Compounds, their preparation and use as Anti-aging, Anti-oxidant and / or colorant in rubber blends and vehicle tyres

By developing dibenzodiazepine derivative compounds, the potential hazards and solubility of existing aging stabilizers in vehicle tires and industrial rubber products have been solved, and better antioxidant effects and reduced frost phenomenon have been achieved. Provides a safer and more effective protection solution.

CN118922410APending Publication Date: 2024-11-08CONTINENTAL REIFEN DEUTSCHLAND GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028011.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-13
Filing Date
2023-03-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing aging stabilizers have potential hazards and poor solubility in vehicle tires and industrial rubber products, resulting in uncontrolled oxidation reactions and undesired frost problems, affecting the protective effect and aesthetics of the material.

Method used

Developed a dibenzodiazepine derivative compound with low potential hazards and good solubility, in place of alternatives to traditional aromatic amine aging stabilizers, with improved production by reacting with hydrogen and ketones or aldehydes. Compounds with antioxidant effects.

Benefits of technology

The compound provides comparable or improved aging stability at high temperatures, reduces frost phenomena, improves the protection of the material, and reduces health hazards. It is suitable for vehicle tires and other industrial rubber products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922410A_ABST
    Figure CN118922410A_ABST
Patent Text Reader

Abstract

The invention relates to a compound (I), a rubber mixture containing the compound, a vehicle tyre comprising the rubber mixture in at least one component, a method for producing the compound and the use of the compound as an aging stabilizer and / or antioxidant and / or dye, in which R1 is selected from the group consisting of: xi) aromatic groups; wherein the aromatic groups optionally carry substituents selected from the group consisting of halogen groups, cyano groups, ester groups, ketone groups, ether groups and thioether groups, and xii) linear, branched and cyclic aliphatic C3-C12-groups wherein X is selected from the group consisting of O (oxygen atom), S (sulfur atom) and N (H) (secondary amino), and wherein Y is selected from the group consisting of O (oxygen atom), S (sulfur atom) and N (H) (secondary amino). # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a compound, a rubber mixture containing the compound, a vehicle tire comprising the rubber mixture in at least one component, a process for producing the compound and the use of the compound as an ageing stabilizer and / or antioxidant and / or dye. Background Art

[0002] It is known that polymeric materials such as, in particular, rubber are used in vehicle tires and industrial rubber products.

[0003] Natural rubber and synthetic polymers (such as IR, BR, SSBR, ESBR, etc.) as well as natural and synthetic oils, fats and lubricants are subject to oxidation reactions over long periods of storage and, in particular, in target applications, which are often at high temperatures, which have an adverse effect on the initially desired properties. Depending on the type of polymer, the polymer chains are shortened until the material liquefies, or subsequently hardens.

[0004] Therefore, aging stabilizers play a vital role in the service life of vehicle tires and other industrial rubber products.

[0005] Known ageing stabilizers include aromatic amines, such as

[0006] 6PPD (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine),

[0007] IPPD (N-isopropyl-N'-phenyl-p-phenylenediamine) or

[0008] SPPD (N-(1-phenylethyl)-N'-phenyl-p-phenylenediamine).

[0009] These molecules can react with oxygen or ozone or with the free radicals formed (such as alkyl, alkoxy and alkyl peroxide radicals) and thus scavenge these and thus protect the polymer from further oxidation reactions.

[0010] However, a disadvantage of these substances is that they may cause cancer.

[0011] Weathering stabilizers that are particularly reactive with ozone and effectively scavenge it are also known as "antiozonants."

[0012] Another problem associated with ageing stabilizers is the problem of unwanted blooming. Here, the slightly poor solubility of the molecules of the ageing stabilizer in the surrounding polymer matrix of the rubber article leads to their diffusion to the surface of the article to be protected and there to form a film which is usually distinguishable in color from the rest of the article. In the case of vehicle tires, this usually manifests itself as a brown coloration of the otherwise black sidewalls. In addition to aesthetic disadvantages, this is also associated with disadvantages in terms of the ageing stabilization effect. This is because the blooming substances are usually removed. This firstly reduces the total amount of ageing stabilizer and also has the effect that further ageing stabilizer molecules diffuse into their place, as a result of which the polymer has a continuously decreasing level of protection. Summary of the invention

[0013] The object of the present invention is to provide novel compounds which can be used as ageing stabilizers, in particular in vehicle tires or other industrial rubber products, which have a particularly low hazard potential and sufficient solubility in the corresponding matrix, for example and in particular in polymers. This is intended to ensure continuous optimal protection from oxygen and ozone and to minimize or prevent the tendency to bloom, while reducing the risk to health.

[0014] The compounds are simultaneously intended to ensure comparable or even improved aging stability compared to aromatic amines such as 6PPD.

[0015] This object is achieved by a compound according to the invention as claimed in claim 1 , a rubber mixture according to the invention containing the compound and a vehicle tire according to the invention comprising the rubber mixture according to the invention in at least one component.

[0016] This object is also achieved by a process according to the invention for producing the compounds according to the invention.

[0017] The compound according to claim 1 has the general formula I):

[0018]

[0019] Where R 1 selected from the group consisting of: xi) aromatic groups, wherein these aromatic groups optionally carry substituents selected from the group consisting of halogen groups, cyano groups, ester groups, keto groups, ether groups and thioether groups,

[0020] and xii) straight chain, branched and cyclic aliphatic C3- to C 12 - groups,

[0021] The group R 2 and R 3may be identical or different from each other and are selected from the group consisting of: linear, branched and cyclic saturated and unsaturated aliphatic C1- to C2- 12 - groups, aryl groups optionally bearing one or more halogen substituents, and halogen groups (of which fluorine, bromine and chlorine are preferred), cyano groups, ester groups, ketone groups, ether groups and thioether groups

[0022] And m takes the value of 0, 1, 2 or 3

[0023] and where n takes the value of 0 or 1 or 2 or 3 or 4,

[0024] wherein X is selected from O (oxygen atom), S (sulfur atom) and N (H) (secondary amino group),

[0025] wherein Y is selected from O (oxygen atom), S (sulfur atom) and N (H) (secondary amino group).

[0026] It is clear to the skilled person that, for example, when m is 0 (zero) or 1 or 2, the corresponding hydrogen atom replaces R 2 Bonded to the corresponding carbon atom of the benzene ring. Of course, this is true for R 3 The same applies to the case where n is less than 4.

[0027] It is also clear to those skilled in the art that (R 2 ) m , (R 3 ) n‘ and R 1 The representation of the bonds of HN to the benzene ring of the structure means that these groups can each be arranged at any position on the corresponding benzene ring, except of course two or more at the same position at the same time, since the tetravalent nature of the carbon atoms of the benzene ring already excludes this possibility.

[0028] In the context of the present invention, "C3- to C 12 -group" is to be understood as meaning a group having 3 to 12 carbon atoms. Irrespective of this, "C1" is used to describe the carbon atom with the highest degree of oxidation / the position with the highest priority according to the Cahn-Ingold-Prelog convention (CIP). It will be clear to a person skilled in the art what this means in the respective context.

