Anti-ferroelectric neuromorphic device and preparation method thereof

By forming a hafnium zirconium oxide film on the substrate and building a built-in field using metal layers with different work functions, the complexity and nonvolatile problems of antiferroelectric neuromorphic devices are solved, and high-performance synapses are achieved Morphological functions meet the needs of emerging synaptic devices.

CN118922058APending Publication Date: 2024-11-08FUDAN UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410974708.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing antiferroelectric neuromorphic devices are complex in preparation, resulting in high production costs and the inability to achieve nonvolatile storage and synaptic morphological characteristics, limiting their application in the field of neuromorphic computing.

Method used

Using a preparation method, including forming a hafnium zirconium oxide film on the substrate and crystallizing it through rapid heat treatment to produce antiferroelectricity, combining first and second metal layers with different work functions, building a built-in field to change The polarization properties of the material achieve nonvolatile and synaptic morphological functions.

Benefits of technology

Reduces production costs, simplifies the process, realizes the preparation of high-performance antiferroelectric neuromorphic devices, meets the needs of emerging synaptic devices, and maintains polarization state after the external electric field is removed, achieving paired pulse promotion and excitability Synaptic morphological characteristics and functions such as postsynaptic current and long-term enhancement/inhibition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922058A_ABST
    Figure CN118922058A_ABST
Patent Text Reader

Abstract

The invention provides an anti-ferroelectric neuromorphic device and a preparation method thereof. The preparation method comprises the following steps: providing a substrate; generating a first metal layer on the substrate as a first electrode; forming a hafnium zirconium oxide thin film on the first metal layer; and forming a second metal layer on the hafnium zirconium oxide thin film. The hafnium zirconium oxide antiferroelectric material has the beneficial effects that the non-volatility of the hafnium zirconium oxide antiferroelectric material is realized, and on the basis of the non-volatility, the neural synaptic morphological characteristics and functions including pulse promotion, excitatory post-synaptic current and long-term enhancement / inhibition can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor manufacturing technology, and in particular to an antiferroelectric neuromorphic device and a preparation method thereof. Background Art

[0002] For building neural networks and artificial intelligence applications, artificial synaptic devices need to have variable accumulation and non-volatile polarization properties to simulate the synaptic connections between biological neurons and realize learning and memory functions.

[0003] Hafnium oxide (HfO2)-based ferroelectric materials are materials with ferroelectric properties, with hafnium oxide as the main component. Ferroelectricity means that within a certain temperature range, the material has spontaneous polarization, and the direction of spontaneous polarization can be reversed under the action of an external electric field. This polarization reversal property makes hafnium oxide-based ferroelectric materials have broad application prospects in fields such as non-volatile memory and neuromorphic computing.

[0004] Hafnium oxide (HfO2)-based ferroelectric materials have attracted much attention in emerging non-volatile memory and neuromorphic computing applications due to their full CMOS compatibility, nm-scale ferroelectricity, fast polarization switching speed and low power consumption. However, they also face key challenges. The main challenge is that due to their high ferroelectric flip barrier and "independent flip" dipole flip mode, devices based on this ferroelectric material have a high coercive field, resulting in problems such as the device operating voltage being incompatible with advanced technology nodes and limited erase and write times.

[0005] As an extension of HfO2-based ferroelectric materials, HZO antiferroelectric materials have strong durability, minimal incremental leakage current under electric field cycling and lower power consumption (due to lower Ec), and are another emerging system of HfO2-based ferroelectric materials.

