Method for producing stretched film

Through the temperature control and process optimization of the original coil film of poly(3-hydroxybutyrate) resin, the process complexity in the production of poly(3-hydroxybutyrate) resin stretch film in the prior art is solved and The pasting problem has achieved efficient and stable manufacturing of tensile films, improving the strength and productivity of the films.

CN118922291APending Publication Date: 2024-11-08KANEKA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028900.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-15
Publication Date
2024-11-08

Smart Images

  • Figure BDA0005051267760000271
    Figure BDA0005051267760000271
  • Figure BDA0005051267760000291
    Figure BDA0005051267760000291
  • Figure HDA0005051267790000011
    Figure HDA0005051267790000011
Patent Text Reader

Abstract

In a method for producing a stretched film by stretching a raw roll film containing a poly (3-hydroxybutyrate)-based resin, the raw roll film is stretched under conditions in which the maximum temperature of the film surface is within the temperature range represented by the following formula. Tm-60 < = maximum temperature (DEG C) of the film surface < = Tm-5. And Tm is the melting point (DEG C) of the original roll film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a stretched film containing a poly(3-hydroxybutyrate)-based resin. Background Art

[0002] In recent years, the separation and recycling of kitchen waste and the processing of compost have been carried out, mainly in Europe, and there is a desire for plastic products that can be processed as compost together with kitchen waste.

[0003] On the other hand, environmental issues caused by discarded plastics have attracted attention, and in particular, it is known that large amounts of plastics are floating in the oceans worldwide through ocean dumping, rivers, etc. Since such plastics retain their shape for a long time, they are pointed out to have an impact on the ecosystem, such as so-called ghost fishing that restricts and captures marine organisms, and when ingested by marine organisms, they remain in the digestive organs and cause feeding disorders.

[0004] In addition, microplastics, which are formed when plastics are destroyed or broken down into microparticles by ultraviolet rays, absorb harmful compounds in the ocean, and have been pointed out to be a problem in which harmful substances enter the food chain through ingestion by marine organisms.

[0005] In response to such marine pollution caused by plastics, the use of biodegradable plastics is expected. However, a report compiled by the United Nations Environment Programme in 2015 pointed out that since plastics such as polylactic acid that can be biodegraded by mixed fertilizers cannot be expected to degrade in a short period of time in the actual ocean with low temperatures, they cannot serve as a countermeasure to marine pollution.

[0006] Among them, poly(3-hydroxybutyrate)-based resins are biodegradable materials even in seawater, and therefore have attracted attention as raw materials for solving the above-mentioned problems.

[0007] As a technique for producing a thin and high-strength resin film, a method of stretching a resin film in a temperature range equal to or higher than the glass transition temperature is known.

[0008] However, due to the characteristics of poly(3-hydroxybutyrate)-based resins, it is difficult to stretch them under general stretching conditions, and various solutions have been investigated.

[0009] For example, Patent Document 1 describes a method for stretching a film containing a poly(3-hydroxybutyrate) resin. The method comprises forming a thermoplastic resin containing a poly(3-hydroxybutyrate) resin as a main component into a film shape, performing a primary stretching by roll rolling at a temperature range of 20 to 90°C, and further performing a secondary stretching in the same direction at a temperature range of 30 to 90°C to produce a stretched film.

[0010] Patent Document 2 describes a method in which an amorphous film is prepared from a molten film of a poly(3-hydroxybutyrate) resin as a raw material, and then the amorphous film is cold stretched at a temperature lower than the glass transition temperature + 20°C (specifically 3°C) to produce a stretched film.

[0011] Patent Document 3 describes a method of producing a stretched film by blending at least 20 wt % of poly(ε-caprolactone) into a copolymer of 3-hydroxybutyrate and 3-hydroxyvalerate, which is one of poly(3-hydroxybutyrate)-based resins, at a temperature range of 40 to 90° C.

[0012] Prior art literature

[0013] Patent Literature

[0014] Patent Document 1: Japanese Patent Application Publication No. 2006-168159

[0015] Patent Document 2: Japanese Patent Application Publication No. 2003-311824

[0016] Patent Document 3: Japanese Patent Application Laid-Open No. 10-110047 Summary of the invention

[0017] Problems to be solved by the invention

[0018] In the method described in Patent Document 1, since the stretching is performed in one direction, a two-step stretching process of primary stretching by roll calendaring and secondary stretching at a high temperature is required, which has a problem of complicating the production process.

[0019] In the method described in Patent Document 2, an amorphous film needs to be produced and then stretched. However, the amorphous film easily adheres to a stretching roller or other tool used for stretching, and thus there is a problem in that productivity cannot be improved.

[0020] The method described in Patent Document 3 requires the addition of 20 wt % or more of poly(ε-caprolactone), and only 80 wt % or less of a poly(3-hydroxybutyrate) resin can be used as the resin component, which limits the composition of the film.

[0021] In view of the above-mentioned current situation, an object of the present invention is to provide a method for producing a stretched film, which is capable of stretching a film composed of a poly(3-hydroxybutyrate)-based resin with good productivity.

[0022] Solution to the problem

[0023] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found that by controlling the temperature conditions when stretching a raw roll film containing a poly(3-hydroxybutyrate) resin to a specific range, a film containing a poly(3-hydroxybutyrate) resin can be stretched with good productivity, thereby completing the present invention.

[0024] That is, the present invention relates to a production method, which is a method for producing a stretched film by stretching an original roll film containing a poly(3-hydroxybutyrate)-based resin, the method comprising:

[0025] A step of stretching the raw film under the condition that the maximum temperature of the film surface is within the temperature range represented by the following formula (1).

[0026] Tm-60≤Maximum temperature of membrane surface(℃)≤Tm-5 (1)

[0027] The above-mentioned Tm is the melting point (° C.) of the above-mentioned original film.

[0028] Another aspect of the present invention relates to a production method, which is a method for producing a biaxially stretched film by biaxially stretching a raw film containing a poly(3-hydroxybutyrate)-based resin, the method comprising:

[0029] The step (i) of stretching the original roll film along a specific direction; and

[0030] Step (ii) of performing stretching in a direction perpendicular to the specific direction,

[0031] The step (ii) is a step of performing stretching under the condition that the maximum temperature of the film surface is within the temperature range represented by the following formula (1).

[0032] Tm-60≤Maximum temperature of membrane surface(℃)≤Tm-5 (1)

[0033] The above-mentioned Tm is the melting point (° C.) of the above-mentioned original film.

[0034] Effects of the Invention

[0035] According to the present invention, a method for producing a stretched film can be provided, which can stretch a film made of a poly(3-hydroxybutyrate)-based resin with good productivity. The stretched film may be a uniaxially stretched film or a biaxially stretched film.

[0036] According to a preferred embodiment of the present invention, a stretched film composed of a poly(3-hydroxybutyrate)-based resin can be produced with good productivity in a continuous process. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1This is a schematic diagram showing an example of a production line for continuously stretching a film according to one embodiment of the present invention.

[0038] Figure 2 This is a plan view showing the shape of a test piece used when measuring the breaking strength of a stretched film in Examples.

[0039] Explanation of symbols

[0040] 11 Delivery roller

[0041] 21 Original roll film

[0042] 22 Stretch Film

[0043] 12 Take-up roller

[0044] 31, 32, 33 preheating rollers

[0045] 34 Upstream stretching roller

[0046] 35 Downstream stretching roller

[0047] 36, 37 Heat treatment roller

[0048] A Heating area

[0049] A1 Upper Nozzle

[0050] A2 Lower Nozzle DETAILED DESCRIPTION

[0051] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following embodiments.

[0052] This embodiment relates to a method for producing a stretched film by stretching a raw film made of a poly(3-hydroxybutyrate)-based resin. First, the raw film will be described.

[0053] <Original roll film>

[0054] The raw film contains a poly(3-hydroxybutyrate)-based resin as a main resin component.

[0055] The poly(3-hydroxybutyrate) resin is an aliphatic polyester resin having 3-hydroxybutyrate as a repeating unit that can be produced by a microorganism. The poly(3-hydroxybutyrate) resin may be a poly(3-hydroxybutyrate) having only 3-hydroxybutyrate as a repeating unit, or a copolymer of 3-hydroxybutyrate and other hydroxyalkanoates. In addition, the poly(3-hydroxybutyrate) resin may be a mixture of a homopolymer and one or more copolymers, or a mixture of two or more copolymers.

[0056] Specific examples of the poly(3-hydroxybutyrate)-based resins include poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), and poly(3-hydroxybutyrate-co-3-hydroxyoctadecanoate). Among them, poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate), and poly(3-hydroxybutyrate-co-4-hydroxybutyrate) are preferred from the perspective of easy industrial production.