[0029] The compounds according to the invention are dibenzodiazepines Ketone derivatives and exhibit lower hazard potential compared to known aniline-based aging stabilizers (possible cleavage products of 6PPD).

[0030] This is a key advantage, especially in industrial applications, such as in vehicle tires or other industrial rubber products, where rubber components may be released through wear or other degradation processes. Ketones are found in a variety of orally administered medications.

[0031] Compared to the known aging stabilizer 6PPD, the compounds according to the invention exhibit an improved antioxidant effect (especially at relatively high temperatures of more than 150° C.), so that the compounds of formula I) achieve a comparable or even improved protective effect, especially in vehicle tires and other industrial rubber products, as well as in oils and lubricants.

[0032] However, the present invention should not be limited to a specific mechanism of action or a specific explanation.

[0033] The compounds according to the invention are therefore suitable as alternatives to 6PPD, the degradation products of which are highly toxic to coho salmon and therefore probably also to other aquatic organisms.

[0034] In addition, the compounds of the invention have sufficient solubility in rubber mixtures, in particular in rubber mixtures for vehicle tires and other industrial rubber products. This minimizes the blooming of the compounds, as is known from many aging stabilizers, which in turn has a favorable effect on the aging stabilization effect. The less blooming of the aging stabilizer, the less aging stabilizer is removed intentionally or unintentionally from the surface of the article to be protected, and the less aging stabilizer is diffused to the surface.

[0035] The compounds of the formula I) according to the invention are particularly suitable as aging stabilizers and / or antiozonants in vehicle tires and / or other technical rubber articles and / or oils and / or lubricants, such as, in particular, air springs, bellows, conveyor belts, belts, drive belts, hoses, rubber belts, profiles, seals, membranes, tactile sensors for medical or robotic applications, or shoe soles or parts thereof.

[0036] The compounds of formula I) according to the invention are particularly suitable for producing rubber articles, in particular air springs, bellows, conveyor belts, belts, drive belts, hoses, rubber belts, profiles, seals, membranes, tactile sensors for medical or robotic applications, or shoe soles or parts thereof.

[0037] To use the compounds of formula I) in the recited preparations or materials, the compounds are used in the compositions and incorporated in the compositions.

[0038] In vehicle tires or other industrial rubber products, the composition is in particular a rubber mixture.

[0039] The present invention further provides the use of compounds of formula I) according to the invention in oils and lubricants, such as fuels or fluids, in particular for engines. In particular, the compounds according to the invention can be used in engines.

[0040] The invention further provides for the use of the compounds of the formula I) according to the invention as dyes in fibers and / or polymers and / or paper and / or in (decorative) paints and coatings.

[0041] The invention encompasses all advantageous embodiments, in particular as reflected in the claims. The invention also includes in particular embodiments resulting from a combination of different features, wherein these features have different levels of preference, so that the invention also includes a combination of a first feature described as "preferred" or described in the case of an advantageous embodiment with another feature described as "particularly preferred", for example.

[0042] Furthermore, all information relating to the properties of the compounds according to the invention also applies to the methods according to the invention for producing the compounds and to the rubber mixtures according to the invention containing the compounds and to the uses according to the invention.

[0043] -N(H)R 1 The radical is preferably arranged in the meta position relative to X.

[0044] Therefore, the compounds according to the invention preferably have the structure of formula II):

[0045]

[0046] Where R 1 , R 2 , R 3 , X and Y as well as m and n are as defined above.

[0047] This achieves the object of the invention particularly well and in particular achieves sufficient solubility of the compound in rubber mixtures, in particular rubber mixtures for vehicle tires.

[0048] As is clear from formulae I) and II), X is incorporated into the ring structure and is selected from O (oxygen atom), S (sulfur atom) and N (H) (secondary amino group).

[0049] It is clear to the skilled person that when X is NH, the nitrogen atom (N) is bonded to the adjacent carbon atom, while the hydrogen atom (H) is bonded only to the nitrogen atom.

[0050] It is preferred, for example and especially in formulas I) and II), that X is in each case NH. This achieves the objects of the invention particularly well and in particular achieves a very good antioxidant effect in polymers and / or rubber mixtures, in particular in polymers and / or rubber mixtures for vehicle tires.

[0051] As is clear, for example, from formulae I) and II), Y is terminally bonded to a carbon atom and

[0052] Selected from O (oxygen atom), S (sulfur atom) and N (H) (secondary amino group).

[0053] It is clear to the skilled person that when Y is NH, the nitrogen atom (N) is bonded to the adjacent carbon atom, while the hydrogen atom (H) is bonded only to the nitrogen atom.

[0054] It is preferred, for example and in particular in the formulae I) and II), that Y is in each case O (ie an oxygen atom), resulting in a carbonyl group (—C═O) next to X.

[0055] This achieves the object of the invention particularly well and in particular achieves a very good antioxidant effect in polymer and / or rubber mixtures, in particular in polymer and / or rubber mixtures for vehicle tires.

[0056] Group R 2 and R 3 are independently identical or different from one another and are selected from the group consisting of: linear, branched and cyclic saturated and unsaturated aliphatic C1- to C2- 12 - groups, aryl groups optionally bearing one or more halogen substituents, and halogen groups (of which fluorine, bromine and chlorine are preferred), cyano groups, ester groups, ketone groups, ether groups and thioether groups.

[0057] By selecting appropriate starting materials, the groups R 2 and R 3 In particular, bonding to the corresponding benzene ring / precursors thereof may have already been possible.

[0058] It is preferred, for example and in particular in formulae I) and II), that m is zero (0).

[0059] It is preferred, for example and in particular in formulae I) and II), that n is zero (0).

[0060] This leads to the preferred structures shown in formula Ia) or IIa):

[0061]

[0062] Where X, Y and R 1 As defined above.

[0063] It is also preferred here that X is N(H) and Y is O.

[0064] Group R 1 Selected from the group consisting of:

[0065] xi) aromatic groups, wherein these aromatic groups optionally carry substituents selected from the group consisting of halogen groups, cyano groups, ester groups, keto groups, ether groups and thioether groups,

[0066] and xii) straight chain, branched and cyclic aliphatic C3- to C 12 -group.

[0067] The aromatic groups of subgroup xi) are, by way of example and preferably, selected from phenyl (—C 6 H 5 ) and benzyl (—CH 2 —C 6 H 5 ), with phenyl being particularly preferred.

[0068] The aromatic groups of subgroup xi) may have substituents.

[0069] As described above, these substituents are selected from the group consisting of a halogen group, a cyano group, an ester group, a ketone group, an ether group and a thioether group.

[0070] It is preferred that the substituent is selected from the group consisting of an ester group, a ketone group, an ether group and a thioether group.

[0071] In a preferred embodiment, the aromatic group is unsubstituted on the two carbon atoms adjacent to the C1 atom (ie the carbon atom bonded to the N atom). In the case of a benzene ring as the basic structure, it is therefore preferred that there is no substituent in the ortho position relative to the N atom.

[0072] In a further preferred embodiment, the aromatic groups of subgroup xi) are unsubstituted.