[0006] However, the preparation process of antiferroelectric neuromorphic devices is too complicated, resulting in high production costs, and traditional processes cannot prepare antiferroelectric neuromorphic devices, resulting in the inability of existing antiferroelectric neuromorphic devices to meet demand, limiting the development of the field of antiferroelectric neuromorphic devices. When in use, it is difficult to achieve synaptic morphological characteristics and functions including paired pulse facilitation, excitatory postsynaptic current and long-term potentiation / depression, making it impossible to meet the requirements of emerging synaptic devices. Summary of the invention

[0007] The purpose of the present invention is to realize the non-volatility of hafnium zirconium oxide antiferroelectric materials, to realize an antiferroelectric neuromorphic device and a preparation method thereof that can realize synaptic morphological characteristics and functions including paired pulse facilitation, excitatory postsynaptic current, long-term potentiation and inhibition, etc.

[0008] In a first aspect, the present invention proposes a method for preparing an antiferroelectric neuromorphic device, comprising: providing a substrate; generating a first metal layer on the substrate as a first electrode; forming a hafnium zirconium oxide film on the first metal layer; forming a second metal layer on the hafnium zirconium oxide film; crystallizing the hafnium zirconium oxide film by rapid heat treatment and generating antiferroelectricity; removing the second metal layer; forming a third metal layer on the hafnium zirconium oxide film; forming a fourth metal layer on the third metal layer as a second electrode, wherein the work function of the first metal layer corresponding to the first electrode and the third and fourth metal layers corresponding to the second electrode are different.

[0009] The method of the present invention has the following beneficial effects: providing a substrate; generating a first metal layer on the substrate as a first electrode; forming a hafnium zirconium oxide film on the first metal layer; forming a second metal layer on the hafnium zirconium oxide film; performing an etching process on the second metal layer; forming a third metal layer on the hafnium zirconium oxide film; forming a fourth metal layer on the third metal layer as a second electrode, wherein the work functions of the first metal layer corresponding to the first electrode and the third and fourth metal layers corresponding to the second electrode are different, thereby reducing production costs, simplifying processes, realizing the preparation of high-performance antiferroelectric neuromorphic devices, and meeting the needs of emerging synaptic devices.

[0010] Optionally, forming a third metal layer on the hafnium zirconium oxide film includes: depositing a 10 nm third metal layer on the hafnium zirconium oxide film using physical vapor deposition, wherein the third metal layer is titanium metal.

[0011] Optionally, a fourth metal layer is formed on the third metal layer as a second electrode, including: depositing a 70nm fourth metal layer on the third metal layer using physical vapor deposition, wherein the fourth metal layer is gold metal.

[0012] Optionally, providing the substrate includes: cleaning the substrate using an RCA cleaning process, and then drying the substrate with nitrogen.

[0013] Optionally, forming a first metal layer on the substrate as a first electrode includes: depositing the first metal layer using physical vapor deposition, wherein the first metal layer has a thickness of 80 nm.

[0014] Optionally, forming a hafnium zirconium oxide film on the first metal layer includes: depositing the hafnium zirconium oxide film using a plasma atomic layer deposition method, with a reaction temperature of 250° C. and a deposition rate of 0.1 nm per cycle.

[0015] Optionally, a plasma atomic layer deposition method is used to deposit a hafnium zirconium oxide film, including: during the deposition process, each time a hafnium source gas is introduced for a deposition cycle, the zirconium source gas is introduced nine times in succession for deposition cycles, and the deposition thickness of the hafnium zirconium oxide film is 6 nm.

[0016] Optionally, a second metal layer is formed on the hafnium zirconium oxide film, including: depositing the second metal layer using physical vapor deposition, the second metal layer is deposited to a thickness of 80 nm, and after depositing the second metal layer using physical vapor deposition, treating the antiferroelectric neuromorphic device at 550° C. for 30 seconds using rapid thermal processing technology.

[0017] Optionally, removing the second metal layer includes: etching the second metal layer using a wet etching process, and the composition ratio of the wet etching solution is as follows:

[0018] NH4H2O∶H2O2∶H2O=1∶2∶5.

[0019] Optionally, the thickness of the first metal layer is 80 nm, the thickness of the hafnium zirconium oxide film is 6 nm, the thickness of the third metal layer is 10 nm, and the thickness of the fourth metal layer is 70 nm.

