionic liquid is transformed into a liquid state through moisture absorption;
[0016] (2) placing a perovskite single crystal on a liquid ionic liquid and allowing it to stand;
[0017] (3) The ionic liquid reacts with the surface of the perovskite single crystal to form a new interface layer, thus realizing the integration of the perovskite single crystal and CMOS.
[0018] [2] The method according to [1], wherein the ionic liquid is methylammonium acetate or methylammonium formate.
[0019] [3] The method according to [1] or [2], wherein the perovskite single crystal is a halide perovskite single crystal.
[0020] [4] The method according to any one of [1] to [3], wherein the perovskite single crystal is MAPbX3, MASnX3 or MAGeX3 single crystal, wherein X is any one of Cl, Br, I or a combination of two or more thereof; preferably, the perovskite single crystal is MAPbBr3 single crystal.
[0021] [5] The method according to any one of [1] to [4], wherein the ionic liquid in step (1) is converted into a liquid state at room temperature.
[0022] [6] The method according to any one of [1] to [5], wherein the ionic liquid in step (1) is converted into a liquid at a humidity of 30 RH% to 60 RH%.
[0023] [7] The method according to any one of [1] to [6], wherein the perovskite single crystal in step (2) is obtained by a temperature inversion crystallization method.
[0024] [8] The method according to any one of [1] to [7], wherein step (2) is carried out at room temperature without applying external pressure.
[0025] [9] An X-ray detector comprising a perovskite single crystal and a CMOS substrate integrated by the method described in any one of [1]-[8].
[0026]
[10] Use of ionic liquid for integrating perovskite single crystal with CMOS substrate, wherein the ionic liquid is used as a connecting layer to realize the integration of perovskite single crystal with CMOS substrate; preferably, the ionic liquid is methylammonium acetate or methylammonium formate.
[0027] Effects of the Invention
[0028] The present invention has the following excellent technical effects:
[0029] 1. The present invention realizes the heterogeneous integration of large-area halide perovskite single crystals and CMOS substrates, improving the sensitivity and stability of X-ray detectors;
[0030] 2. The method of the present invention uses ionic liquid as a connecting layer, provides good mechanical and electrical properties, and ensures the long-term stability of the interface;
[0031] 3. The room temperature processing process in the present invention avoids the potential damage of high temperature to the CMOS substrate and the perovskite single crystal, which is beneficial to the compatibility with the integrated circuit;
[0032] 4. The method of the present invention has simple steps, is easy to operate, and is very suitable for commercial applications;
[0033] 5. The method of the present invention can be extended to other types of halide perovskite materials, providing the possibility for the commercialization of high-performance X-ray detectors. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a test diagram of the bonding strength of the X-ray detector in an embodiment of the present invention. DETAILED DESCRIPTION
[0035] Various exemplary embodiments, features and aspects of the present invention will be described in detail below. The word "exemplary" used here means "used as an example, embodiment or illustrative". Any embodiment described here as "exemplary" is not necessarily interpreted as being superior or better than other embodiments.
[0036] In addition, in order to better illustrate the present invention, numerous specific details are provided in the following specific embodiments. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In other examples, methods, means, equipment and steps well known to those skilled in the art are not described in detail in order to highlight the subject matter of the present invention.
[0037] Unless otherwise stated, the units used in this specification are all international standard units, and the numerical values and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.
[0038] In this specification, the word "may" means both performing a certain process and not performing a certain process.
[0039] In this specification, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.
[0040] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values A and B.
[0041] In the present specification, when "normal temperature" or "room temperature" is used, the temperature may be 15°C to 30°C, further 15°C to 25°C, for example, 20°C.