[0073] R is preferred 1 The bond to the nitrogen atom (N) is via a tertiary carbon atom. This means that the C1 atom is preferably a tertiary carbon atom.

[0074] In the context of the present invention, the term "tertiary carbon atom" is understood to mean a carbon atom which is bonded to only one hydrogen atom.

[0075] Due to the presence of these compounds in rubber mixtures, in particular for vehicle tires and other technical rubber products, relative to secondary and quaternary carbon atoms, this leads to a particularly good protective effect and, in particular, to an optimal reactivity with respect to the mechanisms associated with aging stabilization, wherein undesirable side reactions are avoided.

[0076] In a further advantageous embodiment, in particular in the aforementioned formulae I), II), Ia), IIa), R 1 is a branched or cyclic alkyl group having three to twelve carbon atoms, preferably three to eight carbon atoms, wherein R 1 Particularly preferably, R is selected from 1,3-dimethylbutyl and cyclohexyl, wherein 1Very particular preference is given to 1,3-dimethylbutyl.

[0077] This achieves particularly good solubility in rubber mixtures for vehicle tires and other industrial rubber products.

[0078] In a particularly preferred embodiment, the compounds according to the present invention have the structure of formula III):

[0079]

[0080] The compounds of formula III) have sufficient solubility in polymers, in particular in rubber mixtures for vehicle tires and other industrial rubber products. At the same time, the compounds of formula II) can be produced in a particularly simple, energy-efficient and cost-effective manner and, compared with 6PPD, exhibit comparable or even improved antioxidant effects (especially at temperatures above 150° C.) and therefore comparable or improved aging stabilization effects.

[0081] According to the IUPAC nomenclature, the compound of formula III) may also be referred to as 2-(1,3-dimethylbutylamino)-5,10-dihydro-dibenzo[b,e][1,4]diazepine -11-Keto.

[0082] As mentioned above, the present invention further provides a method for producing a compound having formula I), which method comprises at least the following method steps:

[0083] i) producing or providing a substance having the formula B1):

[0084]

[0085] ii) reacting the compound of formula B1) with hydrogen and a ketone or an aldehyde, preferably a ketone, to obtain the compound of formula I):

[0086]

[0087] Where R 1 selected from the group consisting of: xi) aromatic groups, wherein these aromatic groups optionally carry substituents selected from the group consisting of halogen groups, cyano groups, ester groups, keto groups, ether groups and thioether groups,

[0088] and xii) straight chain, branched and cyclic aliphatic C3- to C 12 - groups,

[0089] The group R 2 and R 3may be identical or different from each other and are selected from the group consisting of: linear, branched and cyclic saturated and unsaturated aliphatic C1- to C2- 12 - groups, aryl groups optionally bearing one or more halogen substituents, and halogen groups (of which fluorine, bromine and chlorine are preferred), cyano groups, ester groups, ketone groups, ether groups and thioether groups

[0090] And m takes the value of 0, 1, 2 or 3

[0091] and where n takes the value of 0 or 1 or 2 or 3 or 4,

[0092] wherein X is selected from O (oxygen atom), S (sulfur atom) and N (H) (secondary amino group),

[0093] wherein Y is selected from O (oxygen atom), S (sulfur atom) and N (H) (secondary amino group).

[0094] All of the above information provided in conjunction with the description of the compounds according to the present invention (including the preferred embodiments) and taking into account the possibility of any kind of hierarchy of preferences for these features and combinations of these features applies to R 1 , R 2 , R 3 , X, Y, m and n.

[0095] When X is N(H) (secondary amino group) and Y is O (oxygen atom), compounds of formula B1) can be produced analogously to, for example, US6919328 according to the following scheme S1):

[0096]

[0097] wherein TEA stands for triethylamine and DMSO stands for dimethyl sulfoxide.

[0098] As indicated above, the group -N(H)R 1 The group -NO2 in the starting material is preferably arranged in the meta position relative to X.

[0099] Therefore, the compounds produced according to the present invention preferably have the structure of formula II):

[0100]

[0101] For this purpose, the starting material of formula B1) preferably has the structure of formula B1a):

[0102]

[0103] Where R 1 , R 2 , R 3, X and Y as well as m and n are as defined above, including all embodiments and combinations of features.

[0104] Here too, in a preferred embodiment, X is N(H) and Y is O.

[0105] It is preferred that the reaction with hydrogen in step ii) is carried out using a suitable catalyst, which in the context of the present invention is referred to as a "hydrogenation catalyst".

[0106] It is preferred that the hydrogenation catalyst is a noble metal catalyst, such as in particular palladium (Pd) or platinum (Pt). It is preferred that the noble metal is used on carbon (C), such as palladium on carbon (Pd / C).

[0107] In addition, other known catalysts such as Raney nickel or copper chromite may also be used.

[0108] Particularly preferred is the reaction with hydrogen in step ii).

[0109] This is carried out using a hydrogenation catalyst.

[0110] The reaction in step ii) is preferably carried out at a temperature of 50 to 130°C, preferably 50 to 100°C, particularly preferably 50 to 80°C, in particular for example 60°C.

[0111] Preference is given to subjecting the reaction mixture to hydrogen at a pressure of 30 to 70 bar, particularly preferably 35 to 45 bar, in particular, for example, 40 bar, and then preferably stirring for 1 to 20 hours, preferably 3 to 13 hours, particularly preferably 5 to 13 hours, in particular, for example, 10 hours.

[0112] The reaction with hydrogen in step ii) is preferably carried out in a vessel suitable for the preferably relatively high pressures, such as in particular in an autoclave or in another pressure reactor.

[0113] Particularly preferred is the reaction in step ii) using a hydrogenation catalyst and carried out with hydrogen at a temperature of 50° C. to 130° C., preferably 50° C. to 100° C., particularly preferably 50° C. to 80° C., and wherein the reaction mixture is subjected to hydrogen at a pressure of 30 to 70 bar, particularly preferably 35 to 45 bar, in particular, for example 40 bar, and the reaction is carried out in an autoclave or in another pressure reactor.

[0114] The ketone in step ii) is the subsequent radical R 1 In the case of an aldehyde, it is correspondingly an aldehyde derivative.

[0115] For simplicity, the abbreviation R is used for aldehydes or ketones. 1 =O, because the group R 1 It is the moiety that remains on the nitrogen atom after reaction with an aldehyde or ketone.

[0116] The ketone used here is preferably methyl isobutyl ketone.

[0117] The solvent in step ii) can be a ketone or an aldehyde, if it is in liquid form, or an inert solvent such as toluene or xylene, especially if the ketone or aldehyde is in solid form. In the latter case, only a stoichiometric amount of the ketone or aldehyde is used as a reactant.

[0118] It is preferred to use the ketone or aldehyde R in liquid form. 1 =0, ketones are particularly preferred as solvents. This makes it possible to dispense with the use of any additional substances such as toluene or xylene.

[0119] Step ii) is preferably followed by purification, for example by filtration and washing with a solvent, in particular ethanol, and / or by column chromatography, for example on silica gel, or by recrystallization from cyclohexane or a long-chain aliphatic compound.