[0057] In addition, by changing the composition ratio of the repeating units, the melting point, crystallinity, Young's modulus, heat resistance and other physical properties can be changed. From the viewpoint of being able to impart physical properties between polypropylene and polyethylene, and being easy to produce industrially and being a plastic useful in terms of physical properties, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) is preferred. In particular, among poly(3-hydroxybutyrate)-based resins that have the property of being easily thermally decomposed when heated to 180°C or above, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) is preferred from the viewpoint of being able to lower the melting point and perform molding processing at low temperatures.

[0058] Examples of commercially available products of poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) include "Kaneka Biodegradable Polymer Green Planet" (registered trademark) manufactured by Kaneka Corporation.

[0059] The melting point, Young's modulus, etc. of the above-mentioned poly(3-hydroxybutyrate-co-3-hydroxyvalerate) change with the ratio of the 3-hydroxybutyrate component to the 3-hydroxyvalerate component. Since the two components are co-crystallized, the crystallinity is as high as 50% or more, which is softer than poly(3-hydroxybutyrate), but the improvement in brittleness is insufficient.

[0060] In the case where the poly(3-hydroxybutyrate)-based resin comprises a copolymer of a 3-hydroxybutyrate unit and other hydroxyalkanoate units, from the viewpoint of achieving both strength and productivity of the stretched film, the average content ratio of the 3-hydroxybutyrate unit and other hydroxyalkanoate units in all monomer units constituting the poly(3-hydroxybutyrate)-based resin is preferably 3-hydroxybutyrate unit / other hydroxyalkanoate = 99 / 1 to 80 / 20 (mol % / mol %), and more preferably 97 / 3 to 85 / 15 (mol % / mol %).

[0061] The average content ratio of each monomer unit in all monomer units constituting the poly(3-hydroxybutyrate)-based resin can be obtained by a method known to those skilled in the art, for example, the method described in paragraph

[0047] of International Publication No. 2013 / 147139. The average content ratio refers to the molar ratio of each monomer unit in all monomer units constituting the poly(3-hydroxybutyrate)-based resin. When the poly(3-hydroxybutyrate)-based resin is a mixture of two or more poly(3-hydroxybutyrate)-based resins, it refers to the molar ratio of each monomer unit contained in the entire mixture.

[0062] The poly(3-hydroxybutyrate)-based resin may be a mixture of at least two poly(3-hydroxybutyrate)-based resins having different types of constituent monomers and / or different content ratios of constituent monomers. In this case, at least one highly crystalline poly(3-hydroxybutyrate)-based resin and at least one low crystalline poly(3-hydroxybutyrate)-based resin may be used in combination.

[0063] Generally speaking, highly crystalline poly(3-hydroxybutyrate)-based resins have excellent productivity but poor mechanical strength, while low crystalline poly(3-hydroxybutyrate)-based resins have poor productivity but excellent mechanical properties. It is speculated that when the two resins are used in combination, the highly crystalline poly(3-hydroxybutyrate)-based resin forms fine resin crystal particles, and the low crystalline poly(3-hydroxybutyrate)-based resin forms tie molecules that cross-link the resin crystal particles. By using these resins in combination, the strength and productivity of the stretched film can be improved.

[0064] The content of 3-hydroxybutyrate units in the highly crystalline poly(3-hydroxybutyrate)-based resin is preferably higher than the average content of 3-hydroxybutyrate units in all monomer units of a mixture constituting the poly(3-hydroxybutyrate)-based resin.

[0065] When the highly crystalline poly(3-hydroxybutyrate)-based resin contains 3-hydroxybutyrate units and other hydroxyalkanoate units, the content ratio of the other hydroxyalkanoate units in the highly crystalline resin is preferably 1 to 5 mol %, more preferably 2 to 4 mol %.

[0066] The highly crystalline poly(3-hydroxybutyrate)-based resin is preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) or poly(3-hydroxybutyrate-co-4-hydroxybutyrate), and more preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).

[0067] The content of 3-hydroxybutyrate units in the low-crystalline poly(3-hydroxybutyrate)-based resin is preferably lower than the average content of 3-hydroxybutyrate units in all monomer units constituting the mixture of the poly(3-hydroxybutyrate)-based resin.

[0068] When the low-crystalline poly(3-hydroxybutyrate)-based resin contains 3-hydroxybutyrate units and other hydroxyalkanoate units, the content ratio of the other hydroxyalkanoate units in the low-crystalline resin is preferably 24 to 99 mol%, more preferably 24 to 50 mol%, further preferably 24 to 35 mol%, and particularly preferably 24 to 30 mol%.

[0069] The low-crystalline poly(3-hydroxybutyrate)-based resin is preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) or poly(3-hydroxybutyrate-co-4-hydroxybutyrate), and more preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).

[0070] When a highly crystalline poly(3-hydroxybutyrate) resin and a low crystalline poly(3-hydroxybutyrate) resin are used in combination, the ratio of each resin to the total amount of the two resins is not particularly limited, but the former is preferably 10% by weight or more and 60% by weight or less, and the latter is preferably 40% by weight or more and 90% by weight or less, and the former is more preferably 25% by weight or more and 45% by weight or less, and the latter is more preferably 55% by weight or more and 75% by weight or less.

[0071] According to one embodiment, in addition to the high-crystalline poly(3-hydroxybutyrate)-based resin and the low-crystalline poly(3-hydroxybutyrate)-based resin, a medium-crystalline poly(3-hydroxybutyrate)-based resin having a crystallinity intermediate between the two resins may be used in combination.

[0072] In the case where the medium-crystalline poly(3-hydroxybutyrate)-based resin contains 3-hydroxybutyrate units and other hydroxyalkanoate units, the content ratio of the other hydroxyalkanoate units in the medium-crystalline resin is preferably 6 mol% or more and less than 24 mol%, more preferably 6 mol% or more and 22 mol% or less, further preferably 6 mol% or more and 20 mol% or less, and preferably 6 mol% or more and 18 mol% or less.

[0073] The above-mentioned medium-crystalline poly(3-hydroxybutyrate)-based resin is preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) or poly(3-hydroxybutyrate-co-4-hydroxybutyrate), and more preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).

[0074] When the above-mentioned medium crystalline poly(3-hydroxybutyrate)-based resin is further used in combination, the ratio of the medium crystalline poly(3-hydroxybutyrate)-based resin to the total of the high crystalline poly(3-hydroxybutyrate)-based resin, the low crystalline poly(3-hydroxybutyrate)-based resin and the medium crystalline poly(3-hydroxybutyrate)-based resin is preferably 1 wt % to 99 wt %, more preferably 5 wt % to 90 wt %, and even more preferably 8 wt % to 85 wt %.

[0075] The method for obtaining a blend of two or more poly(3-hydroxybutyrate)-based resins is not particularly limited, and may be a method of obtaining the blend by microbial production or a method of obtaining the blend by chemical synthesis. In addition, the blend may be obtained by melt-kneading two or more resins using an extruder, a kneader, a Banbury mixer, a roll, etc., or by dissolving two or more resins in a solvent and mixing / drying them to obtain the blend.

[0076] The weight average molecular weight of the poly(3-hydroxybutyrate)-based resin as a whole is not particularly limited, but is preferably 200,000 to 2,000,000, more preferably 250,000 to 1,500,000, and even more preferably 300,000 to 1,000,000 from the viewpoint of achieving a balance between the strength and productivity of the stretched film.

[0077] In addition, when the poly(3-hydroxybutyrate) resin is a mixture of two or more poly(3-hydroxybutyrate) resins, the weight average molecular weight of each poly(3-hydroxybutyrate) resin constituting the mixture is not particularly limited. However, when the above-mentioned high-crystalline poly(3-hydroxybutyrate) resin and low-crystalline poly(3-hydroxybutyrate) resin are used in combination, from the perspective of both the strength and productivity of the stretched film, the weight average molecular weight of the high-crystalline poly(3-hydroxybutyrate) resin is preferably 200,000 to 1,000,000, more preferably 220,000 to 800,000, and further preferably 250,000 to 600,000. On the other hand, from the perspective of both the strength and productivity of the stretched film, the weight average molecular weight of the low-crystalline poly(3-hydroxybutyrate) resin is preferably 200,000 to 2,500,000, more preferably 250,000 to 2,300,000, and further preferably 300,000 to 2,000,000. In addition, when the above-mentioned medium crystalline poly (3-hydroxybutyrate) type resin is further used, from the viewpoint of balancing the strength and productivity of the stretched film, the weight average molecular weight of the medium crystalline poly (3-hydroxybutyrate) type resin is preferably 200,000 to 2.5 million, more preferably 250,000 to 2.3 million, and even more preferably 300,000 to 2,000,000.