[0020] On the second aspect, in some embodiments, an antiferroelectric neuromorphic device is also proposed, which is manufactured using the method proposed in the above embodiment, including a substrate, a first metal layer, a hafnium zirconium oxide film, a third metal layer and a fourth metal layer formed in sequence from bottom to top.

[0021] The beneficial effects of the present invention are as follows: a built-in field can be constructed by using a first electrode and a second electrode with different work functions. The existence of the built-in electric field will affect the charge distribution in the material, thereby changing the polarization characteristics of the material and causing the polarization intensity-voltage loop to shift, thereby achieving the non-volatility of the hafnium zirconium oxide (HZO) antiferroelectric material, that is, non-volatility means that the material can maintain its polarization state after the external electric field is removed; on the basis of non-volatility, the morphological characteristics and functions of the neural synapses including paired pulse facilitation, excitatory postsynaptic current and long-term potentiation / depression can be achieved, and it is expected that the emerging hafnium zirconium oxide (HZO) antiferroelectric material will be applied to the field of neuromorphic computing. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic diagram of the structure of the present invention in a substrate-providing state;

[0023] Figure 2 A schematic diagram of the structure in the first metal layer state is generated for the present invention;

[0024] Figure 3 It is a schematic diagram of the structure of the present invention in which a hafnium zirconium oxide thin film is formed on the first metal layer;

[0025] Figure 4 It is a schematic structural diagram of the present invention in a state where a second metal layer is formed on a hafnium zirconium oxide film;

[0026] Figure 5 It is a schematic diagram of the structure of the present invention after the second metal layer is subjected to an etching process;

[0027] Figure 6 It is a schematic structural diagram of the present invention after a third metal layer is formed on the hafnium zirconium oxide film;

[0028] Figure 7 It is a schematic structural diagram of the present invention in a state where a fourth metal layer is formed on the third metal layer;

[0029] Figure 8 It is a schematic flow chart of the preparation method of the present invention.

[0030] Description of the drawings: 1. substrate; 2. first metal layer; 3. hafnium zirconium oxide film; 4. second metal layer; 5. third metal layer; 6. fourth metal layer. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.

[0032] It should be mentioned that the work function (Work Function) referred to in this application refers to the minimum energy required for an electron inside the semiconductor material to overcome the atomic bonding force and move from the Fermi level (Fermi level, E_F) of the semiconductor to the surface of the material until it leaves the semiconductor and enters a vacuum. In simple terms, it is the difference between the energy (i.e., zero-point energy level) of the semiconductor Fermi level and the stationary electron in a vacuum. Numerically, the work function is usually measured in electron volts (eV). The semiconductor work function is very important for understanding and controlling the electron emission process on the semiconductor surface, especially in the design of fields such as MIS (metal-insulator-semiconductor) structures, Schottky diodes, field emission devices, and metal-semiconductor contacts. In addition, the work function of the semiconductor is affected by many factors, such as doping concentration, temperature, surface reconstruction, the presence of surface adsorbates, etc., which will change the state of the semiconductor surface and further affect its work function value.

[0033] As attached Figure 1and Figure 8 As shown, a method for preparing an antiferroelectric neuromorphic device comprises:

[0034] S101, providing a substrate 1;

[0035] Specifically, a SiO2 / Si substrate 1 can be used. The SiO2 / Si substrate 1 is a composite substrate 1 composed of silicon dioxide (SiO2) and silicon (Si), and refers to a composite material in which a layer of silicon dioxide (SiO2) thin film is formed on the surface of a silicon (Si) wafer by chemical vapor deposition (CVD), thermal oxidation or wet oxidation as an insulating layer.

[0036] In some specific embodiments, providing the substrate 1 includes: performing an RCA cleaning process on the substrate 1, and then drying the substrate 1 with nitrogen gas.