[0042] The present invention realizes the effective integration of large-area halide perovskite single crystal and CMOS substrate by using ionic liquid as a connecting layer, and provides a novel solution for the manufacture of high-performance X-ray detectors. Specifically, the present invention provides a method for integrating perovskite single crystal with CMOS using ionic liquid as a connecting layer, which comprises the following steps:
[0043] (1) Placing ionic liquid powder on a CMOS substrate, the ionic liquid is transformed into a liquid state through moisture absorption;
[0044] (2) placing a perovskite single crystal on a liquid ionic liquid and leaving it there;
[0045] (3) The ionic liquid reacts with the surface of the perovskite single crystal to form a new interface layer, thus realizing the integration of the perovskite single crystal and CMOS.
[0046] In some specific embodiments, the ionic liquid is methylammonium acetate or methylammonium formate.
[0047] In the present invention, methylammonium acetate, also known as methylammonium acetate or methylammonium acetate, referred to as MAAc in English, with a CAS number of 6998-30-7, is a salt obtained by the reaction of acetic acid and methylamine.
[0048] In some specific embodiments, the perovskite single crystal is a halide perovskite single crystal.
[0049] In some preferred embodiments, the perovskite single crystal is MAPbX3, MASnX3 or MAGeX3 single crystal, wherein X is any one or a combination of two or more of Cl, Br, and I. For example, the perovskite single crystal is MAPbBr3 single crystal, MASnBr3 single crystal, MAGeBr3 single crystal or MAPbBrI2 single crystal, etc.
[0050] In some more preferred embodiments, the perovskite single crystal is MAPbBr3 single crystal.
[0051] In some specific embodiments, the ionic liquid in step (1) is converted into a liquid state at room temperature.
[0052] In some specific embodiments, the ionic liquid in step (1) is converted into a liquid state at a humidity of 30 RH%-60 RH%.
[0053] In some specific embodiments, the perovskite single crystal in step (2) is obtained by inversion crystallization. For example, a large-area halide perovskite single crystal is prepared by inversion crystallization, and the crystal surface is polished and smoothed before being used in step (2).
[0054] In some specific embodiments, step (2) is performed at room temperature without external pressure.
[0055] In some specific embodiments, the placement time in step (2) is more than 24 hours, for example, 24, 30, 36, 48 hours, etc.
[0056] In the present invention, the ionic liquid reacts with the surface of the perovskite single crystal to form a new interface layer, which can achieve strong adhesion between the two. The interface layer is characterized by scanning electron microscopy and X-ray photoelectron spectroscopy, confirming that a stable chemical bond is formed between the two, and the ionic liquid reacts with the perovskite single crystal, that is, the perovskite single crystal is fixed on the CMOS substrate by chemical welding, thereby showing stable mechanical properties.
[0057] The present invention also provides an X-ray detector, comprising the perovskite single crystal and a CMOS substrate integrated by the above method. The CMOS-based X-ray detector exhibits high performance, specifically excellent sensitivity and stability.
[0058] In some specific embodiments, the sensitivity of the X-ray detector can reach 90000 μC Gy air -1 cm -2 Above, for example, 91000, 92000, 95000, 98000, 1×10 5 , 1.2×10 5 , 1.5×10 5 , 2×10 5 μC Gy air -1 cm -2 wait.
[0059] In some specific embodiments, the bonding strength of the X-ray detector can reach above 1 MPa, for example, 1, 3, 5, 8, 10, 15, 20 MPa, etc.
[0060] In addition, the present invention also provides the use of ionic liquid for integrating perovskite single crystal with CMOS substrate, wherein the ionic liquid is used as a connecting layer to realize the integration of perovskite single crystal with CMOS substrate.
[0061] In some specific embodiments, the ionic liquid is methylammonium acetate or methylammonium formate.
[0062] In some specific embodiments, the method of integrating a perovskite single crystal with a CMOS substrate using the ionic liquid as a connecting layer is as described above.
[0063] In a specific embodiment, the present invention provides detailed experimental steps and conditions, including the growth method of halide perovskite single crystals, the selection and treatment of ionic liquids, the optimization of the bonding process, and the characterization of the interface layer, etc. Through experimental verification, the excellent performance of this method in X-ray detector integration is demonstrated.