[0120] As mentioned above, the present invention further provides a rubber mixture.

[0121] The rubber mixture according to the invention contains a compound of formula I), for example and preferably a compound of formula III). The rubber mixture according to the invention can in principle be any rubber mixture in which the novel compound of formula I) or III) acts as an aging stabilizer and / or antiozonant with low toxicity, in particular according to the invention.

[0122] The rubber mixture according to the invention contains at least one rubber.

[0123] Preferably, the rubber mixture according to the invention contains 0.1 to 10 phr, particularly preferably 0.1 to 7 phr, very particularly preferably 1 to 6 phr and further preferably 1 to 3 phr of a compound of the formula I), for example and preferably a compound of the formula III).

[0124] The rubber mixture may also contain mixtures of two or more compounds of formula I).

[0125] The unit "phr" (parts per hundred parts of rubber by weight) used in this document is a conventional indication of the amount of a mixture formulation in the rubber industry. The dosages of the individual substances in parts by weight are in this document based on 100 parts by weight of all high molecular weight (M) compounds present in the mixture. w Greater than 20 000 g / mol) of the total mass of the rubber.

[0126] In an advantageous embodiment of the invention, the rubber mixture according to the invention contains at least one diene rubber.

[0127] Thus, the rubber mixture may contain a diene rubber or a mixture of two or more different diene rubbers.

[0128] Diene rubber is a rubber formed by polymerization or copolymerization of a diene and / or a cycloolefin, and thus has a C═C double bond in the main chain or in a side group.

[0129] The diene rubber is preferably selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), epoxidized polyisoprene (ENR), butadiene rubber (BR), butadiene-isoprene rubber, solution-polymerized styrene-butadiene rubber (SSBR), emulsion-polymerized styrene-butadiene rubber (ESBR), styrene-isoprene rubber, polyisoprene rubber having a molecular weight of more than 20 000 g / mol ... w Liquid rubber, halogenated butyl rubber, polynorbornene, isoprene-isobutylene copolymer, ethylene-propylene-diene rubber, nitrile rubber, chloroprene rubber, acrylate rubber, fluororubber, silicone rubber, polysulfide rubber, epichlorohydrin rubber, styrene-isoprene-butadiene terpolymer, hydrogenated acrylonitrile butadiene rubber and hydrogenated styrene-butadiene rubber.

[0130] In particular, nitrile rubber, hydrogenated acrylonitrile-butadiene rubber, chloroprene rubber, butyl rubber, halogenated butyl rubber and / or ethylene-propylene-diene rubber are used in the production of industrial rubber products such as belts, drive belts and hoses, and / or shoe soles. Preferably, mixture compositions for these rubbers which are specific in terms of fillers, plasticizers, vulcanization systems and additives and are known to those skilled in the art are used here.

[0131] The natural polyisoprene and / or synthetic polyisoprene of all embodiments can be cis-1,4-polyisoprene or 3,4-polyisoprene. However, preference is given to using cis-1,4-polyisoprene with a cis-1,4 ratio of >90% by weight. Such polyisoprene can firstly be obtained by stereospecific polymerization in solution with a Ziegler-Natta catalyst or using finely dispersed alkyl lithium. Secondly, natural rubber (NR) is such a cis-1,4-polyisoprene, wherein the cis-1,4 content in the natural rubber is greater than 99% by weight.

[0132] Also further contemplated are mixtures of one or more natural polyisoprenes with one or more synthetic polyisoprenes.

[0133] In the context of the present invention, the term "natural rubber" is understood to mean the naturally occurring rubber that can be obtained from the Hevea rubber tree and "non-Hevea" sources. Non-Hevea sources include, for example, the guayule shrub and dandelions such as, for example, TKS (Taraxacum kok-saghyz; Russian dandelion).

[0134] If the rubber mixture of the present invention contains butadiene rubber (i.e. BR, polybutadiene), it can be of any type known to those skilled in the art. These include so-called high cis types and low cis types, wherein polybutadiene with a cis content of not less than 90% by weight is referred to as high cis type, and polybutadiene with a cis content of less than 90% by weight is referred to as low cis type. An example of low cis polybutadiene is Li-BR (lithium catalyzed butadiene rubber) with a cis content of 20% to 50% by weight. Particularly good properties and low hysteresis of the rubber mixture are achieved with high cis BR.

[0135] The one or more polybutadienes used can be end-group modified and / or functionalized along the polymer chain by modification and functionalization. The modification can be selected from the modification with hydroxyl and / or ethoxy and / or epoxy and / or siloxane groups and / or amino and / or aminosiloxane and / or carboxyl and / or phthalocyanine groups and / or silane-sulfide groups. However, other modifications known to those skilled in the art, also referred to as functionalized, are also useful. Metal atoms can be such functionalized components.

[0136] In the case where at least one styrene-butadiene rubber (styrene-butadiene copolymer) is present in the rubber mixture, this styrene-butadiene rubber can be solution polymerized styrene-butadiene rubber (SSBR) and emulsion polymerized styrene-butadiene rubber (ESBR), and mixtures of at least one SSBR and at least one ESBR are also employable. The terms "styrene-butadiene rubber" and "styrene-butadiene copolymer" are used synonymously in the context of the present invention.

[0137] The styrene-butadiene copolymers used can be end-group modified and / or functionalized along the polymer chain by the modifications and functionalizations listed above for the polybutadienes.

[0138] The at least one diene rubber is preferably selected from the group consisting of natural polyisoprene (NR, natural rubber), synthetic polyisoprene (IR), butadiene rubber (BR), solution polymerized styrene-butadiene rubber (SSBR), emulsion polymerized styrene-butadiene rubber (ESBR), butyl rubber (IIR) and halogenated butyl rubber.

[0139] In a particularly preferred embodiment of the present invention, the at least one diene rubber is selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), butadiene rubber (BR), solution polymerized styrene-butadiene rubber (SSBR) and emulsion polymerized styrene-butadiene rubber (ESBR).

[0140] In a particularly advantageous embodiment of the invention, the rubber mixture contains at least one natural polyisoprene (NR), preferably in an amount of 50 to 100 phr, and in a particularly advantageous embodiment of the invention, in an amount of 80 to 100 phr, even more preferably 95 to 100 phr, and even more preferably 100 phr. Such rubber mixtures exhibit, in particular, optimized tear and wear properties as well as good processability and reversion stability.

[0141] If the rubber mixture contains less than 100 phr of NR, it preferably contains as additional rubber at least one diene rubber selected from the group consisting of synthetic polyisoprene (IR), butadiene rubber (BR), solution-polymerized styrene-butadiene rubber (SSBR) and emulsion-polymerized styrene-butadiene rubber (ESBR).

[0142] In a further particularly advantageous embodiment of the invention, the rubber mixture comprises at least one natural polyisoprene (NR), preferably in an amount of 5 to 55 phr, and in a particularly advantageous embodiment of the invention, in an amount of 5 to 25 phr, even more preferably 5 to 20 phr. Such a rubber mixture exhibits particularly good processability and reversion stability as well as optimized tearing properties and optimal rolling resistance characteristics.