[0037] Specifically, in the semiconductor manufacturing process, cleaning the substrate 1 (e.g., SiO2 / Si substrate 1) is a very important step to remove organic matter, particulate contaminants, and other impurities on the surface to ensure that the subsequently deposited thin film has excellent adhesion and purity;

[0038] In addition, RCA cleaning is a classic semiconductor cleaning process, which mainly includes two steps: sulfuric acid-hydrofluoric acid mixed solution cleaning (SC-1) and ammonium hydroxide-hydrogen peroxide-water mixed solution cleaning (SC-2);

[0039] After cleaning, in order to prevent contamination by impurities again, high-purity nitrogen is usually used to blow dry the substrate 1. As an inert gas, nitrogen is not easy to react with other substances and can effectively blow away moisture from the surface of the substrate 1 without introducing new pollution sources.

[0040] Nitrogen drying is generally performed in a drying cabinet, and the nitrogen flow directed toward the surface of the substrate 1 quickly removes moisture to achieve the purpose of rapid drying while avoiding the risk of secondary contamination caused by natural drying.

[0041] S102, generating a first metal layer 2 on the substrate 1 as a first electrode;

[0042] In some specific embodiments, forming a first metal layer 2 on a substrate 1 as a first electrode includes: depositing the first metal layer 2 using a physical vapor deposition method.

[0043] Specifically, physical vapor deposition (PVD) is a technique for depositing a thin film on a substrate 1, which generally involves converting a material from a solid state to a gas state (evaporation or sputtering), and then condensing it on the substrate 1 to form a first metal layer 2 thin film.

[0044] In some specific embodiments, the thickness of the first metal layer 2 is 80 nm.

[0045] S103, forming a hafnium zirconium oxide thin film 3 on the first metal layer 2;

[0046] In some specific embodiments, forming the hafnium zirconium oxide film 3 on the first metal layer 2 includes: depositing the hafnium zirconium oxide film 3 using a plasma atomic layer deposition method.

[0047] Specifically, in the semiconductor manufacturing process, a hafnium zirconium oxide (HZO) thin film is formed on the first metal layer 2 by plasma enhanced atomic layer deposition (PEALD) technology. PEALD is a very precise thin film growth technology that deposits atomic-level thin films layer by layer through a series of self-limiting chemical reaction steps to achieve extremely high-precision control of film thickness and composition.

[0048] In some specific embodiments, when the reaction temperature is 250° C., the deposition rate is 0.1 nm per cycle.

[0049] In some specific embodiments, plasma atomic layer deposition is used to deposit the hafnium zirconium oxide film 3, including: during the deposition process, after each hafnium source gas is introduced for a deposition cycle, the zirconium source gas is continuously introduced for nine deposition cycles, and the deposition thickness of the hafnium zirconium oxide film 3 is 6nm.

[0050] Specifically, in semiconductor device manufacturing, in order to obtain hafnium zirconium oxide (HZO) thin films with antiferroelectric properties, the plasma atomic layer deposition (PEALD) method is used to accurately control the composition and structure of the film. For the case where the film thickness is required to be 6nm and the deposition rate is 0.1nm / cycle;

[0051] Since the film needs to be deposited to a thickness of 6nm, and each cycle deposits 0.1nm, the total number of cycles required theoretically is 6nm divided by 0.1nm / time, that is:

[0052] Total number of cycles = 6nm / 0.1nm / time = 60 times;

[0053] In addition, in order to give the film antiferroelectric properties, it is necessary to precisely control the ratio of hafnium (Hf) and zirconium (Zr), which is set here to 1:9, meaning that during the deposition process, one cycle out of every 10 cycles is dedicated to depositing hafnium oxide, and the remaining 9 cycles are used to deposit zirconium oxide, ensuring that the ratio of elements in the final film meets the requirements, thereby preparing a 6nm thick HZO film with excellent antiferroelectric properties and suitable for storage applications on the first metal layer 2.