[0078] The weight average molecular weight of the poly(3-hydroxybutyrate) resin can be measured in terms of polystyrene using a gel permeation chromatograph (HPLC GPC system manufactured by Shimadzu Corporation) using a chloroform solution. Any column suitable for measuring the weight average molecular weight may be used as the column in the gel permeation chromatograph.

[0079] The method for producing poly (3-hydroxybutyrate) resins is not particularly limited, and may be a method for producing by chemical synthesis or a method for producing by microorganisms. Among them, a method for producing by microorganisms is preferred. For the method for producing by microorganisms, known methods can be applied. For example, as a copolymer-producing bacterium of 3-hydroxybutyrate and other hydroxyalkanoates, Aeromonas caviae as a P3HB3HV and P3HB3HH producing bacterium, Alcaligenes eutrophus as a P3HB4HB producing bacterium, and the like are known. In particular, regarding P3HB3HH, in order to improve the productivity of P3HB3HH, Alcaligenes eutrophus AC32 strain (FERM BP-6038) (T. Fukui, Y. Doi, J. Bateriol., 179, p4821-4830 (1997)) into which the gene of the P3HA synthase group is introduced is more preferred, and these microorganisms can be cultured under appropriate conditions, and microbial cells that accumulate P3HB3HH in the cells can be used. In addition to the above, genetically modified microorganisms into which various poly(3-hydroxybutyrate) resin synthesis-related genes are introduced can also be used according to the poly(3-hydroxybutyrate) resin to be produced, as long as the culture conditions including the type of substrate are optimized.

[0080] The poly(3-hydroxybutyrate)-based resin may be an unmodified resin or a resin obtained by modifying an unmodified poly(3-hydroxybutyrate)-based resin using a raw material that reacts with the resin such as a peroxide (hereinafter referred to as a "modifying raw material").

[0081] When a modified resin is used as a film raw material, the raw material obtained by reacting the resin with a modifying raw material may be formed into a film in advance, or the modifying raw material may be mixed with the resin and reacted during film forming. In addition, when reacting the resin with the modifying raw material, the entire resin may be reacted with the modifying raw material, or a portion of the resin may be reacted with the modifying raw material to obtain a modified resin, and then the remaining unmodified resin may be added to the modified resin.

[0082] The modifying raw material is not particularly limited as long as it is a compound that can react with the poly(3-hydroxybutyrate)-based resin, but an organic peroxide can be preferably used from the viewpoint of handleability and ease of controlling the reaction with the poly(3-hydroxybutyrate)-based resin.

[0083] Examples of the organic peroxide include diisobutyl peroxide, cumyl peroxyneodecanoate, di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, bis(4-tert-butylcyclohexyl) peroxydicarbonate, bis(2-ethylhexyl) peroxydicarbonate, tert-hexyl peroxyneodecanoate, tert-butyl peroxyneodecanoate, tert-butyl peroxyneoheptanoate, tert-hexyl peroxypivalate, tert-butyl peroxypivalate, di(3,5,5-trimethylhexanoyl) peroxide, dilauroyl peroxide, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexyl peroxide, The organic peroxides of the present invention are tert-butyl peroxide, ...

[0084] The organic peroxide can be used in various forms such as solid and liquid, and may be a liquid substance diluted with a diluent, etc. Among them, an organic peroxide in a form that can be easily mixed with the poly(3-hydroxybutyrate)-based resin (particularly an organic peroxide that is liquid at room temperature (25° C.)) is preferred because it can be more uniformly dispersed in the poly(3-hydroxybutyrate)-based resin and is easy to suppress local modification reactions in the resin composition.

[0085] (Other resins)

[0086] The above-mentioned original roll film may contain other resins other than poly(3-hydroxybutyrate) resins within the range that does not impair the effect of the invention. As such other resins, for example, aliphatic polyester resins such as polybutylene succinate adipate, polybutylene succinate, polycaprolactone, and polylactic acid, and aliphatic aromatic polyester resins such as polybutylene terephthalate adipate, polybutylene terephthalate sebacate, and polybutylene terephthalate azelate may be cited. As other resins, only one type may be included, or two or more types may be included.

[0087] The content of the other resin is not particularly limited, but is preferably 100 parts by weight or less, more preferably 50 parts by weight or less, further preferably 30 parts by weight or less, further preferably 20 parts by weight or less, and particularly preferably 10 parts by weight or less, relative to 100 parts by weight of the poly(3-hydroxybutyrate) resin. In addition, it may be 5 parts by weight or less, or 1 part by weight or less. The lower limit of the content of the other resin is not particularly limited, and may be 0 parts by weight or more.

[0088] The above-mentioned original roll film may contain additives that can be used together with poly (3-hydroxybutyrate) resins within the range that does not impair the effect of the invention. As such additives, there can be listed: colorants such as pigments and dyes, deodorants such as activated carbon and zeolite, fragrances such as vanillin and dextrin, fillers, plasticizers, antioxidants, antioxidants, weather resistance improvers, ultraviolet absorbers, crystal nucleating agents, lubricants, release agents, water repellents, antibacterial agents, sliding improvers, etc. As additives, only one type may be included, or two or more types may be included. Those skilled in the art can appropriately set the content of these additives according to their intended use.

[0089] Hereinafter, the crystal nucleating agent, the lubricant, the filler, and the plasticizer will be described in further detail.

[0090] (Crystallization nucleating agent)

[0091] The original film may also contain a crystal nucleating agent. Examples of the crystal nucleating agent include polyols such as pentaerythritol, galactitol, and mannitol; orotic acid, aspartame, cyanuric acid, glycine, zinc phenylphosphonate, and boron nitride. Among them, pentaerythritol is preferred from the viewpoint of having a particularly excellent effect of promoting the crystallization of poly(3-hydroxybutyrate) resins. One crystal nucleating agent may be used, or two or more crystal nucleating agents may be used, and the ratio of use may be appropriately adjusted according to the purpose.

[0092] The amount of the crystal nucleating agent used is not particularly limited, but is preferably 0.1 to 5 parts by weight, more preferably 0.5 to 3 parts by weight, and even more preferably 0.7 to 1.5 parts by weight, based on 100 parts by weight of the total amount of the poly(3-hydroxybutyrate)-based resin.

[0093] (Lubricant)

[0094] The above-mentioned original roll film may also contain a lubricant. Examples of lubricants include behenic acid amide, oleic acid amide, erucic acid amide, stearic acid amide, palmitic acid amide, N-stearyl behenic acid amide, N-stearyl erucic acid amide, ethylenebisstearic acid amide, ethylenebisoleic acid amide, ethylenebiserucic acid amide, ethylenebislauric acid amide, ethylenebiscapric acid amide, p-phenylenebisstearic acid amide, ethylenediamine, stearic acid and sebacic acid polycondensate, etc. Among them, from the viewpoint of particularly excellent lubricant effect for poly (3-hydroxybutyrate) resins, behenic acid amide or erucic acid amide is preferred. One lubricant may be used, or two or more lubricants may be used, and the usage ratio may be appropriately adjusted according to the purpose.

[0095] The amount of the lubricant used is not particularly limited, but is preferably 0.01 to 5 parts by weight, more preferably 0.05 to 3 parts by weight, and even more preferably 0.1 to 1.5 parts by weight, based on 100 parts by weight of the total amount of the poly(3-hydroxybutyrate)-based resin.

[0096] (Filling material)

[0097] The above-mentioned original roll film may contain a filler. By including a filler, a higher strength stretch film can be made. As the above-mentioned filler, any filler of an inorganic filler and an organic filler can be used, or the two can be used in combination. As an inorganic filler, there is no particular limitation, and examples thereof include: silicates, carbonates, sulfates, phosphates, oxides, hydroxides, nitrides, carbon black, etc. Only one inorganic filler can be used, or two or more can be used in combination.

[0098] The content of the filler is not particularly limited, but is preferably 1 to 100 parts by weight, more preferably 3 to 80 parts by weight, further preferably 5 to 70 parts by weight, and further preferably 10 to 60 parts by weight, relative to 100 parts by weight of the poly(3-hydroxybutyrate) resin. However, the raw film may not contain the filler.

[0099] (Plasticizer)

[0100] The above-mentioned original roll film may contain a plasticizer. As a plasticizer, for example, glyceride compounds, citrate compounds, sebacic acid ester compounds, adipic acid ester compounds, polyether ester compounds, benzoic acid ester compounds, phthalic acid ester compounds, isosorbide compounds, polycaprolactone compounds, dibasic acid ester compounds, etc. can be cited. Among them, from the viewpoint of particularly excellent plasticizing effect on poly (3-hydroxyalkanoate) resins, glyceride compounds, citrate compounds, sebacic acid ester compounds, and dibasic acid ester compounds are preferred. As glyceride compounds, for example, glyceryl diacetyl monolaurate can be cited. As citrate compounds, for example, acetyl citrate tributyl can be cited. As sebacic acid ester compounds, for example, dibutyl sebacic acid can be cited. As dibasic acid ester compounds, for example, benzylmethyl diethylene glycol adipic acid can be cited. One plasticizer can be used, or two or more can be used, and the usage ratio can be appropriately adjusted according to the purpose.