[0143] In a further particularly advantageous embodiment of the invention, the rubber mixture contains at least one polybutadiene (BR, butadiene rubber), preferably in an amount of 10 to 80 phr, more preferably 10 to 50 phr, and in a particularly advantageous embodiment of the invention, in an amount of 15 to 40 phr. This achieves particularly good tear and wear properties and optimal braking characteristics of the rubber mixture of the invention.

[0144] In another particularly advantageous embodiment of the invention, the rubber mixture comprises at least one solution polymerized styrene-butadiene rubber (SSBR), preferably in an amount of 10 to 80 phr, more preferably 30 to 80 phr, and in a particularly advantageous embodiment of the invention, in an amount of 50 to 70 phr. This achieves particularly good rolling resistance properties of the rubber mixture of the invention. In a particularly advantageous embodiment of the invention, SSBR is used in combination with at least one other rubber to achieve an optimal and balanced distribution of properties.

[0145] It is preferred that the rubber mixture contains at least one filler, preferably in an amount of 30 to 500 phr, more preferably 50 to 400 phr, even more preferably 80 to 300 phr.

[0146] In an advantageous embodiment of the invention, the filler is a reinforcing filler preferably selected from the group consisting of carbon black and silica.

[0147] Suitable carbon blacks include any type of carbon black known to those skilled in the art. It is preferred that the carbon black is selected from industrial carbon black and thermal carbon black, with industrial carbon black being more preferred.

[0148] It is preferred that the carbon black has an iodine value according to ASTM D 1510 (also known as iodine adsorption value) between 30 and 250 g / kg, preferably 30 to 180 g / kg, more preferably 40 to 180 g / kg and even more preferably 40 to 130 g / kg, and a DBP value according to ASTM D 2414 of 30 to 200 ml / 100 g, preferably 70 to 200 ml / 100 g, more preferably 90 to 200 ml / 100 g.

[0149] The DBP value according to ASTM D 2414 determines the specific absorption volume of carbon black or light-colored fillers by means of dibutyl phthalate.

[0150] The use of carbon blacks of this type in rubber mixtures, in particular in rubber mixtures for vehicle tires, ensures the best possible compromise between wear resistance and heat buildup, which in turn influences the ecologically relevant rolling resistance.

[0151] Particularly suitable and preferred carbon blacks are carbon blacks having an iodine adsorption value of between 80 and 110 g / kg and a DBP value of 100 to 130 ml / 100 g, such as in particular carbon black of the N339 type.

[0152] The silicon dioxide is preferably amorphous silicon dioxide, such as precipitated silica, which is also referred to as precipitated silicon dioxide. However, for example, fumed silicon dioxide may also be used instead.

[0153] However, it is particularly preferred to use a 2 / g, preferably 35 to 350m 2 / g, more preferably 85 to 320m 2 / g and even more preferably 120 to 235 m 2 / g nitrogen surface area (BET surface area) (according to DIN ISO 9277 and DIN 66132) and 30 to 400 m 2 / g, preferably 30 to 330m 2 / g, more preferably 80 to 300m 2 / g and even more preferably 115 to 200 m 2 / g CTAB surface area (according to ASTM D 3765) of fine dispersion, precipitated silica. Such silica, for example, produces particularly good physical properties of vulcanized rubber in rubber mixtures for tire treads. Advantages in the processing of the mixture can also be produced here by reducing the mixing time while retaining the same product properties, which leads to increased productivity. The silica used can therefore be, for example, from Evonik Silica of the VN3 type (trade name) or highly dispersible silicas known as HD silicas (e.g. from Solvay) 1165MP).

[0154] In a particularly advantageous embodiment of the invention, the rubber mixture contains at least one silica as filler, preferably in an amount of 30 to 500 phr, more preferably 50 to 400 phr, and even more preferably 80 to 300 phr.

[0155] In these amounts, silica is especially present as the sole or principal filler (greater than 50% by weight based on the total filler amount).

[0156] In a further advantageous embodiment of the invention, the rubber mixture contains at least one silica as a further filler, preferably in an amount of 5 to 100 phr, more preferably 5 to 80 phr, and even more preferably 10 to 60 phr.

[0157] In these amounts, silica is especially present as an additional filler in addition to another primary filler such as, in particular, carbon black.

[0158] The terms "silicic acid" and "silica" are used synonymously in the context of the present invention.

[0159] In a particularly advantageous embodiment of the present invention, the rubber mixture according to the present invention contains 0.1 to 60 phr, preferably 3 to 40 phr, particularly preferably 5 to 30 phr, very particularly preferably 5 to 15 phr of at least one carbon black. In these amounts, the carbon black is present in particular as an additional filler in addition to the main filler (such as, in particular, silica).

[0160] In another advantageous embodiment of the present invention, rubber mixture of the present invention contains 30 to 300 phr, preferably 30 to 200 phr, more preferably 40 to 100 phr of at least one carbon black. In these amounts, carbon black exists as the only or main filler, and optionally exists with above-mentioned less amount in combination with silica.

[0161] In a particularly advantageous embodiment of the invention, the rubber mixture contains 5 to 60 phr, more preferably 5 to 40 phr, of at least one carbon black, and 50 to 300 phr, preferably 80 to 200 phr, of at least one silica.

[0162] The rubber mixture may additionally contain reinforcing or non-reinforcing further fillers.

[0163] In the context of the present invention, such additional (non-reinforcing) fillers include aluminosilicates, kaolin, chalk, starch, magnesium oxide, titanium dioxide or rubber gel and also fibers (eg aramid fibers, glass fibers, carbon fibers, cellulose fibers).

[0164] In addition, optional reinforcing fillers are, for example, carbon nanotubes (CNTs, including discrete CNTs, hollow carbon fibers (HCFs) and modified CNTs containing one or more functional groups such as hydroxyl, carboxyl and carbonyl groups), graphite and graphene, and so-called "carbon-silica dual-phase fillers".

[0165] In the context of the present invention, zinc oxide is not included among the fillers.

[0166] The rubber mixture may further contain customary additives in customary amounts by weight, which are preferably added during the production of the mixture in at least one preliminary mixing stage. These additives include

[0167] a) ageing stabilizers known in the prior art,

[0168] For example, p-phenylenediamine, such as N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N,N'-diphenyl-p-phenylenediamine (DPPD), N-(1-phenylethyl)-N'-phenyl-p-phenylenediamine (SPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine (7PPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD),

[0169] or dihydroquinoline, such as 2,2,4-trimethyl-1,2-dihydroquinoline (TMQ),

[0170] b) activators, such as zinc oxide and fatty acids (such as stearic acid) and / or other activators, such as zinc complexes, such as zinc ethylhexanoate,

[0171] c) activators and / or agents for binding fillers, in particular carbon black or silica, for example S-(3-aminopropyl)thiosulfate and / or its metal salts (binding to carbon black) and silane coupling agents (binding to silicon dioxide, in particular silica),

[0172] d) antiozonant wax,

[0173] e) resins, especially tackifying resins,

[0174] f) plasticizing aids, such as 2,2'-dibenzamidodiphenyl disulfide (DBD), and

[0175] g) processing aids, such as, in particular, fatty acid esters and metal soaps, for example zinc soaps and / or calcium soaps,

[0176] h) Plasticizers, such as, in particular, aromatic, naphthenic or paraffinic mineral oil plasticizers, for example MES (mild extraction solvate) or RAE (residual aromatic extract) or TDAE (treated distillate aromatic extract), or rubber liquid oils (RTL) or biomass liquid oils (BTL) preferably having a polycyclic aromatic hydrocarbon content of less than 3% by weight according to method IP 346, or triglycerides, such as rapeseed oil or oil paste or hydrocarbon resins or liquid polymers having an average molecular weight (determined by GPC=gel permeation chromatography in accordance with BS ISO 11344:2004) of between 500 and 20 000 g / mol.