[0054] S104, forming a second metal layer 4 on the hafnium zirconium oxide thin film 3;

[0055] S105, crystallizing the hafnium zirconium oxide thin film and generating antiferroelectricity by rapid thermal treatment;

[0056] In some specific embodiments, a second metal layer 4 is formed on the hafnium zirconium oxide film 3, including: depositing the second metal layer 4 using physical vapor deposition, the second metal layer 4 is deposited to a thickness of 80 nm, and after depositing the second metal layer 4 using physical vapor deposition, treating the antiferroelectric neuromorphic device at 550°C for 30 seconds using rapid thermal processing technology.

[0057] Specifically, a second metal layer 4 is deposited on the HZO film using physical vapor deposition (PVD), and the thickness of the metal layer is set to 80 nm. In addition, this step requires precise control of deposition conditions, such as sputtering power, gas pressure, deposition time, etc., to ensure that the thickness of the metal layer is uniform and has good adhesion to the HZO film.

[0058] In practice, the material of the second metal layer 4 is usually selected to be a metal with good conductivity, compatible with the HZO film and capable of meeting the functional requirements of the device, such as platinum (Pt), aluminum (Al), copper (Cu), etc.

[0059] After the deposition of the second metal layer 4 is completed, the entire antiferroelectric neuromorphic device is heat treated using a rapid thermal processing technique. In this case, the device is placed in a specific high temperature environment and heat treated at 550°C for 30 seconds. The main purpose of the rapid thermal processing is to produce a good interface reaction between the second metal layer 4 and the HZO film and improve the adhesion strength between them. It may also help to improve the antiferroelectric properties of the HZO film and activate the potential charge storage mechanism.

[0060] S106, removing the second metal layer;

[0061] In some specific embodiments, removing the second metal layer includes: etching the second metal layer using a wet etching process, and the composition ratio of the wet etching solution is as follows:

[0062] NH4H2O∶H2O2∶H2O=1∶2∶5,

[0063] Specifically, wet etching uses chemical solutions to react with the metal layer to selectively remove unnecessary parts to form a desired pattern, and uses the principle that the thermal expansion coefficients of the second metal layer 4 and the antiferroelectric layer are different to crystallize the HZO film and generate antiferroelectricity.

[0064] S107, forming a third metal layer 5 on the hafnium zirconium oxide film 3;

[0065] In some specific embodiments, forming the third metal layer 5 on the hafnium zirconium oxide film 3 includes: depositing a 10 nm third metal layer 5 on the hafnium zirconium oxide film 3 using physical vapor deposition, wherein the third metal layer 5 is titanium metal.

[0066] S108, forming a fourth metal layer 6 on the third metal layer 5 as a second electrode;

[0067] The work functions of the first metal layer 2 corresponding to the first electrode and the third metal layer 5 and the fourth metal layer 6 corresponding to the second electrode are different.

[0068] Specifically, the work function describes the minimum energy required for electrons to escape from the interior of a solid into a vacuum. By using a first electrode and a second electrode with different work functions, a built-in field can be constructed. The existence of the built-in electric field will affect the charge distribution in the material, thereby changing the polarization characteristics of the material and shifting the polarization intensity-voltage loop, thereby achieving the non-volatility of hafnium zirconium oxide (HZO) antiferroelectric material. That is, non-volatility means that the material can maintain its polarization state after the external electric field is removed.

[0069] In some specific embodiments, a fourth metal layer 6 is formed on the third metal layer 5 as a second electrode, including: depositing a 70nm fourth metal layer 6 on the third metal layer 5 using physical vapor deposition, wherein the fourth metal layer 6 is gold metal.