[0101] The amount of the plasticizer used is not particularly limited, but is preferably 1 to 20 parts by weight, more preferably 2 to 15 parts by weight, and even more preferably 3 to 10 parts by weight, based on 100 parts by weight of the total amount of the poly(3-hydroxybutyrate) resin. However, the raw film may not contain a plasticizer.

[0102] <Manufacturing of raw film>

[0103] The method for manufacturing the original roll film is not particularly limited, and a known manufacturing method can be appropriately used. Specifically, blow molding, T-die extrusion molding using an extruder equipped with a T-die, calendaring, calendering, etc. are listed. Among them, since a strip-shaped film can be manufactured with good productivity, blow molding or T-die extrusion molding is preferred.

[0104] (Blow molding method)

[0105] The above-mentioned blow molding method refers to a molding method in which a molten resin is extruded in a tubular shape from an extruder having a cylindrical die head installed at the front end, and then a gas is immediately blown into the tube to expand it into a hollow spherical shape, thereby forming it into a film. The blow molding is not particularly limited, and for example, it can be implemented using a general blow molding machine used when thermoplastic resin is film-molded.

[0106] A general blow molding machine refers to a blow molding machine in which a cylindrical die head is installed on a single screw extruder. The above-mentioned single screw extruder only needs to melt and mix the raw material resin input, while maintaining the desired temperature, while obtaining a certain discharge. The screw shape of the single screw extruder is not particularly limited, and from the viewpoint of mixing property, it is preferably equipped with a mixing element. In addition, the structure of the cylindrical die head is not particularly limited, and, from the aspect of less occurrence of welding and easy to obtain uniformity of thickness, a spiral mandrel die head is preferably used.

[0107] The molding temperature during blow molding is not particularly limited as long as it is a temperature at which the resin can be appropriately melted, and is preferably 135 to 200° C. The molding temperature here refers to the resin temperature from the extruder to the discharge from the die. The resin temperature is usually measured, for example, by a thermometer provided on the bushing.

[0108] The pulling speed during blow molding can be determined by the film thickness, width, and resin discharge amount, and can be adjusted within a range that allows bubble stability to be maintained. Generally, 1 to 100 m / min is preferred.

[0109] In blow molding, in order to solidify the discharged molten resin and stabilize the bubble, an air ring blowing from the outside of the bubble can be used. As a blowing structure suitable for the air ring to be used, a plurality of annular slits for blowing air can be provided, which is a slit type that promotes the stabilization of the bubble through the chamber located between the slits.

[0110] The blow-up ratio (hereinafter referred to as BUR) in blow molding is the value obtained by dividing the circumference of the bubble cross section by the diameter of the die head. From the viewpoint of improving film strength, the lower limit of BUR is preferably 1.5 times or more, more preferably 1.7 times or more, further preferably 1.9 times or more, and particularly preferably 2 times or more. In addition, from the viewpoint of molding stability, the upper limit of BUR is preferably 5.5 times or less, more preferably 4.5 times or less, further preferably 4.0 times or less, and particularly preferably 3.5 times or less.

[0111] (T-die extrusion molding method)

[0112] The T-die extrusion molding method is a molding method in which a molten resin is extruded from a slit-shaped discharge port onto a casting roll in a sheet shape by an extruder to form a film. As the T-die, there is no particular limitation, and a known T-die can be appropriately used. For example, the T-die preferably has a discharge port in a shape that can extrude a sheet-shaped thermoplastic resin, and its shape is not particularly limited. In addition, the shape of the above-mentioned discharge port is not particularly limited either.

[0113] In the extrusion step, a sheet-shaped thermoplastic resin is extruded from the outlet of the T-die. The shape of the plastic resin is any sheet-shaped, and its thickness and width are not particularly limited. In order to reduce thickness unevenness and facilitate cooling after extrusion, the thickness is preferably 20 μm to 600 μm.

[0114] In the extrusion step, the melt viscosity of the thermoplastic resin extruded from the outlet of the T-die is not particularly limited, but is preferably 1500 Pa·sec or less to reduce thickness unevenness and prevent the generation of a die line. The melt viscosity can be measured by a known method as appropriate.

[0115] <Crystallinity of original film>

[0116] As the raw film, in order to prevent the film from sticking to the equipment in contact with the film during the preheating process or stretching process described later or during transportation, it is preferred to use a film with a high degree of crystallinity. Specifically, the degree of crystallinity of the raw film is preferably higher than 40%, more preferably higher than 45%, further preferably higher than 48%, and particularly preferably higher than 50%.

[0117] The upper limit of the crystallinity of the raw film is not particularly limited, but is preferably 80% or less, more preferably 70% or less, from the viewpoint of preventing breakage in the stretching step and achieving high-ratio stretching.

[0118] The crystallinity of the original film is mainly determined by the resin temperature during the original film molding and the cooling temperature after molding (for example, the temperature of the wind ring, the temperature of the casting roll, etc.). In addition, the cooling time, the temperature of the gas atmosphere during cooling, the content ratio of the monomer unit in the poly (3-hydroxybutyrate) resin, the combination of the crystal nucleating agent, etc., also have an impact. The crystallinity of the original film can be easily controlled by considering these parameters.

[0119] The crystallinity of the original film can be determined by referring to POLYMER, 1992, Volume 33, Number 7, pp. 1563-1567. For example, it can be determined by the following steps.

[0120] The film to be measured was quickly cut into 2 cm square pieces, laminated to a thickness of 200 to 500 μm, and fixed on a glass holder.

[0121] The glass holder was fixed to a sample holder next to a characteristic X-ray Cu-Kα light source in an XRD device, and XRD measurement was performed in a range of 5 to 40° at a scanning speed of 0.02 to 0.5° / min. As the XRD device, Rint2500 manufactured by Rigaku Corporation can be used.

[0122] For the waveform obtained by this measurement, the area (integrated intensity) of the waveform with zero point correction performed on both ends is defined as Ia+Ic (area of ​​halo from amorphous part + area of ​​peak from crystalline part). Thus, Ic is defined as the area of ​​the waveform obtained by deducting (in a manner that maintains the symmetry of the scattering peak intensity) the halo from the amorphous part. The crystallinity is calculated by the mathematical formula: Ia / (Ia+Ic)×100.

[0123] In addition, from the time of sampling to the start of measurement, the sample was stored frozen at 0°C or lower in order to suppress the progress of crystallization.

[0124] <Thickness of original film>

[0125] The thickness of the original film is not particularly limited and can be appropriately set in consideration of the target thickness of the stretched film, the stretch ratio, the strength, etc. For example, it is preferably 20 to 1000 μm, more preferably 30 to 750 μm, and even more preferably 40 to 500 μm.

[0126] <Stretching process>

[0127] In the stretching step, the film is stretched while the temperature of the film is controlled within a specific range.

[0128] The stretching direction in the stretching process is not particularly limited, and the film can be stretched in any direction in the plane direction. In the case where the original roll film is a strip-shaped film, the stretching direction can be any direction in the MD direction or TD direction of the film, preferably the MD direction. Here, the MD direction is also referred to as the machine direction, the travel direction, or the length direction. The TD direction is a direction perpendicular to the MD direction, also referred to as the vertical direction or the width direction.

[0129] The specific method of stretching is not particularly limited, and preferably a method of stretching the film by stretching it along the stretching direction. Stretching the film along the stretching direction means pulling the film along the stretching direction. On the other hand, when a method of stretching the film by applying pressure along the thickness direction of the film, such as roller calendering in which the film is sandwiched between two rollers, is used, the original roll film is easily attached to the calendering roller, and sometimes the productivity of the stretched film is reduced.

[0130] The method of stretching the film in the stretching direction is not particularly limited. When the film is stretched in an intermittent manner, the film may be pulled in the stretching direction while holding the end portions of the film.

[0131] When the film is continuously conveyed while being stretched in the MD direction, for example, a roller longitudinal stretching machine can be used to give a difference in the rotation speed of the rollers between the multiple rollers conveying the film, thereby stretching in the MD direction. The stretching ratio in the MD direction can be determined by the ratio of the rotation speed of the rollers before stretching to the rotation speed of the rollers after stretching.

[0132] When the film is continuously conveyed while being stretched in the TD direction, for example, a transverse stretching machine such as a clip-type tenter can be used to clamp both ends of the film in the width direction and pull it in the TD direction, thereby stretching it in the TD direction. The stretching ratio in the TD direction can be determined by the ratio of the width of the film clamped before stretching to the width of the film clamped after stretching.