[0177] When a mineral oil is used it is preferably selected from the group consisting of DAE (distillate aromatic extract), RAE (residual aromatic extract), TDAE (treated distillate aromatic extract), MES (mild extracted solvent) and naphthenic oils.

[0178] In a particularly advantageous embodiment, the rubber mixture according to the invention contains no aging stabilizers from the group of p-phenylenediamines, in particular those listed above under a), in addition to the compounds of the invention of formula I), for example of formula III. In a particularly preferred embodiment, the rubber mixture according to the invention contains in particular 0 to 0.1 phr, in particular 0 phr, of a further aging stabilizer based on p-phenylenediamine and selected from the group comprising, preferably consisting of: N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N-(1-phenylethyl)-N'-phenyl-p-phenylenediamine (SPPD), N,N'-diphenyl-p-phenylenediamine (DPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine (7PPD).

[0179] Very small amounts of p-phenylenediamine, preferably 0 to 0.1 phr, particularly preferably 0 phr, and the compounds of formula I), for example of formula III), present according to the invention enable comparable protective effects to be achieved at lower toxicity. The compounds of formula I), for example of formula III), according to the invention, replace the p-phenylenediamines listed as known in the prior art.

[0180] In a further advantageous embodiment of the invention, at least one further representative of the listed p-phenylenediamine ageing stabilizers is present and the compounds of the invention thus only partially replace the p-phenylenediamines known from the prior art. This also achieves the advantages of the invention, but not to the optimum extent.

[0181] In an advantageous embodiment, in addition to the compound of formula I) according to the invention, an aging stabilizer based on dihydroquinoline (such as TMQ) is present in the rubber mixture. The amount of dihydroquinoline (such as especially TMQ) present is preferably 0.1 to 3 phr, in particular 0.5 to 1.5 phr.

[0182] Antiozonant waxes (group d above) are considered separately and are present in the rubber mixture in preferred embodiments of the invention, regardless of whether further aging stabilizers a) are present.

[0183] The silane coupling agent may be of any type known to those skilled in the art.

[0184] Furthermore, one or more different silane coupling agents can be used in combination with one another. The rubber mixture can therefore contain a mixture of different silanes.

[0185] Silane coupling agents react with surface silanol groups or other polar groups of silicon dioxide, in particular of silica, during (in situ) mixing of rubber / rubber mixtures or in the context of pretreatment (premodification) even before adding fillers to the rubber.

[0186] Coupling agents known from the prior art are difunctional organosilanes which have at least one alkoxy, cycloalkoxy or phenoxy group as a leaving group on the silicon atom and a group as a further functional group which, possibly after cleavage, can enter into a chemical reaction with the double bonds of the polymer. The latter group may, for example, comprise the following chemical groups:

[0187] -SCN, -SH, -NH2 or -S x -(where x=2 to 8).

[0188] Thus, silane coupling agents that can be used include, for example, 3-mercaptopropyltriethoxysilane, 3-thiocyanatopropyltrimethoxysilane or 3,3'-bis(triethoxysilylpropyl)polysulfides having 2 to 8 sulfur atoms, such as 3,3'-bis(triethoxysilylpropyl)tetrasulfide (TESPT), the corresponding disulfide (TESPD) or mixtures of sulfides having 1 to 8 sulfur atoms with various sulfides in different contents. TESPT can also be used, for example, as a mixture with industrial carbon black (trade name TESPD from Evonik). )Add to.

[0189] End-capped mercaptosilanes, such as those known, for example, from WO 99 / 09036, can also be used as silane coupling agents. It is also possible to use silanes as described in WO 2008 / 083241 A1, WO 2008 / 083242 A1, WO 2008 / 083243 A1 and WO 2008 / 083244 A1. Useful silanes include, for example, those sold under the name NXT by Momentive, USA in many variants, such as, in particular, 3-octanoylthio-1-propyltriethoxysilane, or by Evonik Industries under the name VP Si The ones that are sold.

[0190] The total proportion of further additives is preferably from 3 to 150 phr, more preferably from 3 to 100 phr and most preferably from 5 to 80 phr.

[0191] Zinc oxide (ZnO) may be contained in the above-mentioned amount in the total proportion of other additives.

[0192] This can be any type of zinc oxide known to those skilled in the art, such as ZnO granules or powder. Conventionally used zinc oxide usually has a particle size of less than 10 m 2 However, it is also possible to use a BET surface area of ​​10 to 100 m 2 / g of BET surface area of ​​zinc oxide, such as "nano zinc oxide".

[0193] The rubber mixtures of the invention are preferably used in vulcanized form, in particular in vehicle tires or other vulcanized industrial rubber articles.

[0194] The terms "vulcanized" and "cross-linked" are used synonymously in the context of the present invention.

[0195] The vulcanization of the rubber mixture of the present invention is preferably carried out in the presence of sulphur and / or sulphur donors by means of vulcanization accelerators, some of which can simultaneously serve as sulphur donors. The accelerator is selected from the group consisting of thiazole accelerators, thiol-containing accelerators, sulfenamide accelerators, thiocarbamate accelerators, thiuram accelerators, thiophosphate accelerators, thiourea accelerators, xanthate accelerators and guanidine accelerators.

[0196] It is preferred to use a sulfenamide accelerator selected from the group consisting of N-cyclohexyl-2-benzothiazolylsulfenamide (CBS), N,N-dicyclohexylbenzothiazolyl-2-sulfenamide (DCBS), benzothiazolyl-2-sulfonylmorpholine (MBS), N-tert-butyl-2-benzothiazolylsulfenamide (TBBS) and a guanidine accelerator such as diphenylguanidine (DPG).

[0197] The sulfur donor substance used can be selected from any one of the sulfur donor substances known to those skilled in the art.

[0198] Vulcanization retarders may also be present in the rubber mixture.

[0199] The production of rubber mixture is preferably carried out by conventional methods in the rubber industry in addition, wherein at first in one or more mixing stages, produce a primary mixture of all the ingredients except the vulcanization system (for example sulphur and the material that affects vulcanization). Final mixture is produced by adding the vulcanization system in the final mixing stage.