[0070] Specifically, the steps of forming the Au / Ti top electrode by physical vapor deposition (PVD) are as follows: depositing a 10 nm thick Ti layer: placing the substrate 1 to be processed into the PVD chamber, ensuring that the surface is clean and the positioning is accurate, setting the PVD equipment, selecting titanium (Ti) as the target material, and setting the deposition parameters, such as sputtering power, argon pressure, gas flow, etc., to ensure the deposition rate and film quality; starting the deposition process until a 10 nm thick titanium metal layer is formed on the surface of the substrate 1, which will serve as the bottom layer or bonding layer of the Au / Ti top electrode, providing good adhesion and conductivity; depositing a 70 nm thick Au layer: after completing the deposition of the titanium layer, there is no need to move the substrate 1, and continue to deposit a gold (Au) layer directly on the original titanium metal layer, adjust the PVD equipment parameters to adapt to the characteristics of the gold target, and also ensure that the deposition rate and thickness are accurately controlled, and start the deposition process of the gold layer until its thickness reaches 70 nm, covering the previous titanium layer to form a top electrode (i.e., the second electrode) of the Au / Ti double-layer structure.

[0071] Au provides good conductivity and oxidation resistance, while Ti enhances the adhesion and stability of Au to the underlying material.

[0072] In some specific embodiments, an antiferroelectric neuromorphic device is also proposed, which is manufactured using the method described in the above embodiment, and includes a substrate 1, a first metal layer 2, a hafnium zirconium oxide film 3, a third metal layer 5 and a fourth metal layer 6 formed in sequence from bottom to top, and the third metal layer 5 and the fourth metal layer 6 form a stacked structure of Au / Ti and are set as the second electrode.

[0073] In some specific embodiments, the thickness of the first metal layer is 80 nm, the thickness of the hafnium zirconium oxide film is 6 nm, the thickness of the third metal layer is 10 nm, and the thickness of the fourth metal layer is 70 nm.

[0074] For ease of understanding, this embodiment further illustrates the specific implementation process of the above method in combination with a specific application scenario system.

[0075] Step 1, such as Figure 1 As shown, a substrate 1 is provided, the substrate 1 is cleaned by an RCA cleaning process, and then the substrate 1 is dried by nitrogen gas;

[0076] Step 2, such as Figure 2 As shown, a first metal layer 2 is generated on a substrate 1 as a first electrode. The first metal layer 2 is deposited by physical vapor deposition, and the thickness of the first metal layer 2 is 80 nm.

[0077] Step 3, such as Figure 3As shown, a hafnium zirconium oxide film 3 is formed on the first metal layer 2, and the hafnium zirconium oxide film 3 is deposited by plasma atomic layer deposition. When the reaction temperature is 250° C., the deposition rate is 0.1 nm per cycle. During the deposition process, after each hafnium source gas is introduced for a deposition cycle, the zirconium source gas is continuously introduced for nine deposition cycles. The deposition thickness of the hafnium zirconium oxide film 3 is 6 nm.

[0078] Step 4, such as Figure 4 As shown, a second metal layer 4 is formed on the hafnium zirconium oxide film 3, and the second metal layer 4 is deposited by physical vapor deposition. The thickness of the second metal layer 4 is 80 nm. After the second metal layer 4 is deposited by physical vapor deposition, the antiferroelectric neuromorphic device is treated at 550° C. for 30 seconds by rapid thermal processing technology;

[0079] Step 5, such as Figure 5 As shown, the second metal layer 4 is subjected to an etching process, and the second metal layer is etched using a wet etching process, and the composition ratio of the wet etching solution is as follows:

[0080] NH4H2O∶H2O2∶H2O=1∶2∶5;

[0081] Step 6, such as Figure 6 As shown, a third metal layer 5 is formed on the hafnium zirconium oxide film 3, and a 10 nm third metal layer 5 is deposited on the hafnium zirconium oxide film 3 by physical vapor deposition, wherein the third metal layer 5 is titanium metal;

[0082] Step 7, such as Figure 7 As shown, a fourth metal layer 6 is formed on the third metal layer 5 as a second electrode; a 70nm fourth metal layer 6 is deposited on the third metal layer 5 by physical vapor deposition, and the fourth metal layer 6 is gold metal.