[0133] In the method for producing a stretched film of the present embodiment, the stretching step is performed while controlling the film temperature. Specifically, the raw film is stretched under the condition that the maximum temperature of the film surface is within the temperature range represented by the following formula (1).

[0134] Tm-60≤Maximum temperature of membrane surface(℃)≤Tm-5 (1)

[0135] The Tm is the melting point (° C.) of the original film. Here, the melting point of the original film refers to the top temperature of the melting point peak in the DSC curve obtained by differential scanning calorimetry. The details of differential scanning calorimetry will be described later in Example 1.

[0136] The maximum temperature of the film surface is the maximum temperature during the period when a force that stretches the original film in the stretching direction acts in the stretching step.

[0137] It can be inferred that by controlling the maximum temperature of the film surface during stretching to be within the above temperature range close to the melting point of the original film, a part of the resin crystals contained in the original film can be melted. Therefore, regardless of the crystallinity of the original film, stretching can be performed with good productivity. That is, according to this embodiment, even if an original film with high crystallinity that is generally difficult to stretch is used, stretching can be performed with good productivity.

[0138] If the film is stretched at a temperature where the maximum temperature on the film surface is lower than Tm-60 (°C), the original roll film has a high degree of crystallinity and becomes too hard. Therefore, the film may break due to the force acting on the film during the stretching process, or uneven stretching may occur, making it difficult to obtain a uniformly stretched film. From the viewpoint of suppressing uneven stretching, the lower limit of the maximum temperature on the film surface is preferably above Tm-50 (°C), more preferably above Tm-40 (°C), further preferably above Tm-30 (°C), further preferably above Tm-20 (°C), and particularly preferably above Tm-15 (°C). Within the range described above, the higher the maximum temperature on the film surface, the more uneven stretching can be suppressed and a high stretch ratio can be achieved.

[0139] On the other hand, if the film is stretched at a maximum temperature on the surface of the film higher than Tm-5°C (°C), the film will melt and break during stretching, making it difficult to obtain a stretched film. From the viewpoint of avoiding melt breakage of the film, the upper limit of the maximum temperature on the surface of the film is preferably Tm-7 (°C) or less, more preferably Tm-8 (°C) or less, and further preferably Tm-9 (°C) or less.

[0140] In order to control the film temperature in the stretching step, the film is preferably heated so that the maximum temperature of the film surface falls within the above-mentioned temperature range during stretching.

[0141] The method for heating the film is not particularly limited, and examples thereof include: a method of contacting the film being stretched with hot air heated to the above temperature range, a method of heating the film being stretched using an auxiliary heating device such as an infrared heater, a method of stretching the film in a heating furnace adjusted to a given temperature, a method of heating the stretching roller on the upstream side in the traveling direction of the film to the above temperature range while continuously conveying the film and stretching the film using a pair of stretching rollers, etc. These may be used alone or in combination of multiple types.

[0142] In order to easily perform heating, the film may be stretched by bringing a roll heated to the above-mentioned temperature range into contact with the original film.

[0143] However, the method for stretching the film is preferably a non-contact heating method in which the heating device heated to the above temperature range does not contact the original film. According to this method, the problem of film sticking to the heating device can be avoided, so the productivity of the stretched film can be further improved.

[0144] One of the preferred methods of the non-contact heating method is a method in which hot air is brought into contact with the film being stretched. In this method, the temperature of the hot air that comes into contact with the film may be set to fall within the above-mentioned temperature range.

[0145] When the film is stretched using a pair of stretching rollers while being continuously transported, it is preferred that hot air is brought into contact with the film between the stretching roller on the upstream side and the stretching roller on the downstream side in the traveling direction of the film. At this time, the temperature of the stretching roller is preferably lower than the above temperature range. According to this method, it is possible to avoid the film from sticking to the stretching roller.

[0146] Among the methods using hot air, a floating heating method is particularly preferred from the viewpoint of heating efficiency. Floating heating refers to a method of heating the film by blowing hot air from an upper nozzle and a lower nozzle to both sides of the film. A plurality of upper nozzles and a plurality of lower nozzles may be alternately arranged toward the surface of the film, and the film may be heated by hot air blown from the upper nozzle and the lower nozzle respectively when the film does not contact any of the upper nozzle and the lower nozzle.

[0147] Another preferred embodiment of the non-contact heating method is infrared radiation heating in which the film being stretched is irradiated with infrared rays. This heating method is preferred because the film surface and the inside of the film can be heated to the same temperature in a short period of time, and the entire film can be stretched uniformly.

[0148] As the infrared ray to be irradiated, electromagnetic waves in a normal infrared region can be used, and any of near infrared ray: wavelength 0.74 μm to 1.5 μm, mid infrared ray: wavelength 1.5 μm to 3.0 μm, and far infrared ray: wavelength 3.0 μm to 1 mm can be used.

[0149] When the film is stretched using a pair of stretching rollers while being continuously conveyed, it is preferred that infrared rays are irradiated to the film between the stretching roller on the upstream side and the stretching roller on the downstream side in the traveling direction of the film. At this time, the temperature of the stretching roller is preferably lower than the above temperature range. According to this method, it is possible to avoid the film from sticking to the stretching roller.

[0150] The stretching ratio that can be achieved in the stretching process described above is not particularly limited, and is preferably 1.1 times or more, more preferably 1.5 times or more, and further preferably 2 times or more. According to this embodiment, a high stretching ratio can be achieved with good productivity. The upper limit of the stretching ratio is not particularly limited, and can be appropriately determined, for example, it can be 8 times or less, or it can be 7 times or less.

[0151] <Optional preheating process>

[0152] According to the manufacturing method of this embodiment, it is preferred to pre-heat the raw film to a temperature lower than the highest temperature of the film surface reached in the stretching process before performing the heating in the stretching process. By pre-performing such a pre-heating process, the temperature control of the film in the stretching process can be more efficiently implemented, and the productivity of the stretched film can be further improved.

[0153] The maximum temperature of the film surface reached in the preheating step is preferably a temperature lower than the above-mentioned Tm-60 (°C), more preferably below Tm-65 (°C). The lower limit of the above-mentioned maximum temperature is not particularly limited, but is preferably 50°C or higher, more preferably 60°C or higher, and particularly preferably 70°C or higher.

[0154] There is no particular limitation on the method for heating the film in the preheating step, and various heating methods described in the stretching step can be appropriately adopted. In addition, a method of heating the film by contacting a roller other than the stretching roller can also be adopted. These methods can be used alone or in combination.

[0155] In the preheating step, since the heating temperature is low, the roller is not easily attached to the film. Therefore, it is preferable to adopt a method of heating by bringing the roller into contact with the film.

[0156] When the film is stretched while being continuously conveyed, it is preferred to perform preheating using a stretching roller on the upstream side in the film's traveling direction and / or at least one preheating roller disposed upstream of the stretching roller on the upstream side in the film's traveling direction. It is particularly preferred to perform preheating using a plurality of rollers, and it is particularly preferred to perform preheating by setting the set temperatures of the rollers among the plurality of rollers so that they gradually increase along the film's traveling direction.

[0157] <Optional heat treatment process>

[0158] It is preferred that the film after the stretching step is subjected to a heat treatment step to cool the film to a temperature lower than the film temperature during the stretching step. By performing this step, the strength of the stretched film can be increased and the physical properties of the stretched film can be stabilized.

[0159] The cooling temperature in the optional heat treatment step is, for example, preferably 30 to 150°C, more preferably 40 to 140°C, further preferably 40 to 120°C, particularly preferably 50 to 110°C.

[0160] There is no particular limitation on the method for controlling the film temperature in the optional heat treatment step, and the various heating methods described in the stretching step and the preheating step can be appropriately adopted. The above methods can be used alone or in combination of two or more.

[0161] When the film is stretched while being continuously conveyed, it is preferred to carry out the above-mentioned heat treatment process using a stretching roller on the downstream side of the film's traveling direction, and / or using at least one heat treatment roller arranged closer to the downstream than the stretching roller on the downstream side of the film's traveling direction.

[0162] The optional heat treatment process is preferably carried out while applying tension to the film in the direction of stretching. Thus, thermal shrinkage of the film can be avoided. When tension is applied along the MD direction, for example, the rotation speeds of the plurality of rollers conveying the film can be controlled separately. When tension is applied along the TD direction, for example, the heat treatment process can be carried out while clamping both ends of the film in the width direction with a transverse stretching machine and pulling along the TD direction.

[0163] However, the film is not substantially stretched in the heat treatment step. “The film is not substantially stretched” means that the film is not intentionally stretched in the heat treatment step.

[0164] <Continuous production method of a preferred embodiment>

[0165] The method for producing a stretched film according to the present embodiment may be performed batchwise, but is preferably performed continuously from the viewpoint of productivity of the stretched film.