[0200] The final mixture is further processed and brought into a suitable shape, for example by means of an extrusion operation or calendering.

[0201] The rubber mixture of the invention is particularly suitable for use in vehicle tires, in particular pneumatic vehicle tires. In principle, it is conceivable to use it in all tire components, in particular in the outer components, in particular and preferably in the flange profiles, the tread and / or the side tread. In the case of a tread with a crown / base construction, the rubber mixture of the invention is preferably used at least in the crown.

[0202] For use in vehicle tires, the mixture is brought into the corresponding shape (preferably of the outer part) as a final mixture before vulcanization and applied in a known manner during the production of the green vehicle tire.

[0203] As mentioned above, carried out the production of rubber mixture of the present invention, this rubber mixture is used as any other body mixture in vehicle tire.Difference is the shaping after the extrusion operation / calendering of mixture.The shape of the rubber mixture not yet vulcanized for one or more different body mixtures so obtained is then used for the construction of green tire.

[0204] Here "body mix" refers to the rubber mix used for the internal parts of the tire, such as mainly squeegees, innerliners (inner layers), core profiles, belts, shoulders, belt profiles, carcasses, bead reinforcements, bead profiles, flange profiles and hoop strips.

[0205] The uncured green tire is subsequently vulcanized.

[0206] In order to use the rubber mixture of the invention in drive belts and other belts, in particular in conveyor belts, the extruded, not yet vulcanized mixture is brought into a suitable shape and is generally provided simultaneously or subsequently with strength members, such as synthetic fibers or steel cords. This generally provides a multilayer construction consisting of one and / or more layers of rubber mixture, one and / or more layers of identical and / or different strength members and one and / or more further layers of identical and / or another rubber mixture.

[0207] The invention further provides a vehicle tire which comprises, in at least one component, a rubber mixture according to the invention, which contains the compound according to the invention.

[0208] The vulcanized vehicle tire comprises at least one vulcanized rubber of the rubber mixture of the present invention in at least one component. It is known to those skilled in the art that most substances (e.g., rubber present) already exist or may exist in a chemically modified form after mixing or only after vulcanization.

[0209] In the context of the present invention, "vehicle tyres" are intended to mean pneumatic vehicle tyres and all-rubber tyres, including tyres for industrial and construction site vehicles, trucks, cars and two-wheeler tyres.

[0210] It is preferred that the vehicle tire of the invention comprises the rubber mixture of the invention in at least one outer component, wherein the outer component is preferably the tread, the sidewall and / or the flange profile.

[0211] The vehicle tire according to the invention can therefore also contain in two or more components a rubber mixture according to the invention, optionally with an adjusted composition, which contains a compound according to the invention of the formula I). DETAILED DESCRIPTION

[0212] The present invention will now be described in more detail with reference to exemplary embodiments.

[0213] The compound of formula III) as an exemplary embodiment of the compound of formula I) is produced in the following manner as shown in Schemes S1a) and S2):

[0214] S1a)

[0215]

[0216] The synthesis is carried out according to US Pat. No. 6,919,328 according to S1a).

[0217] 2-(1,3-Dimethylbutylamino)-5,10-dihydro-dibenzo[b,e][1,4]diazepine -11-Keto (with Synthesis of compounds of formula III):

[0218]

[0219] 0.30 g (1.12 mmol, 1 equivalent (eq.)) of 2-nitro-5,10-dihydro-dibenzo[b,e][1,4]diazepine -11-ketone, 0.10 g of platinum on carbon (Pt / C) (5%) (0.4 g on 4.67 mmol substrate) and 20.0 ml of methyl isobutyl ketone (MIBK) were weighed into a stainless steel autoclave equipped with a Teflon inliner. The reaction mixture was then subjected to 40 bar of hydrogen (H2) and the mixture was stirred at 60°C for 10 hours. After the reaction was complete, excess hydrogen was released and the suspension was passed through Filter and wash with ethanol. Concentrate the filtrate to dryness and dry under vacuum. Purify the product by column chromatography (cyclohexane / acetate). Brown solid; yield 0.18 g (50% of theory).

[0220] 1 H-NMR (nuclear magnetic resonance) (500 MHz, DMSO-d6) δ = 9.72 (s, 1H), 7.20 (s, 1H), 6.97-6.82 (m, 5H), 6.77 (d, J = 8.5 Hz, 1H), 6.63 (dd, J = 8.6, 2.9 Hz, 1H), 5.00 (d, J = 8.3 Hz, 1H), 3.31 (s, 1H), 1.71 (dh, J = 13.4, 6.5 Hz, 1H), 1.44-1.32 (m, 5H), 1.18 (dt, J = 13.8, 6.9 Hz, 1H), 1.03 (d, J = 6.2 Hz, 3H), 0.89 (d, J = 6.6 Hz, 3H), 0.85 (d, J = 6.6 Hz, 3H).

[0221] ESI-MS (electrospray ionization mass spectrometry) [M+H] + =310.

[0222] Measurement of Oxidation Induction Time (OIT)

[0223] The potential protective effect of compounds of formula III) as ageing stabilizers was investigated under laboratory conditions by measuring the oxidation induction time.

[0224] For this purpose, the compound of formula III) and 6PPD were in each case mixed with a polymer (liquid synthetic polyisoprene (IR), LIR-50, Kuraray, weight-average molecular weight distribution M w =54 000 g / mol, glass transition temperature T g = -63°C) were heated together at a constant temperature at three different temperatures (180°C; 165°C; 150°C) until oxidation began.

[0225] Heating to 180°C was performed as follows:

[0226] The starting temperature was 35°C, heated to 170°C at a heating rate of 20 K / min (Kelvin / minute), and heated to 180°C at a heating rate of 1 K / min; purge gas: nitrogen (N2), volume flow rate 50 ml / min).

[0227] The sample was maintained under isothermal conditions at 180° C. for 5 minutes under N 2 atmosphere, and then the atmosphere was switched to O 2 atmosphere (volume flow rate 50 ml / min).

[0228] Heating to 165° C. was carried out analogously by first heating to 155° C. at a heating rate of 20 K / min (Kelvin / minute) and then heating to 165° C. at a heating rate of 1 K / min.

[0229] Heating to 150° C. was carried out analogously by first heating to 140° C. at a heating rate of 20 K / min (Kelvin / minute) and then heating to 150° C. at a heating rate of 1 K / min.

[0230] Oxidation was determined via one peak using DSC (Differential Scanning Calorimetry).

[0231] The time until oxidation was measured in each case in minutes.

[0232] The results compared with the known weathering stabilizer 6PPD are summarized in Table 1.

[0233] Table 1

[0234]

[0235] Taking into account the measurement accuracy of ± (plus / minus) 10 minutes, it is evident that the compound of formula III) achieves an improved protection effect compared to 6PPD at temperatures above 150° C., since the time taken until oxidation starts is significantly longer.

[0236] At 150° C., the time taken until the oxidation started was too long, and the experiments were therefore terminated after 900 minutes in each case. Therefore, the differences between 6PPD and the compound of formula III) have not been experimentally determined to date.