[0083] Through the description of the above implementation methods, technicians in the relevant field can clearly understand that for the convenience and simplicity of description, only the division of the above functional modules is used as an example. In actual applications, the above functions can be assigned to different functional modules as needed, that is, the internal structure of the device is divided into different functional modules to complete all or part of the functions described above. The specific working process of the system, device and unit described above can refer to the corresponding process in the aforementioned method embodiment, and will not be repeated here.

[0084] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.

Claims

1. A method for preparing an antiferroelectric neuromorphic device, characterized in that: include: providing a substrate; Generating a first metal layer on the substrate as a first electrode; forming a hafnium zirconium oxide thin film on the first metal layer; forming a second metal layer on the hafnium zirconium oxide film; The hafnium zirconium oxide thin film is crystallized and antiferroelectricity is generated by rapid thermal processing; removing the second metal layer; forming a third metal layer on the hafnium zirconium oxide film; forming a fourth metal layer on the third metal layer as a second electrode; The work functions of the first metal layer corresponding to the first electrode and the third metal layer and the fourth metal layer corresponding to the second electrode are different.

2. The method according to claim 1, characterized in that Forming a third metal layer on the hafnium zirconium oxide film comprises: A 10 nm third metal layer is deposited on the hafnium zirconium oxide film by physical vapor deposition, wherein the third metal layer is titanium metal.

3. The method according to claim 1, characterized in that A fourth metal layer is formed on the third metal layer as a second electrode, comprising: A 70 nm fourth metal layer of gold metal is deposited on the third metal layer using physical vapor deposition.

4. The method according to claim 1, characterized in that: Providing the substrate includes: performing an RCA cleaning process on the substrate, and then drying the substrate with nitrogen.

5. The method according to claim 1, characterized in that Forming a first metal layer on a substrate as a first electrode includes: depositing the first metal layer using a physical vapor deposition method, wherein the first metal layer has a thickness of 80 nm.

6. The method according to claim 1, characterized in that Forming a hafnium zirconium oxide thin film on the first metal layer includes: The hafnium zirconium oxide film was deposited by plasma atomic layer deposition. When the reaction temperature was 250°C, the deposition rate was 0.1 nm per cycle.

7. The method according to claim 6, characterized in that Deposition of hafnium zirconium oxide thin films using plasma atomic layer deposition, including: During the deposition process, after each hafnium source gas is introduced for a deposition cycle, the zirconium source gas is introduced nine times in succession for deposition cycles. The deposition thickness of the hafnium zirconium oxide film is 6 nm.

8. The method according to claim 1, characterized in that: forming a second metal layer on the hafnium zirconium oxide film, comprising: The second metal layer is deposited by physical vapor deposition. The thickness of the deposited second metal layer is 80 nm. After the second metal layer is deposited by physical vapor deposition.

9. The method according to claim 1, characterized in that: The antiferroelectric neuromorphic device was treated at 550 °C for 30 seconds by rapid thermal processing technique.

10. The method according to claim 1, characterized in that Removing the second metal layer includes: The two metal layers are etched using a wet etching process, and the composition ratio of the wet etching solution is: NH4H2O∶H2O2∶H2O=1∶2∶5.

11. An antiferroelectric neuromorphic device, characterized in that: The invention comprises a substrate, a first metal layer, a hafnium zirconium oxide film, a third metal layer and a fourth metal layer which are sequentially formed from bottom to top.

12. The antiferroelectric neuromorphic device according to claim 10, characterized in that: The thickness of the first metal layer is 80 nm, the thickness of the hafnium zirconium oxide film is 6 nm, the thickness of the third metal layer is 10 nm, and the thickness of the fourth metal layer is 70 nm.

13. The antiferroelectric neuromorphic device according to claim 11, characterized in that: The substrate is made of silicon dioxide / silicon, the third metal layer is made of titanium metal, and the fourth metal layer is made of gold metal.