[0166] When the process is carried out continuously, it is preferred to carry out each step while continuously conveying the film. Specifically, it is preferred to carry out any preheating step, stretching step and any heat treatment step in sequence while continuously feeding one end of the film from the original film rolled into a roll. In addition, it is preferred to continuously wind up the stretched film after each step with a winding roller.

[0167] When the film is continuously transported, its transport speed is not particularly limited, and from the viewpoint of the productivity of the film, it is preferably more than 5m / minute in the stage before the stretching starts. In addition, from the viewpoint of the stability of production, it is preferably less than 50m / minute in the stage before the stretching starts.

[0168] Figure 1 An example of a production line for continuously stretching a film while conveying the film is shown. The arrow in the figure indicates the traveling direction of the film.

[0169] The strip-shaped raw film 21 is manufactured from a raw material including a poly(3-hydroxybutyrate) resin or the like by a blow molding method or a T-die extrusion molding method, and is wound up on a delivery roller 11. One end of the raw film 21 is delivered from the delivery roller 11, and is transported along a given path by a plurality of conveying rollers while being subjected to a given treatment including stretching, and is wound up on a winding roller 12 to form a stretched film 22.

[0170] The plurality of conveying rollers are composed of three preheating rollers 31, 32, 33, a pair of stretching rollers 34, 35, and two heat treatment rollers 36, 37 in order from the delivery roller 11 along the travel direction. However, the number of preheating rollers and the number of heat treatment rollers are not limited to the above.

[0171] The roller surface temperatures of the preheating rollers 31, 32, 33 and the upstream stretching roller 34 are set to 60°C, 80°C, 100°C, and 110°C, respectively, in a manner that they are gradually increased along the traveling direction. By bringing the original film into contact with these rollers, a preheating process of gradually heating the original film can be implemented. Since the set temperature of these rollers is relatively low, the film is prevented from sticking to each roller.

[0172] The film is stretched between a pair of stretching rollers 34 and 35. The rotation speed of the downstream stretching roller 35 is controlled to be faster than the rotation speed of the upstream stretching roller 34, and the original film is stretched in the MD direction by the difference in rotation speed.

[0173] A heating area A is provided between a pair of stretching rollers 34 and 35. In the heating area, a plurality of upper nozzles A1 and a plurality of lower nozzles A2 are respectively opposite to the upper surface and the lower surface of the film. A plurality of upper nozzles A1 are arranged along the traveling direction of the film, and the same is true for the lower nozzles A2. The film being stretched is heated by spraying hot air from each nozzle to the film being transported.

[0174] By controlling the temperature of the hot air in advance to a temperature within the range of Tm-60 (°C) or more and Tm-5 (°C) or less (when Tm is, for example, 146°C, an example of the temperature of the hot air is 137°C), the maximum temperature of the film surface during stretching can be controlled within the range of Tm-60 (°C) or more and Tm-5 (°C) or less. Thus, the stretching of the original roll film containing the poly (3-hydroxybutyrate) resin can be performed with good productivity.

[0175] In addition, it is also preferable to replace the upper nozzle A1 and the lower nozzle A2 with infrared heaters to heat the film.

[0176] The surface temperatures of the downstream stretching roller 35 and heat treatment rollers 36 and 37 are set to 50° C. The film is cooled by contacting these rollers to perform the heat treatment process. Since the set temperature of these rollers is low, the film is prevented from sticking to each roller.

[0177] The film having undergone the preheating step, the stretching step, and the heat treatment step as described above is wound up on the winding roll 12 to become the stretched film 22. Here, the stretched film can be continuously manufactured.

[0178] <Method for producing biaxially oriented film>

[0179] Another method for producing a stretched film of the present invention may be a method for producing a biaxially stretched film. In this method, the stretching step includes: a step (i) of stretching the original roll film along a specific direction, and a step (ii) of controlling the temperature of the film within a specific range and performing stretching in a direction perpendicular to the specific direction. Steps (i) and (ii) may be performed sequentially (stepwise biaxial stretching) or simultaneously (simultaneous biaxial stretching).

[0180] The stretching direction in step (i) is not particularly limited, and the film may be stretched in any direction in the plane direction of the film. When the original film is a strip-shaped film, the stretching direction may be any direction in the MD direction or TD direction of the film, and the MD direction is preferred.

[0181] The stretching direction in step (ii) is not particularly limited as long as it is perpendicular to the stretching direction in step (i). When the original film is a strip-shaped film, the stretching direction may be any direction in the MD direction or TD direction of the film, and is preferably the TD direction.

[0182] The specific stretching method used in the step (i) and the step (ii) is not particularly limited, and the above-mentioned methods can be used as appropriate.

[0183] In the method for producing a biaxially stretched film of the present embodiment, step (ii) is performed while controlling the film temperature. Specifically, stretching is performed under the condition that the maximum temperature of the film surface is within the temperature range represented by the above formula.

[0184] In this embodiment, the maximum temperature of the film surface in the above formula refers to the maximum temperature during the period when the force pulling the film along the stretching direction in step (ii) acts. In addition, the preferred numerical range of the maximum temperature of the film surface in step (ii) is the same as above, so the description is omitted.

[0185] As for the method of heating the film, it is also the same as above, and it is preferred to use a non-contact heating method, among which a method of making hot air contact the film being stretched or a method of irradiating infrared rays is preferred. In the case where the film is stretched along the TD direction while the film is continuously conveyed and the two ends of the film in the width direction are clamped, it is preferred to make hot air contact the film in the area where the two ends in the width direction are clamped in the traveling direction of the film, or to irradiate infrared rays.

[0186] The stretching ratio achieved in step (ii) is not particularly limited and may be the same as described above.

[0187] On the other hand, the temperature conditions during stretching in step (i) are not particularly limited, and it is preferably performed while controlling the film temperature. Specifically, it is preferred that the original film be stretched in a specific direction under the condition that the maximum temperature of the film surface is within the temperature range represented by the following formula (1).

[0188] Tm-60≤Maximum temperature of membrane surface(℃)≤Tm-5 (1)

[0189] The above-mentioned Tm is the melting point (° C.) of the above-mentioned original film.

[0190] The preferred temperature conditions and heating methods in step (i) are the same as those described above, and therefore are not described herein. The maximum temperature of the film surface in formula (1) refers to the maximum temperature during the period in which the force pulling the film in the stretching direction in step (i) acts.

[0191] The stretching ratio achieved in step (i) is not particularly limited, and is preferably 1.1 times or more, more preferably 1.5 times or more, and further preferably 2 times or more. According to this embodiment, a high stretching ratio can be achieved with good productivity. The upper limit of the stretching ratio is not particularly limited, and can be appropriately determined, for example, it can be 8 times or less, or it can be 7 times or less.

[0192] In the method for producing a biaxially stretched film of the present embodiment, before performing the heating in step (i) and / or step (ii) (particularly the heating in step (i)), it is preferred to pre-heat the film to a temperature lower than the highest temperature of the film surface reached in step (i) and / or step (ii). By pre-implementing such a pre-heating step, the temperature control of the film in step (i) and / or step (ii) can be implemented more efficiently, and the productivity of the biaxially stretched film can be further improved. The conditions in the pre-heating step are as described above.

[0193] In the method for producing a biaxially stretched film of this embodiment, it is preferred that a heat treatment process is performed on the biaxially stretched film after the stretching process to cool the film to a temperature lower than the film temperature during the stretching process. By performing this process, the strength of the biaxially stretched film can be improved, and the physical properties of the biaxially stretched film can also be stabilized. The conditions in the heat treatment process are also as described above.

[0194] The method for producing a biaxially stretched film of the present embodiment may be carried out batchwise, but is preferably carried out continuously as described above from the viewpoint of productivity of the biaxially stretched film.

[0195] <Stretch film>

[0196] The stretched film (including biaxially stretched film. The same applies below) that can be manufactured by this embodiment can improve strength and stabilize film properties, so it is preferably high in crystallinity. Specifically, the crystallinity of the stretched film is preferably higher than 40%, more preferably 50% or more, further preferably 55% or more, and particularly preferably 60% or more. The upper limit is not particularly limited, and can be 100% or less, 90% or less, or 80% or less.

[0197] The crystallinity of the stretched film is mainly determined by the crystallinity of the original roll film, the heating temperature during stretching, the cooling temperature of any heat treatment process, etc. In addition, the time required for each process, the thickness of the film, etc. also have an impact. The crystallinity of the stretched film can be easily controlled by considering these parameters.

[0198] The crystallinity of the stretched film can be measured in the same manner as the method for measuring the crystallinity of the above-mentioned original film.