[0237] Therefore, the compounds of the formula III) according to the invention, which are representatives of the compounds of the formula I) according to the invention, are more environmentally friendly and less harmful to health than the other representatives of the 6PPD / substance class as described above and are also comparable or even better aging stabilizers.

[0238] At the same time, the compounds of the formula III) according to the invention, which are representative of the compounds of the formula I) according to the invention, exhibit sufficient solubility in rubber mixtures. This minimizes blooming, which in turn has a favorable effect on the protective effect.

[0239] The compounds of the formula I) therefore generally make it possible to achieve an improved protective effect for the possible applications listed.

[0240] For use in rubber mixtures for vehicle tires, during the production of the rubber mixture, the compounds of formula I), for example of formula III), according to the invention are added in one of the mixing stages in a manner known to the person skilled in the art, for example instead of the aging stabilizers known from the prior art, such as 6PPD, 7PPD or IPPD etc.

[0241] For this purpose, compounds of the formula III) were incorporated, by way of example, in various amounts as indicated in Table 2. The resulting inventive examples are identified as E1 and E2.

[0242] As a comparison, rubber mixtures of otherwise identical composition were used which contained 6PPD instead of the compound of formula III) as aging stabilizer, wherein in each case, on a mol / mol basis, substitutions were made between V1 and E1 and between V2 and E2. The amounts in Table 2 are reported in phr. A reference (Ref.) without aging stabilizer is also reported.

[0243] In all mixtures, the sum of the amounts of aging stabilizer (6PPD or formula III) and plasticizer oil MES was 10 phr.

[0244] Table 2

[0245]

[0246]

[0247] Compared to rubber mixtures comprising 6PPD, the inventive examples show comparable or even improved aging stability effects.

Claims

1. A compound having formula I): I) Where R 1 selected from the group consisting of: xi) aromatic groups, wherein these aromatic groups optionally carry substituents selected from the group consisting of halogen groups, cyano groups, ester groups, keto groups, ether groups and thioether groups, and xii) straight chain, branched and cyclic aliphatic C3- to C 12 - groups, The group R 2 and R 3 may be identical or different from each other and are selected from the group consisting of: linear, branched and cyclic saturated and unsaturated aliphatic C1- to C2- 12 - groups, aryl groups optionally bearing one or more halogen substituents, and halogen groups - of which fluorine, bromine and chlorine are preferred, cyano groups, ester groups, ketone groups, ether groups and thioether groups And m takes the value of 0, 1, 2 or 3 and where n takes the value of 0 or 1 or 2 or 3 or 4, wherein X is selected from O (oxygen atom), S (sulfur atom) and N (H) (secondary amino group), wherein Y is selected from O (oxygen atom), S (sulfur atom) and N (H) (secondary amino group).

2. The compound according to claim 1, characterized in that The compound has the structure of formula II): II) Where R 1 , R 2 , R 3 , X and Y and m and n are as defined in claim 1.

3. The compound according to claim 1 or 2, characterized in that X is NH.

4. A compound as claimed in any one of the preceding claims, characterized in that Y is O.

5. A compound as claimed in any one of the preceding claims, characterized in that m is zero (0) and / or n is zero (0).

6. A compound as claimed in any one of the preceding claims, characterized in that R 1 Bonded to the nitrogen atom (N) via a tertiary carbon atom.

7. A compound as claimed in any one of the preceding claims, characterized in that R 1 It is a branched or cyclic alkyl group having 3 to 12 carbon atoms, preferably 3 to 8 carbon atoms.

8. A compound as claimed in any one of the preceding claims, characterized in that R 1 is selected from 1,3-dimethylbutyl and cyclohexyl, wherein R 1 Preferred is 1,3-dimethylbutyl.

9. A compound as claimed in any one of the preceding claims, characterized in that The compound has the structure of formula III) III) 10. A rubber mixture comprising The compound according to any one of claims 1 to 9, wherein the rubber mixture preferably contains at least one diene rubber, the at least one diene rubber being particularly preferably selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), butadiene rubber (BR), solution-polymerized styrene-butadiene rubber (SSBR), emulsion-polymerized styrene-butadiene rubber (ESBR), butyl rubber (IIR) and halogenated butyl rubber.

11. A vehicle tire comprising the rubber mixture as claimed in claim 10 in at least one component, preferably in at least one external component, wherein the external component is preferably a tread, a sidewall and / or a flange profile.

12. Use of a compound according to any one of claims 1 to 9 as an ageing stabilizer and / or antiozonant, in particular in vehicle tires and / or other technical rubber products and / or oils and / or lubricants, such other technical rubber products as in particular air springs, bellows, conveyor belts, belts, drive belts, hoses, rubber belts, profiles, seals, membranes, tactile sensors for medical or robotic applications, or shoe soles or parts thereof.

13. Use of a compound according to any one of claims 1 to 9 for producing rubber articles, in particular air springs, bellows, conveyor belts, belts, drive belts, hoses, rubber belts, profiles, seals, membranes, tactile sensors for medical or robotic applications, or shoe soles or parts thereof.

14. Use of a compound as claimed in any one of claims 1 to 9 as a dye in fibers and / or polymers and / or paper and / or in (decorative) paints and coatings.

15. A method for producing a compound of formula I), comprising at least the following method steps: i) producing or providing a substance having the formula B1): B1) ii) reacting the compound of formula B1) with hydrogen and a ketone or an aldehyde, preferably a ketone, to obtain the compound of formula I): I) Where R 1 selected from the group consisting of: xi) aromatic groups, wherein these aromatic groups optionally carry substituents selected from the group consisting of halogen groups, cyano groups, ester groups, keto groups, ether groups and thioether groups, and xii) straight chain, branched and cyclic aliphatic C3- to C 12 - groups, The group R 2 and R 3 may be identical or different from each other and are selected from the group consisting of: linear, branched and cyclic saturated and unsaturated aliphatic C1- to C2- 12 - groups, aryl groups optionally bearing one or more halogen substituents, and halogen groups - of which fluorine, bromine and chlorine are preferred, cyano groups, ester groups, ketone groups, ether groups and thioether groups And m takes the value of 0, 1, 2 or 3 and where n takes the value of 0 or 1 or 2 or 3 or 4, wherein X is selected from O (oxygen atom), S (sulfur atom) and N (H) (secondary amino group), wherein Y is selected from O (oxygen atom), S (sulfur atom) and N (H) (secondary amino group).

16. The method of claim 15, wherein: The reaction in step ii) is carried out using a hydrogenation catalyst and / or with hydrogen at a temperature of 50 to 130° C., preferably 50 to 100° C., particularly preferably 50 to 80° C., and / or the reaction mixture is subjected to hydrogen at a pressure of 30 to 70 bar, particularly preferably 35 to 45 bar, in particular, for example 40 bar, and the reaction is carried out in an autoclave or in another pressure reactor.

17. The method according to any one of claims 15 or 16, characterized in that The compound of formula I) has the structure of formula II): II) And wherein the substance having formula B1) has the structure of formula B1a): B1a) Where R 1 , R 2 , R 3 , X and Y and m and n are as defined in claim 15.