[0064] Example
[0065] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0066] This example describes a method of using ionic liquid methylammonium acetate (MAAc) as a connecting layer to form a 20 cm 2 A method for integrating MAPbBr3 single crystals with CMOS substrates. First, under a controlled dry environment, MAAc powder is placed on a CMOS substrate, and then placed in a natural environment (temperature of 25°C and humidity of 40%) to transform into a liquid state through natural moisture absorption. Subsequently, a MAPbBr3 single crystal pre-grown using a cooling crystallization method is placed on liquid MAAc, and the single crystal naturally adheres to the substrate without external pressure. After keeping at room temperature for 24 hours, MAAc reacts with the surface of the single crystal to form a new interface layer, thereby achieving strong adhesion between the two. The interface layer was characterized by scanning electron microscopy (SEM) and X-ray photoelectron spectroscopy (XPS), confirming the formation of a stable chemical bond between MAAc and MAPbBr3.
[0067] Finally, the integrated structure exhibited stable mechanical properties and excellent X-ray detection performance. The X-ray detector made using the integrated structure had an adhesion strength of up to 10 MPa and a 5 μC Gy air -1 cm -2 sensitivity. Figure 1 This is the bonding strength test chart of the X-ray detector. The bonding strength corresponding to the inflection point is (5g*9.8N / kg) / (70μm*70μm)=10MPa, where 5g is the vertical coordinate corresponding to the inflection point, indicating that the critical stress is 5g, and 70μm*70μm represents the area of each pixel.
[0068] It should be noted that, although the technical solution of the present invention is introduced with specific examples, those skilled in the art will appreciate that the present invention should not be limited thereto.
[0069] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.
Claims
1. A method for integrating a perovskite single crystal with a CMOS using an ionic liquid as a connecting layer, comprising the following steps: (1) Placing ionic liquid powder on a CMOS substrate, the ionic liquid is transformed into a liquid state through moisture absorption; (2) placing a perovskite single crystal on a liquid ionic liquid and allowing it to stand; (3) The ionic liquid reacts with the surface of the perovskite single crystal to form a new interface layer, thus realizing the integration of the perovskite single crystal and CMOS.
2. The method according to claim 1, characterized in that The ionic liquid is methylammonium acetate or methylammonium formate.
3. The method according to claim 1 or 2, characterized in that: The perovskite single crystal is a halide perovskite single crystal.
4. The method according to any one of claims 1 to 3, characterized in that: The perovskite single crystal is MAPbX3, MASnX3 or MAGeX3 single crystal, wherein X is any one of Cl, Br, I or a combination of two or more thereof; preferably, the perovskite single crystal is MAPbBr3 single crystal.
5. The method according to any one of claims 1 to 4, characterized in that: The ionic liquid in step (1) is converted into a liquid state at room temperature.
6. The method according to any one of claims 1 to 5, characterized in that: The ionic liquid in step (1) is converted into a liquid state at a humidity of 30 RH%-60 RH%.
7. The method according to any one of claims 1 to 6, characterized in that: The perovskite single crystal in step (2) is obtained by a temperature inversion crystallization method.
8. The method according to any one of claims 1 to 7, characterized in that: Step (2) is carried out at room temperature without applying external pressure.
9. An X-ray detector, comprising a perovskite single crystal and a CMOS substrate integrated by the method according to any one of claims 1 to 8.
10. Use of ionic liquids for integrating perovskite single crystals with CMOS substrates, wherein: The ionic liquid is used as a connecting layer to realize the integration of the perovskite single crystal and the CMOS substrate; preferably, the ionic liquid is methylammonium acetate or methylammonium formate.
Citation Information
Patent Citations
Preparation method of X-ray detector with MAPbI3 single crystal as core
CN117858586A