[0199] The thickness of the stretched film that can be manufactured by this embodiment is not particularly limited, and can be appropriately set by a person skilled in the art. From the perspective of uniform wall thickness, appearance, strength, lightness, etc. of the film, it is preferably 10 to 200 μm, more preferably 15 to 150 μm, and further preferably 20 to 100 μm. In addition, the thickness of the biaxially stretched film is preferably 5 to 200 μm, more preferably 8 to 150 μm, and further preferably 10 to 100 μm.

[0200] The stretched film may be laminated with other layers, such as resin layer, inorganic layer, metal layer, metal oxide layer, and printed layer. These other layers may be laminated layers, coating layers, or vapor-deposited layers.

[0201] The stretched film has high strength even though it is thin, and therefore can be suitably used as a packaging film, a heat-sealable film, a twist film, and the like.

[0202] In the following items, preferred embodiments of the present disclosure are listed, but the present invention is not limited to the following items.

[0203] [Project 1]

[0204] A manufacturing method is a method for manufacturing a stretched film by stretching an original roll film containing a poly(3-hydroxybutyrate)-based resin, the method comprising:

[0205] The step of stretching the raw film under the condition that the highest temperature of the film surface is within the temperature range represented by the following formula (1),

[0206] Tm-60≤Maximum temperature of membrane surface(℃)≤Tm-5 (1)

[0207] The above-mentioned Tm is the melting point (° C.) of the above-mentioned original film.

[0208] [Project 2]

[0209] The production method according to item 1, wherein the temperature range represented by the above formula (1) is a temperature range represented by the following formula (2).

[0210] Tm-30≤Maximum temperature of membrane surface(℃)≤Tm-5 (2)

[0211] [Item 3]

[0212] The production method according to item 1 or 2, wherein the crystallinity of the original film is higher than 40%.

[0213] [Item 4]

[0214] The production method according to any one of items 1 to 3, wherein the stretched film has a crystallinity higher than 40%.

[0215] [Item 5]

[0216] The production method according to any one of items 1 to 4, wherein the stretched film has a crystallinity of 50% or more.

[0217] [Item 6]

[0218] The production method according to any one of items 1 to 5, wherein the film is heated so that the highest temperature of the film surface during the stretching falls within the temperature range.

[0219] [Item 7]

[0220] The production method according to item 6, wherein the heating is performed by at least one non-contact heating method selected from the group consisting of hot air heating and infrared radiation heating.

[0221] [Item 8]

[0222] The manufacturing method according to item 7, wherein the hot air heating is a floating method.

[0223] [Item 9]

[0224] The production method according to item 7 or 8, further comprising, before performing the non-contact heating method, a step of preheating the original film to a temperature lower than the highest temperature of the film surface.

[0225] [Item 10]

[0226] The production method according to any one of items 6 to 10, wherein the heating is performed by bringing a roll heated to the temperature range into contact with the original film.

[0227] [Item 11]

[0228] The production method according to any one of items 1 to 10, wherein the stretching is performed by making a difference in the rotation speed of a plurality of rollers that convey the film.

[0229] [Item 12]

[0230] The production method according to any one of items 1 to 11, wherein the stretching ratio achieved by the stretching is 1.1 to 8 times.

[0231] [Item 13]

[0232] The production method according to any one of items 1 to 12, wherein the original film roll is a film produced by a blow molding method.

[0233] [Item 14]

[0234] The manufacturing method according to Item 13, wherein in the blow molding method, the blow ratio is 2 times or more.

[0235] [Item 15]

[0236] The production method according to any one of items 1 to 12, wherein the raw film is a film produced by a T-die extrusion molding method.

[0237] [Item 16]

[0238] The production method according to any one of items 1 to 15, wherein the poly(3-hydroxybutyrate)-based resin comprises poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).

[0239] [Item 17]

[0240] The production method according to any one of items 1 to 16, wherein the stretched film is a biaxially stretched film.

[0241] The manufacturing method comprises:

[0242] Step (i) of stretching the original film in a specific direction, and

[0243] Step (ii) of performing stretching in a direction perpendicular to the specific direction,

[0244] The step (ii) is a step of performing stretching under the condition that the maximum temperature of the surface of the film is within the temperature range represented by the formula (1).

[0245] [Item 18]

[0246] The production method according to item 17, wherein the step (i) is performed under the condition that the maximum temperature of the film surface is within the temperature range represented by the following formula (1).

[0247] Tm-60≤Maximum temperature of membrane surface(℃)≤Tm-5 (1)

[0248] The above-mentioned Tm is the melting point (° C.) of the above-mentioned original film.

[0249] [Item 19]

[0250] The production method according to item 17 or 18, wherein the step (i) and the step (ii) are performed sequentially.

[0251] [Item 20]

[0252] The production method according to item 17 or 18, wherein the step (i) and the step (ii) are performed simultaneously.

[0253] Example

[0254] The present invention will be described in more detail below with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples at all.

[0255] The following raw materials were used in Examples and Comparative Examples.

[0256] (Poly (3-hydroxybutyrate) resin)

[0257] A-1: poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (average content ratio 3HB / 3HH=94 / 6 (mol% / mol%), weight average molecular weight 600,000 g / mol, glass transition temperature 6°C)

[0258] It was manufactured according to the method described in Example 1 of International Publication No. 2019 / 142845.

[0259] (Evaluation of film thickness)

[0260] The thickness was measured with a vernier caliper at 10 locations at intervals of 10 cm along the TD direction of the film, and the arithmetic mean of the thicknesses at the 10 locations was calculated as the film thickness.

[0261] (Method for determination of melting point)

[0262] The melting point of each resin was determined by differential scanning calorimetry in accordance with JIS K-7121.

[0263] Specifically, first, about 4 to 5 mg of the resin to be measured is accurately weighed, and the temperature is raised from 0° C. to 180° C. at a heating rate of 10° C. / min using a differential scanning calorimeter (SSC5200 manufactured by Seiko Instruments Inc.) to obtain a DSC curve. In the obtained DSC curve, the top temperature of the melting point peak is taken as the melting point.

[0264] (Method for determining crystallinity)

[0265] The crystallinity of the original film and the stretched film was measured.

[0266] The film to be measured was quickly cut into 2 cm square pieces, laminated to a thickness of 200 to 500 μm, and fixed on a glass holder.

[0267] The glass holder was fixed to a sample holder near a characteristic X-ray Cu-Kα light source in an XRD device (Rint2500 manufactured by Rigaku Corporation), and XRD measurement was performed in a range of 5 to 40° at a scanning speed of 0.02 to 0.5° / min.

[0268] For the waveform obtained by this measurement, the area (integrated intensity) of the waveform with zero point correction performed on both ends is defined as Ia+Ic (area of ​​halo from amorphous part + area of ​​peak from crystalline part). Thus, Ic is defined as the area of ​​the waveform obtained by deducting (in a manner that maintains the symmetry of the scattering peak intensity) the halo from the amorphous part. The crystallinity is calculated by the mathematical formula: Ia / (Ia+Ic)×100.

[0269] The crystallinity was calculated by the mathematical formula: Ia / (Ia+Ic)×100.

[0270] (Determination of breaking strength)

[0271] As for the breaking strength of the stretched film, the Figure 2 A test piece of the shape shown (a test piece in accordance with the old JIS K7113-2 1 / 3) was subjected to a tensile test at a tensile speed of 100 mm / min along the tensile direction of the stretched film in accordance with JIS K7127 using a tensile testing machine (manufactured by Shimadzu Corporation: EZ-LX 1 kN), and the stress (breaking strength) when the test piece broke was determined.

[0272] [Production of Poly(3-hydroxybutyrate) Resin Particles P-1]

[0273] With respect to 100 parts by weight of the poly(3-hydroxybutyrate) resin A-1, 0.5 parts by weight of behenic acid amide (BNT-22H manufactured by Nippon Seika Co., Ltd.) as a lubricant, 0.5 parts by weight of erucic acid amide, and 1.0 parts by weight of pentaerythritol as a crystal nucleating agent were dry-blended. The barrel temperature and the die head temperature were set at 150°C. The obtained dry blend was put into a co-rotating twin-screw extruder and extruded, and passed through a water tank filled with hot water at 45°C to solidify the strands, which were cut with a pelletizer to obtain resin pellets P-1. The melting point of the resin pellets P-1 was 146°C.

[0274] <Example 1>

[0275] use The resin particles P-1 were fed into a single-screw extruder and a blow molding machine having a blow molding die (die diameter 100 mm, die lip gap 1.0 mm) to obtain an original roll film with a thickness of 70 μm and a crystallinity of 58% at an output of 29 kg / h, a resin temperature of 165°C, a film folding width of 390 mm (blowing ratio 2.5), and a pulling speed of 5 m / min.

[0276] A 100 mm × 200 mm test piece was cut from the obtained original roll film (cut in the manner of short side in the MD direction), and placed in a hot air oven while keeping the two long sides, and the film temperature was kept at 135°C, and uniaxially stretched to 2 times at a speed of 400 mm / min in the MD direction (at this time, the two short sides were not fixed). Then, the obtained film was heat treated at 50°C to obtain a stretched film with a thickness of 27 μm and a crystallinity of 61%. It should be noted that the breaking strength of the stretched film is recorded in Table 1.

[0277] <Example 2>

[0278] Connect the T-die with a width of 350mm The barrel temperature and die temperature of the single screw extruder were set to 165°C, respectively. The resin pellets P-1 were added to the single screw extruder to melt them, and the molten resin at a temperature of 165°C was extruded in a film form through a T die. The film-like molten resin was extruded onto a casting roll set at 60°C, and molded at a pulling speed of 10m / min. After cooling to a film temperature of 60°C, the film was peeled off from the casting roll to obtain an original roll film with a thickness of 70μm and a crystallinity of 58%.

[0279] The obtained raw film was stretched in the same manner as in Example 1 except that the stretching ratio was changed to 3 times, thereby obtaining a stretched film having a thickness of 27 μm and a crystallinity of 62%.

[0280] <Example 3>

[0281] The original roll film obtained in Example 2 was contacted with three preheating rollers and an upstream stretching roller (the surface temperature of each roller was adjusted to 60°C, 80°C, 100°C, and 110°C in sequence) and transported. The film was continuously heated to 137°C in a hot air furnace with nozzles for blowing hot air arranged above and below the transported film, and the film was stretched to 3 times along the travel direction by the roller speed difference before and after the hot air furnace. Then, a heat treatment was further performed at 50°C using a transport roller adjusted to 50°C to obtain a stretched film with a thickness of 40μm and a crystallinity of 62%. It should be noted that the breaking strength of the stretched film is recorded in Table 1.

[0282] <Examples 4 to 6>

[0283] A stretched film was obtained by the same method as in Example 3 except that the stretching ratio was changed to 4 times, 5 times, and 6 times, respectively. The thickness, crystallinity, and breaking strength of the stretched film are shown in Table 1.

[0284] <Examples 7 and 8>

[0285] A film stretched 2 or 3 times was obtained by the same method as in Example 3, except that the thickness of the original film was changed to 80 μm and a far-infrared heater was placed on the film to heat the film to 126° C. or 135° C. instead of using a hot air furnace equipped with a nozzle for blowing hot air. The thickness, crystallinity, and breaking strength of the stretched film are shown in Table 1.

[0286] <Example 9>

[0287] The film was stretched in the same manner as in Example 1 except that the film temperature during stretching was changed to 110° C. and the stretching ratio was changed to 1.5 times. The thickness, crystallinity, and breaking strength of the stretched film are shown in Table 1.

[0288] <Comparative Example 1>

[0289] Stretching was performed in the same manner as in Example 1 except that the film temperature during stretching was changed to 145° C. As a result, the film melted and broke during stretching, and could not be stretched.

[0290] <Comparative Example 2>

[0291] Stretching was performed in the same manner as in Example 1 except that the film temperature during stretching was changed to 60° C. As a result, the film was broken during stretching due to insufficient heating of the film, and stretching could not be performed.

[0292]

[0293] According to Table 1, in Examples 1 to 9 in which the film was stretched at a temperature 5 to 60°C lower (here 86 to 141°C) than the melting point (here 146°C), stretched films were produced with good productivity.

[0294] On the other hand, in Comparative Example 1, in which the film temperature during stretching was set higher than the above range, the film melted and broke. In Comparative Example 2, in which the film temperature during stretching was set lower than the above range, the film broke due to stretching, uneven stretching occurred, and a uniform stretched film could not be obtained.

[0295] <Example 10>

[0296] First, through the same procedure as in Example 1, a uniaxially stretched film was obtained.

[0297] A 100 mm x 100 mm test piece was cut from the obtained uniaxially stretched film, and placed in a hot air oven while maintaining all four sides, and the film temperature was maintained at 120° C. The film was stretched to 2 times in the TD direction at a speed of 400 mm / min, thereby obtaining a biaxially stretched film.

[0298] Then, the obtained film was heat-treated at 50° C. to obtain a biaxially stretched film having a thickness of 15 μm and a crystallinity of 62%. Table 2 shows the breaking strengths in the MD and TD directions of the obtained biaxially stretched film.

[0299] <Example 11>

[0300] By the same procedure as in Example 2, an original film having a thickness of 300 μm and a crystallinity of 58% was obtained.

[0301] Furthermore, the obtained raw film was biaxially stretched in the same manner as in Example 10 to obtain a biaxially stretched film having a thickness of 50 μm and a crystallinity of 62%. Table 2 shows the breaking strengths in the MD and TD directions of the obtained biaxially stretched film.

[0302] <Comparative Example 3>

[0303] Stretching was performed in the same manner as in Example 11 except that the film temperature during stretching in the TD direction was changed to 60° C. As a result, the film was broken during stretching due to insufficient heating of the film, and stretching could not be performed.

[0304] <Comparative Example 4>

[0305] Stretching was performed in the same manner as in Example 11 except that the film temperature during stretching in the TD direction was changed to 145° C. As a result, the film melted and broke during stretching, and could not be stretched.

[0306] [Table 2]

[0307]

[0308] According to Table 2, in Examples 10 and 11 in which the film was stretched in the TD direction at a temperature 5 to 60°C lower (here 86 to 141°C) than the melting point (here 146°C), biaxially stretched films could be produced with good productivity.

[0309] On the other hand, in Comparative Example 3, where the film temperature during TD stretching was set below the above temperature range, the film broke due to stretching. In Comparative Example 4, where the film temperature during TD stretching was set above the above temperature range, the film melted and broke.

Claims

1. A method for producing a stretched film by stretching a raw film comprising a poly(3-hydroxybutyrate) resin, the method comprising: The process of stretching the raw film under the condition that the maximum temperature of the film surface is within the temperature range represented by the following formula (1), Tm-60≤Maximum temperature of membrane surface(℃)≤Tm-5 (1) The Tm is the melting point (° C.) of the original film.

2. The manufacturing method according to claim 1, wherein The temperature range represented by the formula (1) is the temperature range represented by the following formula (2), Tm-30≤Maximum temperature of membrane surface(℃)≤Tm-5 (2) 3. The manufacturing method according to claim 1 or 2, wherein: The crystallinity of the original roll film is higher than 40%.

4. The manufacturing method according to claim 1 or 2, wherein: The stretched film has a crystallinity higher than 40%.

5. The manufacturing method according to claim 1 or 2, wherein: The stretched film has a crystallinity of 50% or more.

6. The manufacturing method according to claim 1 or 2, wherein: The film is heated so that the maximum temperature of the film surface during the stretching falls within the temperature range.

7. The manufacturing method according to claim 6, wherein: The heating is performed by at least one non-contact heating method selected from the group consisting of hot air heating and infrared radiation heating.

8. The manufacturing method according to claim 7, wherein: The hot air heating is a floating method.

9. The manufacturing method according to claim 7, wherein: Before performing the non-contact heating method, the method further includes preheating the original film to a temperature lower than the highest temperature of the film surface.

10. The manufacturing method according to claim 6, wherein: The heating is performed by bringing a roller heated to a temperature within the above-mentioned temperature range into contact with the raw film.

11. The manufacturing method according to claim 1 or 2, wherein: The stretching is performed by creating a difference in the rotation speed of a plurality of rollers that transport the film.

12. The manufacturing method according to claim 1 or 2, wherein: The stretching ratio achieved by the stretching is 1.1 to 8 times.

13. The manufacturing method according to claim 1 or 2, wherein: The raw film roll is a film produced by a blow molding method.

14. The manufacturing method according to claim 13, wherein: In the blow molding method, the blow ratio is 2 times or more.

15. The manufacturing method according to claim 1 or 2, wherein: The original roll film is a film produced by a T-die extrusion molding method.

16. The manufacturing method according to claim 1 or 2, wherein: The poly(3-hydroxybutyrate)-based resin includes poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).

17. The manufacturing method according to claim 1 or 2, wherein: The stretched film is a biaxially stretched film, The manufacturing method comprises: Step (i) of stretching the original film roll along a specific direction; and (ii) performing stretching in a direction perpendicular to the specific direction, The step (ii) is a step of performing stretching under the condition that the maximum temperature of the film surface is within the temperature range represented by the formula (1).

18. The manufacturing method according to claim 17, wherein: The step (i) is carried out under the condition that the maximum temperature of the film surface is within the temperature range represented by the following formula (1), Tm-60≤Maximum temperature of membrane surface(℃)≤Tm-5 (1) The Tm is the melting point (° C.) of the original film.

19. The manufacturing method according to claim 17, wherein: The steps (i) and (ii) are performed sequentially.